Diamond-copper composite material and preparation method thereof
A diamond-copper composite with a Ti 3-x Zr x SiC2 transition layer improves interfacial bonding and thermal conductivity, addressing stability issues for high-performance thermal management.
Patent Information
- Application Number
- CN202411059603.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-12-03
AI Technical Summary
The poor wettability and high thermal stress at the interface of diamond-copper composites hinder effective bonding and stability, limiting their use in high-performance thermal management materials.
A diamond-copper composite material with a Ti 3-x Zr x SiC2 transition layer and a copper plating layer, prepared via a molten salt method and chemical plating, enhances interfacial bonding and thermal conductivity.
The composite material achieves high density and improved thermal conductivity, reducing the risk of debonding and enhancing stability for high-power electronic components.
Smart Images

Figure CN119061387A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of composite materials, in particular to a diamond-copper composite material and a preparation method thereof. Background Art
[0002] With the development of emerging technologies such as artificial intelligence, 5G, and the Internet of Things, the demand for semiconductor products with higher performance and lower energy consumption has increased significantly. However, the advantages of high-frequency and high-power performance have not been fully utilized due to the problem of heat junction in the active area. Traditional substrate and packaging heat dissipation technology is difficult to solve the "heat" bottleneck problem.
[0003] Diamond-copper composite materials have the advantages of low density, high thermal conductivity and adjustable thermal expansion coefficient, and have become the research focus of the new generation of thermal management materials. However, the wettability between diamond and copper is very poor. Even under high temperature conditions, the contact angle between the two is still as high as 128°, and diamond and copper do not react chemically with each other. The general sintering preparation process often makes it difficult to directly and effectively bond the interface between diamond and copper, resulting in poor density of the prepared composite material. In addition, there is a huge difference in the thermal expansion coefficients of diamond and copper, and thermal stress will appear at the interface between the two phases of the composite material, thereby greatly increasing the risk of debonding at the interface of the diamond-copper composite material, seriously affecting the working stability of the diamond-copper composite material. Summary of the invention
[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a diamond-copper composite material and a preparation method thereof.
[0005] The technical solutions adopted are as follows:
[0006] A diamond-copper composite material comprises a diamond matrix, a transition layer and a copper plating layer;
[0007] The transition layer includes Ti 3-x Zr x SiC2;
[0008] Among them, 0<x≤0.5.
[0009] Furthermore, 0.1≤x≤0.3.
[0010] Further, x=0.27.
[0011] The present invention also provides a method for preparing a diamond-copper composite material:
[0012] The molten salt method is used to form Ti-containing 3-x Zr x A transition layer of SiC2 is formed, and then a copper plating layer is formed on the transition layer by chemical plating.
[0013] Furthermore, the preparation method of the diamond-copper composite material provided by the present invention is as follows:
[0014] First, Zr powder, Ti powder and Si powder are mixed and ground to obtain a first mixed material, then diamond powder is mixed with the first mixed material to obtain a second mixed material, and then the second mixed material is mixed with a molten salt medium to obtain a third mixed material. Under argon protection, the third mixed material is heated to 1250-1450° C., kept warm for 1-5 hours, and then cooled to room temperature, washed with water and ethanol, and then dried to obtain an intermediate;
[0015] The intermediate is added into the plating solution to carry out chemical copper plating at 40-50°C, and the product is washed with water and then dried.
[0016] Furthermore, the mass ratio of diamond powder to the first mixed material is 5-10:1.
[0017] Furthermore, the mass ratio of the second mixed material to the molten salt medium is 1-3:1-3, and the mass ratio of the second mixed material to the molten salt medium is preferably 1:1.
[0018] Furthermore, the molten salt medium includes sodium chloride and potassium chloride, the mass ratio of the sodium chloride to the potassium chloride is 1-5:1-5, and the mass ratio of the sodium chloride to the potassium chloride is preferably 1:1.
[0019] Furthermore, the intermediate is also subjected to sensitization treatment, and the sensitization treatment is specifically as follows:
[0020] The stannous chloride and hydrochloric acid solution are mixed to obtain a sensitizing solution, the intermediate is added to the sensitizing solution and ultrasonically treated for 10-30 minutes, then filtered out, washed with water, and dried.
[0021] Furthermore, the pH of the plating solution is 12-13, and each 1L of the plating solution includes the following components:
[0022] Copper sulfate 7-10g / L, glyoxylic acid 3-5mg / L, disodium ethylenediaminetetraacetate 15-25g / L, 2,2'-bipyridine 0.8-1.2g / L, polyethylene glycol 1-5mg / L, and the balance is water.
