Electrically-assisted photocatalytic CO2 cycloaddition integrated catalytic electrode as well as preparation method and application thereof
Through the electrically assisted photocatalytic technology of loading conjugated polymers on the conductive self-support, the high temperature, high pressure and high cost problems of the existing CO2 cycloaddition reaction process are solved, and efficient CO2 cycloaddition under normal temperature and pressure are achieved. , significantly improves the efficiency and yield of the catalyst and has industrial application value.
Patent Information
- Application Number
- CN202411209484.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing CO2 cycloaddition reaction processes have problems such as high temperature and high pressure, complex processes, high pollution, high energy consumption and low catalytic efficiency. The prepared catalysts are costly, difficult to synthesize, and low yield.
Using an electrically assisted photocatalytic CO2 cycloaddition integrated catalytic electrode, the conjugated polymer is loaded on the conductive self-support and the combination of photocatalysis and electrocatalysis can realize CO2 and epoxide at normal temperature and pressure. Cycloaddition reaction to prepare cyclic carbonate.
It realizes high efficiency, low cost and low energy consumption of CO2 cycloaddition reaction, improves the efficiency and yield of the catalyst, and is suitable for industrial applications.
Smart Images

Figure CN119061434A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalytic preparation, and specifically relates to an electrically assisted photocatalytic CO 2 Cycloaddition integrated catalytic electrode and preparation method and application thereof. Background Art
[0002] As the main component of greenhouse gases, the concentration of carbon dioxide in the atmosphere affects the Earth's heat balance. The chemical transformation of carbon dioxide is an important way to slow down its accumulation in the atmosphere and obtain value-added chemicals. Among the various chemical fixation methods of carbon dioxide, the carbon dioxide cycloaddition reaction is the most important for CO2 fixation. 2 The utilization rate is 100%, and its product (cyclic carbonate) is widely used as electrolyte for secondary batteries, which has huge economic benefits.
[0003] However, CO 2 It is a thermodynamically very stable inert molecule. The existing preparation process of cyclic carbonates uses metal organic frameworks (MOFs), Schiff bases, ionic liquids, etc. as catalysts, and is carried out at high temperature (100-160°C) and high pressure (1-5MPa). This preparation process is complex in synthesis, highly polluting, has high reaction energy consumption, and low catalytic efficiency. It is urgent to develop a method that can achieve CO at room temperature and pressure. 2 Cycloaddition reaction technology.
[0004] Compared with photocatalysis, electrocatalysis is more efficient. Khoshro et al. (Synthesis of cyclic carbonates through cycloaddition of electrocatalytic activated CO 2 to epoxides under mild conditions) found that under the electrocatalysis of nickel (II) complexes, CO 2 It can undergo cycloaddition reaction with epoxides under mild conditions (atmospheric CO pressure, room temperature) to obtain cyclic carbonates. Yang et al. (Electrochemical activation of carbon dioxide in ionic liquid: synthesis of cyclic carbonates at mild reaction conditions) used ionic liquid as a conductive medium to electrochemically activate CO 2 At room temperature, without any additional supporting electrolyte or catalyst, CO 2 It can undergo cycloaddition reaction with epoxides to synthesize cyclic carbonates. Zhang et al. (Highly efficient electrocatalysis for the fixation of CO2 into cyclic carbonates with carbon sphere-loaded copper nanoparticles cathode material) reported a carbon sphere-loaded highly dispersed Cu nanoparticle catalyst that can electrocatalyze CO at room temperature and atmospheric pressure. 2 It reacts with epoxides to form cyclic carbonates.
