Low-ruthenium ternary metal oxide electrolyzed water catalyst and preparation method thereof
A low-ruthenium ternary metal oxide catalyst addresses stability and cost issues in water electrolysis by using cheaper antimony and tin oxides, achieving high OER activity and stability for industrial applications.
Patent Information
- Application Number
- CN202411031455.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-12-03
AI Technical Summary
Existing water electrolysis technologies face challenges with expensive precious metal-based anode catalysts, particularly Ru-based materials, which have stability issues and slow kinetics for oxygen evolution reaction (OER) under acidic conditions.
A low-ruthenium ternary metal oxide catalyst with a molecular formula Ru x Sn 1-x Sb y O z (0 < x < 1, 0 < y < 1, 2 < z < 4) is synthesized using a simple wet chemical method, incorporating cheaper antimony and tin oxides to reduce ruthenium content and enhance stability and activity.
The catalyst demonstrates high OER activity with reduced overpotential (174 mV at 10 mA cm -2) and excellent stability in acidic environments, facilitating industrial mass production with lower equipment and operation costs.
Smart Images

Figure HDA0004970030100000011 
Figure HDA0004970030100000012 
Figure HDA0004970030100000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water electrolysis catalysts, and specifically relates to a low-ruthenium ternary metal oxide water electrolysis catalyst and a preparation method thereof. Background Art
[0002] In recent years, renewable energy has developed rapidly. However, due to its intermittent, volatile and random characteristics, it has a great impact on the power grid, resulting in serious power abandonment. Using renewable energy to generate electricity and produce hydrogen by electrolysis of water can effectively solve the problem of renewable energy power abandonment. The technology of hydrogen production by electrolysis of water was invented in 1789, developed rapidly in the 1920s, and further attracted the attention of scientific researchers in the 1970s due to the introduction of the concept of hydrogen economy. At present, the mature hydrogen production technologies by electrolysis of water mainly include proton exchange membrane water electrolysis (PEMWE) hydrogen production technology and alkaline water electrolysis hydrogen production technology. Among them, the proton exchange membrane water electrolysis hydrogen production technology has excellent performance, with the characteristics of high current density, low ohmic loss, high gas purity and strong flexibility. Therefore, it is one of the green hydrogen preparation technologies that are most suitable for renewable energy.
[0003] However, the corresponding electrode catalyst materials are all precious metals and are expensive; the reaction occurring at the anode is an oxygen evolution reaction (OER) with four electron transfer, which has slow kinetics and requires extremely high activity of the anode catalyst; during anode electrolysis, a high oxidation potential is applied to the anode and the local environment is acidic, which requires extremely high corrosion resistance of the anode catalyst. Therefore, the anode catalyst is one of the key bottleneck technologies in PEMWE technology. At present, the commonly used anode catalyst materials are mainly iridium (Ir)-based materials and ruthenium (Ru)-based materials. Compared with Ir-based materials, Ru-based materials have lower costs, higher activities, and better application prospects, but their stability is biased.
[0004] In summary, when designing Ru-based materials as anode catalysts, the amount of precious metals should be reduced, the stability of the Ru-based catalysts should be improved, the activity of the Ru-based catalysts should be maintained, and the preparation process should be simple and easy. Based on this, the present invention is proposed. Summary of the invention
[0005] The technical problem solved by the present invention is to propose an anode catalyst for water electrolysis and a preparation method thereof, wherein the catalyst has a small amount of precious metal added, takes into account both OER catalytic activity and stability, and has a simple preparation process.
[0006] The technical means adopted by the present invention are: a low-ruthenium ternary metal oxide water electrolysis catalyst, the catalyst molecular formula is Ru x Sn1-x Sb y O z , where 0 <x<1,0<y<1,2<z<4。
[0007] 2. The water electrolysis catalyst as claimed in claim 1, characterized in that its molecular formula is Ru 0.5 Sn 0.5 Sb 0.2 O 2.5 , which showed high activity under acidic conditions at 10 mA cm -2 The overpotential is 174mV.
[0008] A method for synthesizing a water electrolysis catalyst comprises the following steps:
[0009] S1, adding a ruthenium salt precursor, an antimony salt precursor and a tin salt precursor to an alcohol solution, then adding a small amount of hydrochloric acid, and ultrasonicating to obtain a solution;
[0010] S2, evaporating the solution to dryness and drying to obtain a black solid;
[0011] S3, calcining the solid obtained in S2 to obtain a metal oxide solid powder; oxidizing the precursor in an air atmosphere to become an oxide;
[0012] S4, grinding the powder obtained in S3;
[0013] S5, washing the ground solid powder by centrifugation, and freeze-drying to obtain the catalyst.
[0014] Among the raw materials described in step S1, the ruthenium salt precursor is one or more of anhydrous ruthenium trichloride and ruthenium trichloride hydrate; the antimony salt precursor is one or more of antimony trichloride and antimony pentachloride; the tin salt precursor is one or more of anhydrous tin tetrachloride and tin tetrachloride pentahydrate.