[0023] Beneficial effects of the present invention:
[0024] The present invention provides a diamond-copper composite material. By setting a transition layer, a diamond substrate and a copper plating layer can be directly and effectively bonded at the interface, thereby improving the density and thermal conductivity of the prepared diamond-copper composite material, and forming a thermal expansion coefficient gradient, thereby greatly reducing the risk of debonding at the interface of the diamond-copper composite material and improving the working stability of the diamond-copper composite material.
[0025] Ti3SiC2 has the characteristics of both metal and ceramic. In this application, it is doped with Zr to form Ti 3-x Zr x SiC2 solid solution can improve the hardness, elastic modulus and affinity of the transition layer with the copper coating through the strengthening effect brought by Zr atoms, so that the transition layer and the copper coating can be more closely combined. Moreover, after the transition layer is formed, it does not need to be activated by palladium. After sensitization treatment, chemical copper plating can be directly performed, which improves production efficiency, avoids the use of relatively expensive palladium chloride, and reduces production costs.
[0026] After testing, it is found that the diamond-copper composite material prepared by the present invention has high density and good thermal conductivity, and can be used as a high-performance thermal management material in high-power electronic components. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the surface microscopic morphology of the diamond-copper composite material prepared in Example 1. It can be seen that the copper plating layer on its surface is complete and dense, and has good overall uniformity and flatness. DETAILED DESCRIPTION
[0028] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0029] Embodiment 1:
[0030] This embodiment provides a diamond-copper composite material, including a diamond substrate, a transition layer and a copper plating layer;
[0031] The transition layer includes Ti 2.73 Zr 0.27 SiC2;
[0032] The preparation method of the above diamond-copper composite material is as follows:
[0033] Weigh Zr powder, Ti powder and Si powder according to a molar ratio of 0.27:2.73:1, mix and grind the Zr powder, Ti powder and Si powder in a mortar for 5 hours to obtain a first mixed material, then mix 120 mesh diamond powder with the first mixed material in a mass ratio of 8:1 to obtain a second mixed material, then mix the same mass of the second mixed material with a molten salt medium (the mass ratio of sodium chloride and potassium chloride is 1:1) to obtain a third mixed material, and under argon protection, heat the third mixed material to 1350°C at a rate of 10°C / min, keep it warm for 2 hours, then cool it to room temperature, wash it repeatedly with water and ethanol, and then dry it to obtain an intermediate;
[0034] Dilute 50 ml of concentrated hydrochloric acid with 500 ml of water to prepare a hydrochloric acid solution, mix 25 g of stannous chloride and the hydrochloric acid solution to obtain a sensitizing solution, add 50 g of the intermediate to the sensitizing solution and ultrasonically treat for 30 minutes, filter out the solid, wash with water until neutral and dry, add it to a 50°C plating solution for chemical copper plating for 90 minutes, filter after chemical copper plating, and wash the product with water and dry it.
[0035] The pH of the plating solution is 12-13, and each 1L of plating solution includes the following ingredients:
[0036] Copper sulfate 8g / L, glyoxylic acid 45mg / L, disodium ethylenediaminetetraacetate 20g / L, 2,2'-bipyridine 1g / L, polyethylene glycol 2000 2mg / L, and the balance is water.
[0037] Embodiment 2:
[0038] This embodiment provides a diamond-copper composite material, including a diamond substrate, a transition layer and a copper plating layer;
[0039] The transition layer includes Ti 2.73 Zr 0.27 SiC2;
[0040] The preparation method of the above diamond-copper composite material is as follows:
[0041] Weigh Zr powder, Ti powder and Si powder according to a molar ratio of 0.27:2.73:1, mix and grind the Zr powder, Ti powder and Si powder in a mortar for 5 hours to obtain a first mixed material, then mix 120 mesh diamond powder with the first mixed material in a mass ratio of 8:1 to obtain a second mixed material, then mix the same mass of the second mixed material with a molten salt medium (the mass ratio of sodium chloride and potassium chloride is 1:1) to obtain a third mixed material, and under argon protection, heat the third mixed material to 1450°C at a rate of 10°C / min, keep it warm for 2 hours, then cool it to room temperature, wash it repeatedly with water and ethanol, and then dry it to obtain an intermediate;
[0042] Dilute 50 ml of concentrated hydrochloric acid with 500 ml of water to prepare a hydrochloric acid solution, mix 25 g of stannous chloride and the hydrochloric acid solution to obtain a sensitizing solution, add 50 g of the intermediate to the sensitizing solution and ultrasonically treat for 30 minutes, filter out the solid, wash with water until neutral and dry, add it to a 50°C plating solution for chemical copper plating for 90 minutes, filter after chemical copper plating, and wash the product with water and dry it.
[0043] The pH of the plating solution is 12-13, and each 1L of plating solution includes the following ingredients:
[0044] Copper sulfate 8g / L, glyoxylic acid 45mg / L, disodium ethylenediaminetetraacetate 20g / L, 2,2'-bipyridine 1g / L, polyethylene glycol 2000 2mg / L, and the balance is water.