[0005] The above preparation methods still have the problems of high cost, difficult synthesis and low yield. 2 Cycloaddition reactions still have problems such as low system efficiency and slow conversion rate. Summary of the invention
[0006] The purpose of the present invention is to provide an electrically assisted photocatalytic CO 2 A cycloaddition integrated catalytic electrode and a preparation method and application thereof, the method is easy to obtain the target product, has low cost and high yield, and the prepared integrated catalytic electrode is applied to CO 2 In the preparation of cyclic carbonates by cycloaddition, the reaction efficiency and conversion rate can be improved.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is: an electrically assisted photocatalytic CO 2 The preparation method of the cycloaddition integrated catalytic electrode comprises the following steps:
[0008] S1, pickling the conductive self-supporting body with dilute hydrochloric acid, then washing with deionized water and acetone, drying, and slicing for later use;
[0009] S2, weighing a certain amount of metal precursor and dissolving it in a solvent, stirring and dispersing it evenly to form a solution, and then taking a piece of the conductive self-supporting body treated in step S1 and immersing it in the solution, so that the metal precursor is fully adsorbed on the conductive self-supporting body;
[0010] S3, weighing a certain amount of organic ligand and adding it to the mixed solution obtained in step S2, stirring and dispersing it evenly;
[0011] S4, transferring the solution obtained in step S3 to a sealed container with a lid, heating to 80-220° C., and maintaining for 2-72 hours to obtain a conductive self-supporting body loaded with a conjugated polymer;
[0012] S5. After washing the conductive self-supporting body loaded with the conjugated polymer obtained in step S4, the conductive self-supporting body is placed in a vacuum drying oven for drying to obtain an integrated catalytic electrode.
[0013] Preferably, in step S1, the conductive self-supporting body is one of a conductive metal mesh, a conductive metal foam, carbon paper, a carbon cloth, and a carbonized wood; the concentration of the dilute hydrochloric acid is 1 to 5 mol / L, the pickling temperature is 20 to 80° C., and the pickling time is 0.5 to 6 h; and the surface is washed three times with deionized water and acetone respectively.
[0014] Preferably, in step S2, the metal precursor is one or two of iron nitrate, iron sulfate, iron hydrochloride, cobalt nitrate, cobalt sulfate, cobalt hydrochloride, nickel nitrate, nickel sulfate, nickel hydrochloride, copper nitrate, copper sulfate, copper hydrochloride, zinc nitrate, zinc sulfate, and zinc hydrochloride; the solvent is one or two of methanol, ethanol, ethylene glycol, pentanol, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, toluene, xylene, and mesitylene; and the concentration of the metal precursor in the solution is 0.001 to 1 mol / L.
[0015] Preferably, in step S3, the organic ligand is one of 1,2,4,5-tetracyanobenzene, 1,2,4,5-tetraethynylbenzene, tetrakis(4-carboxyphenyl)porphine, 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin, 2,3,9,10,16,17,23,24-octaaminometallicphthalocyanine compounds, and 2,3,9,10,16,17,23,24-octahydroxymetallicphthalocyanine compounds; and the molar ratio between the organic ligand and the metal precursor is (0.2-5):1.
[0016] Preferably, in step S4, the structure of the conjugated polymer contains a metal-phthalocyanine unit or a metal-porphyrin unit.
[0017] Preferably, in step S5, the substrate is washed with anhydrous ethanol and deionized water three times respectively; the drying temperature is 40-60°C, and the drying time is 11-13 hours; in the integrated catalytic electrode, the loading amount of the conjugated polymer on the conductive self-supporting body is 0.1-5 mg / cm 2 .
[0018] To achieve the above object, the present invention also provides the above-mentioned electric-assisted photocatalytic CO 2 An integrated catalytic electrode obtained by the preparation method of a cycloaddition integrated catalytic electrode.
[0019] To achieve the above object, the present invention also provides the above-mentioned electrically assisted photocatalytic CO 2 Preparation method of cycloaddition integrated catalytic electrode The integrated catalytic electrode obtained in CO 2 The application of cycloaddition in the preparation of cyclic carbonates is as follows: the above-mentioned integrated catalytic electrode is used as the cathode, the magnesium rod is used as the sacrificial anode, the ionic liquid is used as the solvent and the electrolyte, the reaction substrate epoxide and the co-catalyst are added into the photoreactor, and CO is introduced.2 , a certain voltage is applied to the cathode and anode, and a simulated light source or sunlight is used for illumination to carry out a cycloaddition reaction.