[0015] The evaporation and drying temperature in step S2 is 40-60° C., and the evaporation and drying time are both 8-12 hours.
[0016] The heat treatment temperature in step S3 is 300° C. and the time is 0.5-2 h.
[0017] In step S2, evaporation is performed in an oil bath; in step S3, heat treatment is performed in a muffle furnace; in step S4, an agate mortar is used.
[0018] The alcohol solution in step S1 is ethanol or isopropanol; the hydrochloric acid is a 37% hydrochloric acid solution; the ultrasound is set to a frequency of 12-24kHz, a total power of 2000W, an output power of 20%-50% of the total power, and an ultrasound duration of 10-30min
[0019] Application of water electrolysis catalyst in oxygen evolution reaction in acidic environment.
[0020] Compared with the prior art, the low-ruthenium ternary metal oxide water electrolysis catalyst and the preparation method thereof disclosed in the present invention have the following beneficial effects:
[0021] The invention is synthesized by a simple wet chemical method, has low equipment cost and operation cost, and is easy to realize industrial mass production.
[0022] The present invention uses cheaper oxides of antimony and tin as matrix materials in the synthesis process of ruthenium-based catalysts, thereby reducing the amount of precious metal ruthenium.
[0023] The oxides of antimony and tin are acid-resistant oxides. After forming ternary metal oxides with ruthenium, they can be used as electrocatalysts for OER, remain stable during oxygen evolution, and are not corroded, thus improving the stability of ruthenium-based catalysts.
[0024] The ruthenium element in the catalyst of the present invention interacts with the antimony and tin elements, optimizes the internal electronic structure, and greatly reduces the overpotential of OER. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the XRD pattern of the catalyst prepared in Example 1 of the present invention.
[0026] Figure 2 This is the TEM spectrum of the catalyst prepared in Example 1 of the present invention.
[0027] Figure 3 This is a graph of the catalytic activity of the catalyst prepared in Example 1 of the present invention in oxygen evolution reaction in 0.5M H2SO4 measured by linear voltammetric scanning in a three-electrode system.
[0028] Figure 4 This is a graph of the catalytic stability of the catalyst prepared in Example 1 of the present invention in the oxygen evolution reaction in 0.5MH2SO4 measured by chronopotentiometry in a three-electrode system. DETAILED DESCRIPTION
[0029] The present invention provides a low-ruthenium ternary metal oxide water electrolysis catalyst, the catalyst molecular formula is Ru x Sn 1-x Sb y O z , where 0 <x<1,0<y<1,2<z<4。
[0030] The preparation method comprises the following steps:
[0031] S1, adding a ruthenium salt precursor, an antimony salt precursor and a tin salt precursor to an alcohol solution, then adding a small amount of hydrochloric acid, and ultrasonicating to obtain a solution;
[0032] S2, evaporate the solution to dryness and dry to obtain a black solid; generally evaporate to dryness in an oil bath
[0033] S3, calcining the solid obtained in S2 to obtain a metal oxide solid powder; generally, heat treatment is performed in a muffle furnace to oxidize the precursor in an air atmosphere to become an oxide;
[0034] S4, grinding the powder obtained in S3; generally using an agate mortar;
[0035] S5, washing the ground solid powder by centrifugation, and freeze-drying to obtain the catalyst.
[0036] Among the raw materials described in step S1, the ruthenium salt precursor is one or more of anhydrous ruthenium trichloride and ruthenium trichloride hydrate; the antimony salt precursor is one or more of antimony trichloride and antimony pentachloride; the tin salt precursor is one or more of anhydrous tin tetrachloride and tin tetrachloride pentahydrate.
[0037] The evaporation and drying temperature in step S2 is 40-60° C., and the evaporation and drying time are both 8-12 hours.
[0038] Wherein, the heat treatment temperature in step S3 is 300° C. and the time is 0.5-2 h.
[0039] Wherein, the alcohol solution described in step S1 is ethanol or isopropanol; the hydrochloric acid is a 37% hydrochloric acid solution; the ultrasound is set to a frequency of 12-24kHz, a total power of the equipment is 2000W, an output power is 20%-50% of the total power, and the ultrasound duration is 10-30min.
[0040] Example 1
[0041] S1, add 0.415 g of hydrated ruthenium chloride, 0.085 g of anhydrous antimony trichloride and 0.614 g of tin chloride pentahydrate to 10 mL of ethanol, then add 0.5 mL of hydrochloric acid, and ultrasonicate for 0.5 h to obtain a solution;
[0042] S2, evaporate the solution to dryness in an oil bath at 60°C for 12 h, and then dry it in a forced air oven at 60°C for 12 h to obtain a black solid;
[0043] S3, the solid obtained in S2 is placed in a muffle furnace for calcination at a heating rate of 10 °C min -1 , raised to 300°C, calcined for 0.5h to obtain a metal oxide solid powder;
[0044] S4, grinding the powder obtained in S3; generally using an agate mortar;
[0045] S5, centrifuging the ground solid powder, washing it with deionized water, and freeze-drying it to obtain the catalyst.