[0045] Embodiment 3:
[0046] This embodiment provides a diamond-copper composite material, including a diamond substrate, a transition layer and a copper plating layer;
[0047] The transition layer includes Ti 2.73 Zr 0.27 SiC2;
[0048] The preparation method of the above diamond-copper composite material is as follows:
[0049] Weigh Zr powder, Ti powder and Si powder according to a molar ratio of 0.27:2.73:1, mix and grind the Zr powder, Ti powder and Si powder in a mortar for 5 hours to obtain a first mixed material, then mix 120 mesh diamond powder with the first mixed material in a mass ratio of 8:1 to obtain a second mixed material, then mix the same mass of the second mixed material with a molten salt medium (the mass ratio of sodium chloride and potassium chloride is 1:1) to obtain a third mixed material, and under argon protection, heat the third mixed material to 1250°C at a rate of 10°C / min, keep it warm for 2 hours, then cool it to room temperature, wash it repeatedly with water and ethanol, and then dry it to obtain an intermediate;
[0050] Dilute 50 ml of concentrated hydrochloric acid with 500 ml of water to prepare a hydrochloric acid solution, mix 25 g of stannous chloride and the hydrochloric acid solution to obtain a sensitizing solution, add 50 g of the intermediate to the sensitizing solution and ultrasonically treat for 30 minutes, filter out the solid, wash with water until neutral and dry, add it to a 50°C plating solution for chemical copper plating for 90 minutes, filter after chemical copper plating, and wash the product with water and dry it.
[0051] The pH of the plating solution is 12-13, and each 1L of plating solution includes the following ingredients:
[0052] Copper sulfate 8g / L, glyoxylic acid 45mg / L, disodium ethylenediaminetetraacetate 20g / L, 2,2'-bipyridine 1g / L, polyethylene glycol 2000 2mg / L, and the balance is water.
[0053] Embodiment 4:
[0054] The method is basically the same as Example 1, except that the pH value of the plating solution is 12-13, and each 1L of the plating solution includes the following components:
[0055] Copper sulfate 10g / L, glyoxylic acid 3mg / L, disodium ethylenediaminetetraacetate 25g / L, 2,2'-bipyridine 0.8g / L, polyethylene glycol 2000 5mg / L, and the balance is water.
[0056] Embodiment 5:
[0057] The method is basically the same as Example 1, except that the pH value of the plating solution is 12-13, and each 1L of the plating solution includes the following components:
[0058] Copper sulfate 7g / L, glyoxylic acid 5mg / L, disodium ethylenediaminetetraacetate 15g / L, 2,2'-bipyridine 1.2g / L, polyethylene glycol 2000 1mg / L, and the balance is water.
[0059] Comparative Example 1:
[0060] The present invention is basically the same as Example 1, except that the present embodiment provides a diamond-copper composite material, including a diamond substrate, a transition layer and a copper plating layer;
[0061] The transition layer includes Ti3SiC2;
[0062] The preparation method of the above diamond-copper composite material is as follows:
[0063] Ti powder and Si powder were weighed in a molar ratio of 3:1, and the Ti powder and Si powder were mixed and ground in a mortar for 5 hours to obtain a first mixed material, and then 120 mesh diamond powder was mixed with the first mixed material in a mass ratio of 8:1 to obtain a second mixed material, and then the same mass of the second mixed material was mixed with a molten salt medium (the mass ratio of sodium chloride and potassium chloride was 1:1) to obtain a third mixed material, and under argon protection, the third mixed material was heated to 1350°C at a rate of 10°C / min, kept warm for 2 hours, and then cooled to room temperature, and washed repeatedly with water and ethanol and then dried to obtain an intermediate;
[0064] Dilute 50 ml of concentrated hydrochloric acid with 500 ml of water to prepare a hydrochloric acid solution, mix 25 g of stannous chloride and the hydrochloric acid solution to obtain a sensitizing solution, add 50 g of the intermediate to the sensitizing solution and ultrasonically treat for 30 minutes, filter out the solid, wash with water until neutral and dry, add it to a 50°C plating solution for chemical copper plating for 90 minutes, filter after chemical copper plating, and wash the product with water and dry it.
[0065] The pH of the plating solution is 12-13, and each 1L of plating solution includes the following ingredients:
[0066] Copper sulfate 8g / L, glyoxylic acid 45mg / L, disodium ethylenediaminetetraacetate 20g / L, 2,2'-bipyridine 1g / L, polyethylene glycol 2000 2mg / L, and the balance is water.