[0020] Preferably, the electrically assisted photocatalytic cycloaddition reaction is carried out at room temperature, and the CO 2 The pressure is maintained at 1 atm, and the reaction time is 0.5 to 2 hours; the simulated light source uses an LED or a xenon lamp with a power of 10 to 300 W; the mass ratio of the co-catalyst to the epoxide is 1:(40 to 250); the concentration of the epoxide in the ionic liquid is 0.1 to 5 mol / L; direct current is applied to the cathode and the anode, and the voltage is -3.0 V to -1.0 V.
[0021] Preferably, the co-catalyst is tetrabutylammonium bromide; and the epoxy compound is styrene oxide.
[0022] The present invention loads conjugated polymers such as polyphthalocyanine and polyporphyrin on the basis of a conductive self-supporting body to form an integrated catalytic electrode. Among them, the conductive self-supporting body plays the role of conducting electrons and supporting / dispersing catalysts, and conjugated polymers such as two-dimensional polyphthalocyanine and polyporphyrin not only have conductivity and can accelerate electron transfer, but also have a certain light response ability and can generate photogenerated electron-hole pairs under light. Among them, the highly dispersed single metal site can be used as a catalytic center, and the porous conjugated polymer is conducive to the mass transfer and adsorption of reactant molecules. Therefore, the conjugated polymer has excellent chemical catalysis and photocatalytic activity.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] The method of the present invention is easy to obtain the target product, has low cost and high yield, and the prepared integrated catalytic electrode can realize the preparation of cyclic carbonates, has many advantages such as low cost, low energy consumption, simple process, high catalyst efficiency, and fast conversion speed. It can also realize the catalytic conversion of epoxides under natural light, and has high industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The present invention is to contain MN 4 Schematic diagram of the structure of the metal-phthalocyanine conjugated polymer with active center;
[0026] Figure 2 TEM image (a) and spherical aberration electron microscope image (b) of the conjugated polymer containing iron-phthalocyanine units prepared in Example 3. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] Unless otherwise specified, the materials and reagents used in the following examples are all commercially available.
[0029] Example 1
[0030] An electrically assisted photocatalytic CO 2 The preparation method of the cycloaddition integrated catalytic electrode comprises the following steps:
[0031] S1. Pickle the carbon paper with 3 mol / L dilute hydrochloric acid at 20°C for 6 h, then wash it with deionized water and acetone three times each, dry it, and slice it for later use;
[0032] S2. Weigh 2 mmol of ferric chloride, dissolve it in 20 ml of N,N-dimethylformamide, stir and disperse it evenly to form a solution, then take a piece of the above carbon paper and immerse it in the above solution to allow the ferric chloride to be fully adsorbed on the carbon paper;
[0033] S3, weigh 1 mmol of 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin, add it to the above solution, and stir to disperse it evenly;
[0034] S4, transferring the above solution into a sealed container with a lid, heating to 85° C., and maintaining for 24 hours to obtain carbon paper loaded with a conjugated polymer containing an iron-porphyrin unit;
[0035] S5. The carbon paper loaded with the conjugated polymer containing the iron-porphyrin unit was washed with anhydrous ethanol and deionized water for three times respectively, and dried in a vacuum drying oven at 60° C. for 12 h to obtain an integrated catalytic electrode. In the integrated catalytic electrode, the loading amount of the conjugated polymer on the carbon paper was 3 mg / cm 2 .