[0046] The crystal structure of the catalyst material obtained above is Figure 1 The XRD diffraction spectrum in the figure shows that it is a tetragonal crystal system, the diffraction peaks corresponding to each crystal plane are obvious, and the crystallinity is good.
[0047] The catalyst material is obtained by Figure 2 The TEM photos in the figure can be confirmed to be nanoparticles with a size of 5-10nm and a relatively uniform distribution.
[0048] Example 2
[0049] The preparation steps and conditions are basically the same as those in Example 1, except that the amount of hydrated ruthenium chloride added in S1 is changed to 0.249 g.
[0050] Example 3
[0051] The preparation steps and conditions are basically the same as those in Example 1, except that the amount of hydrated ruthenium chloride added in S1 is changed to 0.083 g.
[0052] Application Example 1
[0053] The Ru obtained in Example 1 of the present invention 0.5 Sn 0.5 Sb 0.2 O 2.5 It is used for oxygen evolution reaction in acidic electrolyte. In the three-electrode test system, graphite is used as the counter electrode and silver-silver chloride is used as the reference electrode. The test system selects 0.5 mol L -1 H2SO4 is the electrolyte.
[0054] S1: 10 mg of supported catalyst was added to 5 mL of a mixed solvent of water and isopropanol, and 50 μL of Nafion solution (5 wt%) was added dropwise to form a uniform catalyst ink after ultrasonic treatment. A certain amount of ink was then evenly applied to a glassy carbon rotating disk electrode with a diameter of 5 mm. After drying, it was used as a working electrode for testing. The loading was 0.2 mg cm -2 , the disc speed in the test was 1600rpm.
[0055] S2 uses linear voltammetry to test the electrocatalytic oxygen evolution performance of the sample. The linear voltammetry scan rate is 5mVs -1 , potential range 1.35-1.75V (vs.RHE),
[0056] S3 The stability of the catalyst obtained in Example 1 of the present invention was tested by chronopotentiometry, where the current density was set to 50 mA cm -2 .
[0057] The catalytic activity of the catalyst material prepared above is good, reaching 10 mA cm in 0.5 M H2SO4 solution. -2 The overpotential required for the current density is only 174mV.
[0058] The catalytic stability of the catalyst material prepared above is good, and the -2 At a current density of 1.5 Å, the catalytic activity can be maintained for more than 70 h.
[0059] Embodiments 2 and 3 of the present invention can also achieve the same beneficial effects as embodiment 1.
Claims
1. A low-ruthenium ternary metal oxide water electrolysis catalyst, characterized in that the catalyst molecular formula is Ru x Sn 1- x Sb y O z , where 0 <x<1,0<y<1,2<z<4。 2. The water electrolysis catalyst according to claim 1, characterized in that Its molecular formula is Ru 0.5 Sn 0.5 Sb 0.2 O 2.5 , which showed high activity under acidic conditions at 10 mA cm -2 The overpotential is 174mV.
3. A method for synthesizing a water electrolysis catalyst as claimed in claims 1-2, characterized in that: The following steps are involved: S1, adding a ruthenium salt precursor, an antimony salt precursor and a tin salt precursor to an alcohol solution, then adding a small amount of hydrochloric acid, and ultrasonicating to obtain a solution; S2, evaporating the solution to dryness and drying to obtain a black solid; S3, calcining the solid obtained in S2 to obtain a metal oxide solid powder; oxidizing the precursor in an air atmosphere to become an oxide; S4, grinding the powder obtained in S3; S5, washing the ground solid powder by centrifugation, and freeze-drying to obtain the catalyst.
4. The method for synthesizing the water electrolysis catalyst as claimed in claim 3, characterized in that: Among the raw materials described in step S1, the ruthenium salt precursor is one or more of anhydrous ruthenium trichloride and ruthenium trichloride hydrate; the antimony salt precursor is one or more of antimony trichloride and antimony pentachloride; the tin salt precursor is one or more of anhydrous tin tetrachloride and tin tetrachloride pentahydrate.
5. The method for synthesizing the water electrolysis catalyst according to claim 3, characterized in that: The evaporation and drying temperature in step S2 is 40-60° C., and the evaporation and drying time are both 8-12 hours.
6. The method for synthesizing the water electrolysis catalyst according to claim 3, characterized in that: The heat treatment temperature in step S3 is 300° C. and the time is 0.5-2 h.
7. The method for synthesizing the water electrolysis catalyst according to claim 3, characterized in that: In step S2, evaporation is performed in an oil bath; in step S3, heat treatment is performed in a muffle furnace; in step S4, an agate mortar is used.
8. The method for synthesizing the water electrolysis catalyst according to claim 3, characterized in that: The alcohol solution described in step S1 is ethanol or isopropanol; the hydrochloric acid is a 37% hydrochloric acid solution; the ultrasound is set to a frequency of 12-24kHz, a total power of the equipment of 2000W, an output power of 20%-50% of the total power, and an ultrasound duration of 10-30min.
9. Use of the water electrolysis catalyst as described in claims 1-2 in oxygen evolution reaction in an acidic environment.