[0067] Comparative Example 2:
[0068] The method is basically the same as Example 1, except that the intermediate is not subjected to sensitization treatment;
[0069] This embodiment provides a diamond-copper composite material, including a diamond substrate, a transition layer and a copper plating layer;
[0070] The transition layer includes Ti 2.73 Zr 0.27 SiC2;
[0071] The preparation method of the above diamond-copper composite material is as follows:
[0072] Weigh Zr powder, Ti powder and Si powder according to a molar ratio of 0.27:2.73:1, mix and grind the Zr powder, Ti powder and Si powder in a mortar for 5 hours to obtain a first mixed material, then mix 120 mesh diamond powder with the first mixed material in a mass ratio of 8:1 to obtain a second mixed material, then mix the same mass of the second mixed material with a molten salt medium (the mass ratio of sodium chloride and potassium chloride is 1:1) to obtain a third mixed material, and under argon protection, heat the third mixed material to 1350°C at a rate of 10°C / min, keep it warm for 2 hours, then cool it to room temperature, wash it repeatedly with water and ethanol, and then dry it to obtain an intermediate;
[0073] The intermediate is added into a 50°C plating solution for chemical copper plating for 90 minutes. After the chemical copper plating, the product is filtered and washed with water and then dried.
[0074] The pH of the plating solution is 12-13, and each 1L of plating solution includes the following ingredients:
[0075] Copper sulfate 8g / L, glyoxylic acid 45mg / L, disodium ethylenediaminetetraacetate 20g / L, 2,2'-bipyridine 1g / L, polyethylene glycol 2000 2mg / L, and the balance is water.
[0076] Performance Testing:
[0077] The diamond-copper composite materials prepared in Examples 1-5 and Comparative Examples 1-2 were used as samples for performance testing;
[0078] The density of the samples was measured by Archimedes drainage method;
[0079] The thermal conductivity of the sample was measured using the laser flash method using a LFA457 laser thermal conductivity meter.
[0080] The test results are shown in Table 1 below:
[0081] Table 1:
[0082]
[0083] It can be seen from Table 1 above that the diamond-copper composite material prepared in the present invention has high density and good thermal conductivity.
[0084] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A diamond-copper composite material, characterized in that: It includes a diamond substrate, a transition layer and a copper plating layer; The transition layer includes Ti 3-x Zr x SiC2; Among them, 0<x≤0.
5.
2. The diamond-copper composite material according to claim 1, characterized in that: 0.1≤x≤0.3。 3. The diamond-copper composite material according to claim 1, characterized in that: x=0.27。 4. A method for preparing a diamond-copper composite material according to any one of claims 1 to 3, characterized in that: The molten salt method is used to form Ti-containing 3-x Zr x A transition layer of SiC2 is formed, and then a copper plating layer is formed on the transition layer by chemical plating.
5. The method for preparing the diamond-copper composite material according to claim 4, characterized in that: The details are as follows: First, Zr powder, Ti powder and Si powder are mixed and ground to obtain a first mixed material, then diamond powder is mixed with the first mixed material to obtain a second mixed material, and then the second mixed material is mixed with a molten salt medium to obtain a third mixed material. Under argon protection, the third mixed material is heated to 1250-1450° C., kept warm for 1-5 hours, and then cooled to room temperature, washed with water and ethanol, and then dried to obtain an intermediate; The intermediate is added into the plating solution to carry out chemical copper plating at 40-50°C, and the product is washed with water and then dried.
6. The method for preparing the diamond-copper composite material according to claim 5, characterized in that: The mass ratio of diamond powder to the first mixed material is 5-10:
1.
7. The method for preparing the diamond-copper composite material according to claim 5, characterized in that: The mass ratio of the second mixed material to the molten salt medium is 1-3:1-3, and the mass ratio of the second mixed material to the molten salt medium is preferably 1:
1.
8. The method for preparing the diamond-copper composite material according to claim 5, characterized in that: The molten salt medium includes sodium chloride and potassium chloride, the mass ratio of the sodium chloride to the potassium chloride is 1-5:1-5, and the mass ratio of the sodium chloride to the potassium chloride is preferably 1:
1.
9. The method for preparing the diamond-copper composite material according to claim 5, characterized in that: The intermediate is also subjected to sensitization treatment, and the sensitization treatment is specifically as follows: The stannous chloride and hydrochloric acid solution are mixed to obtain a sensitizing solution, the intermediate is added to the sensitizing solution and ultrasonically treated for 10-30 minutes, then filtered out, washed with water, and dried.
10. The method for preparing the diamond-copper composite material according to claim 5, characterized in that: The pH of the plating solution is 12-13, and each 1L of plating solution includes the following ingredients: Copper sulfate 7-10g / L, glyoxylic acid 3-5mg / L, disodium ethylenediaminetetraacetate 15-25g / L, 2,2'-bipyridine 0.8-1.2g / L, polyethylene glycol 1-5mg / L, and the balance is water.