[0036] Example 2
[0037] An electrically assisted photocatalytic CO 2 The preparation method of the cycloaddition integrated catalytic electrode comprises the following steps:
[0038] S1. Pickle the nickel foam with 3 mol / L dilute hydrochloric acid at 40°C for 3 h, then wash it with deionized water and acetone for 3 times each, dry it, and slice it for later use;
[0039] S2, weigh 0.2 mmol of nickel nitrate, dissolve it in 20 ml of N,N-dimethylformamide, stir and disperse it evenly to form a solution, then take a piece of the above nickel foam and immerse it in the above solution to allow the nickel nitrate to be fully adsorbed on the nickel foam;
[0040] S3, weigh 1 mmol of 2,3,9,10,16,17,23,24-octaaminophthalocyanine zinc and add it to the above solution, stir and disperse it evenly;
[0041] S4. Transfer the above solution to a sealed container with a lid, heat to 120°C, and maintain for 48 hours to obtain Figure 1 The nickel foam shown is loaded with a conjugated polymer containing nickel-phthalocyanine units;
[0042] S5. The nickel foam loaded with the conjugated polymer containing nickel-phthalocyanine units was washed with anhydrous ethanol and deionized water for three times respectively, and dried in a vacuum drying oven at 60° C. for 12 h to obtain an integrated catalytic electrode. In the integrated catalytic electrode, the loading amount of the conjugated polymer on the nickel foam was 0.5 mg / cm 2 .
[0043] Example 3
[0044] An electrically assisted photocatalytic CO 2 The preparation method of the cycloaddition integrated catalytic electrode comprises the following steps:
[0045] S1. The carbon cloth was pickled with 3 mol / L dilute hydrochloric acid at 80°C for 0.5 h, then washed with deionized water and acetone for 3 times each, dried, and sliced for later use;
[0046] S2. Weigh 2 mmol of ferric nitrate, dissolve it in 120 ml of a mixed solvent of N,N-dimethylformamide / ethylene glycol (volume ratio is 1:1), stir and disperse it evenly to form a solution, then take a piece of the above carbon cloth and immerse it in the above solution to allow the ferric nitrate to be fully adsorbed on the carbon cloth;
[0047] S3, weigh 4 mmol of 1,2,4,5-tetracyanobenzene and add it to the above solution, stirring and dispersing it evenly;
[0048] S4. Transfer the above solution to a sealed container with a lid, heat to 180°C, and maintain for 72 hours to obtain Figure 1 The carbon cloth shown is loaded with a conjugated polymer containing iron-phthalocyanine units;
[0049] S5. The carbon cloth loaded with the conjugated polymer containing the iron-phthalocyanine unit was washed with anhydrous ethanol and deionized water for three times respectively, and dried in a vacuum drying oven at 60° C. for 12 h to obtain an integrated catalytic electrode. In the integrated catalytic electrode, the loading amount of the conjugated polymer on the carbon cloth was 1.0 mg / cm 2 .from Figure 2 It can be seen that Fe is dispersed in the form of single atoms in the conjugated polymer containing iron-phthalocyanine units.
[0050] Example 4
[0051] An electrically assisted photocatalytic CO 2The preparation method of the cycloaddition integrated catalytic electrode comprises the following steps:
[0052] S1. The carbonized wood was pickled with 1 mol / L dilute hydrochloric acid at 20°C for 6 h, then washed with deionized water and acetone for 3 times each, dried, and sliced for later use;
[0053] S2. Weigh 2 mmol of cobalt sulfate, dissolve it in 20 ml of a xylene / pentanol mixed solution (volume ratio of 1:10), stir and disperse it evenly to form a solution, then take a piece of the carbonized wood and immerse it in the solution to allow the cobalt sulfate to be fully adsorbed on the carbonized wood;
[0054] S3, weigh 6 mmol of 1,2,4,5-tetraethynylbenzene, add it to the above solution, and stir to disperse it evenly;
[0055] S4. The above solution was transferred to a sealed container with a lid, heated to 220°C, and maintained for 12 hours to obtain a load such as Figure 1 Carbonized wood of the conjugated polymer containing cobalt-phthalocyanine units as shown;
[0056] S5. The carbonized wood loaded with the conjugated polymer containing cobalt-phthalocyanine units was washed with anhydrous ethanol and deionized water for three times respectively, and dried in a vacuum drying oven at 60° C. for 12 h to obtain an integrated catalytic electrode. In the integrated catalytic electrode, the loading amount of the conjugated polymer on the carbonized wood was 2 mg / cm 2 .
[0057] Application Example 1:
[0058] The integrated catalytic electrode prepared in Example 1 was used as the cathode, the magnesium rod was used as the sacrificial anode, the ionic liquid was used as the solvent and electrolyte, and styrene oxide was used as the reaction substrate. 100 mg of tetrabutylammonium bromide was weighed and added to 100 ml of styrene oxide / ionic liquid solution with a molar concentration of 1 mol / L, and high-purity CO was introduced. 2 Gas, CO in photoreactor 2 The pressure was 1atm, a 300W xenon light source (equipped with an AM 1.5 filter) was used for irradiation, and a -3.0V voltage was applied to the cathode and anode. After reacting for 0.5 hours, centrifugation was performed and the liquid portion was detected by gas chromatography to obtain the yield of styrene carbonate.
[0059] Application Example 2:
[0060] The integrated catalytic electrode prepared in Example 2 was used as the cathode, the magnesium rod was used as the sacrificial anode, the ionic liquid was used as the solvent and electrolyte, and styrene oxide was used as the reaction substrate. 300 mg of tetrabutylammonium bromide was weighed and added to 100 ml of styrene oxide / ionic liquid solution with a molar concentration of 5 mol / L, and high-purity CO was introduced.2 The gas was irradiated with a 10W LED light source, and a voltage of -3.0V was applied to the cathode and anode. After reacting for 1 hour, centrifugal separation was performed, and the liquid portion was detected by gas chromatography to obtain the yield of styrene carbonate.
[0061] Application Example 3:
[0062] The integrated catalytic electrode prepared in Example 3 was used as the cathode, the magnesium rod was used as the sacrificial anode, the ionic liquid was used as the solvent and electrolyte, and styrene oxide was used as the reaction substrate. 30 mg of tetrabutylammonium bromide was weighed and added to 100 ml of styrene oxide / ionic liquid solution with a molar concentration of 0.1 mol / L, and high-purity CO was introduced. 2 Gas, CO in photoreactor 2 The pressure was 1atm, a 300W xenon light source (equipped with an AM 1.5 filter) was used for irradiation, and a -1.0V voltage was applied to the cathode and anode. After reacting for 2 hours, centrifugation was performed and the liquid portion was detected by gas chromatography to obtain the yield of styrene carbonate.
[0063] Application Example 4:
[0064] The integrated catalytic electrode prepared in Example 4 was used as the cathode, the magnesium rod was used as the sacrificial anode, the ionic liquid was used as the solvent and electrolyte, and styrene oxide was used as the reaction substrate. 100 mg of tetrabutylammonium bromide was weighed and added to 100 ml of styrene oxide / ionic liquid solution with a molar concentration of 2 mol / L, and high-purity CO was introduced. 2 Gas, CO in photoreactor 2 The pressure was 1atm, a 300W xenon light source (equipped with an AM 1.5 filter) was used for irradiation, and a voltage of -2.0V was applied to the cathode and anode. After reacting for 1 hour, centrifugation was performed and the liquid portion was detected by gas chromatography to obtain the yield of styrene carbonate.
[0065] Comparative Application Example 1:
[0066] The integrated catalytic electrode prepared in Example 1 was used as the cathode, the magnesium rod was used as the sacrificial anode, the ionic liquid was used as the solvent and electrolyte, and styrene oxide was used as the reaction substrate. 100 mg of tetrabutylammonium bromide was weighed and added to 100 ml of styrene oxide / ionic liquid solution with a molar concentration of 1 mol / L, and high-purity CO was introduced. 2 Gas, CO in photoreactor 2 The pressure was 1 atm, and a 300 W xenon light source (equipped with an AM 1.5 filter) was used for irradiation. After reacting for 0.5 hours, centrifugation was performed, and the liquid portion was detected by gas chromatography to obtain the yield of styrene carbonate.
[0067] Comparative Application Example 2:
[0068] The integrated catalytic electrode prepared in Example 1 was used as the cathode, the magnesium rod was used as the sacrificial anode, the ionic liquid was used as the solvent and electrolyte, and styrene oxide was used as the reaction substrate. 100 mg of tetrabutylammonium bromide was weighed and added to 100 ml of styrene oxide / ionic liquid solution with a molar concentration of 1 mol / L, and high-purity CO was introduced. 2 Gas, CO in photoreactor 2 The pressure was 1 atm, and a voltage of -2.0 V was applied to the cathode and the anode. After the reaction for 0.5 hours, centrifugation was performed and the liquid portion was detected by gas chromatography to obtain the yield of styrene carbonate.
[0069] The performance of the catalyst was evaluated by the yield and selectivity of styrene carbonate (SC). Yield (%): X = C SC / C 0 ×100, selectivity (%) = C SC / (C 0 -C SO )×100.
[0070] Among them, C 0 , C SO and C SC They represent the concentration of styrene oxide before and after the reaction and the concentration of styrene carbonate produced, respectively.
[0071] The yields and selectivities obtained from the above application examples 1-4 and comparative application examples 1-2 are shown in Table 1 below:
[0072] Table 1 Performance of the integrated catalytic electrode in catalytic CO2 cycloaddition to styrene carbonate under different reaction conditions
[0073] Yield (%) Selectivity (%) Application Example 1 86 98.1 Application Example 2 92 97.0 Application Example 3 96 98.6 Application Example 4 91 99.8 Comparative Application Example 1 72 64.2 Comparative Application Example 2 35 29.5
[0074] It can be seen from Table 1 that without electrical assistance and without light, the yield of styrene carbonate is only about 72% and 35%, respectively, and the selectivity is only 64.2% and 29.5%, respectively; under electrical-assisted photocatalysis, the integrated catalytic electrode obtained in Example 4 can obtain a yield of styrene carbonate of up to 98%, and a selectivity of up to 99.8%, which reflects the important role of electrical-assisted photocatalysis. The integrated catalytic electrode prepared by the present invention is suitable for electrical-assisted photocatalysis of CO 2 Cycloaddition to prepare cyclic carbonates.
Claims
1. A method for preparing an electrically assisted photocatalytic CO2 cycloaddition integrated catalytic electrode, characterized in that: The following steps are involved: S1, pickling the conductive self-supporting body with dilute hydrochloric acid, then washing with deionized water and acetone, drying, and slicing for later use; S2, weighing a certain amount of metal precursor and dissolving it in a solvent, stirring and dispersing it evenly to form a solution, and then taking a piece of the conductive self-supporting body treated in step S1 and immersing it in the solution, so that the metal precursor is fully adsorbed on the conductive self-supporting body; S3, weighing a certain amount of organic ligand and adding it to the mixed solution obtained in step S2, stirring and dispersing it evenly; S4, transferring the solution obtained in step S3 to a sealed container with a lid, heating to 80-220° C., and maintaining for 2-72 hours to obtain a conductive self-supporting body loaded with a conjugated polymer; S5. After washing the conductive self-supporting body loaded with the conjugated polymer obtained in step S4, the conductive self-supporting body is placed in a vacuum drying oven for drying to obtain an integrated catalytic electrode.
2. The method for preparing an electrically assisted photocatalytic CO2 cycloaddition integrated catalytic electrode according to claim 1, characterized in that: In step S1, the conductive self-supporting body is one of a conductive metal mesh, a conductive metal foam, a carbon paper, a carbon cloth, and a carbonized wood; the concentration of the dilute hydrochloric acid is 1 to 5 mol / L, the pickling temperature is 20 to 80° C., and the pickling time is 0.5 to 6 h; and the self-supporting body is washed three times with deionized water and acetone respectively.
3. The method for preparing an electrically assisted photocatalytic CO2 cycloaddition integrated catalytic electrode according to claim 1 or 2, characterized in that: In step S2, the metal precursor is one or two of iron nitrate, iron sulfate, iron hydrochloride, cobalt nitrate, cobalt sulfate, cobalt hydrochloride, nickel nitrate, nickel sulfate, nickel hydrochloride, copper nitrate, copper sulfate, copper hydrochloride, zinc nitrate, zinc sulfate, and zinc hydrochloride; the solvent is one or two of methanol, ethanol, ethylene glycol, pentanol, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, toluene, xylene, and mesitylene; the concentration of the metal precursor in the solution is 0.001 to 1 mol / L.
4. The method for preparing an electrically assisted photocatalytic CO2 cycloaddition integrated catalytic electrode according to claim 1 or 2, characterized in that: In step S3, the organic ligand is one of 1,2,4,5-tetracyanobenzene, 1,2,4,5-tetraethynylbenzene, tetrakis(4-carboxyphenyl)porphine, 5,10,15,20-tetrakis(4-carboxyphenyl)porphyrin, 2,3,9,10,16,17,23,24-octaaminometallicphthalocyanine compounds, and 2,3,9,10,16,17,23,24-octahydroxymetallicphthalocyanine compounds; and the molar ratio between the organic ligand and the metal precursor is (0.2-5):
1.
5. The method for preparing an electrically assisted photocatalytic CO2 cycloaddition integrated catalytic electrode according to claim 1 or 2, characterized in that: In step S4, the structure of the conjugated polymer contains a metal-phthalocyanine unit or a metal-porphyrin unit.
6. The method for preparing an electrically assisted photocatalytic CO2 cycloaddition integrated catalytic electrode according to claim 1 or 2, characterized in that: In step S5, the electrode is washed with anhydrous ethanol and deionized water for three times respectively; the drying temperature is 40-60°C and the drying time is 11-13 hours; in the integrated catalytic electrode, the loading amount of the conjugated polymer on the conductive self-supporting body is 0.1-5 mg / cm 2 .
7. An integrated catalytic electrode obtained by the method for preparing an electrically assisted photocatalytic CO2 cycloaddition integrated catalytic electrode according to any one of claims 1 to 6.
8. The use of the integrated catalytic electrode according to claim 7 in the preparation of cyclic carbonates by CO2 cycloaddition, wherein the specific application process is: The integrated catalytic electrode described in claim 7 is used as the cathode, the magnesium rod is used as the sacrificial anode, and the ionic liquid is used as the solvent and electrolyte. The reaction substrate epoxide and the co-catalyst are added to the photoreactor, CO2 is introduced, a certain voltage is applied to the cathode and the anode, and a simulated light source or sunlight is used for illumination to carry out the cycloaddition reaction.
9. The use according to claim 8, characterized in that: The electrically assisted photocatalytic cycloaddition reaction is carried out at room temperature, the CO2 pressure in the photoreactor is 1 atm, and the reaction time is 0.5 to 2 hours; the simulated light source uses an LED or a xenon lamp with a power of 10 to 300 W; the mass ratio of the co-catalyst to the epoxide is 1:(40 to 250); the concentration of the epoxide in the ionic liquid is 0.1 to 5 mol / L; direct current is applied to the cathode and the anode, and the voltage is -3.0 V to -1.0 V.
10. The use according to claim 8, characterized in that: The co-catalyst is tetrabutylammonium bromide; and the epoxy compound is styrene oxide.