Method for increasing pulling rod length of gallium-doped single crystal

By non-sustaining doping phosphorus elements during the gallium-doped single crystal drawing process, the problems of insufficient length and accumulation of impurity concentration of gallium-doped single crystal drawing rods are solved, and different resistivity products and production efficiency improvements are achieved to meet customer needs. .

CN119061466APending Publication Date: 2024-12-03INNER MONGOLIA ZHONGHUAN GCL PHOTOVOLTAIC MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310629473.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the insufficient length of the gallium-doped single crystal pull rod has led to an increase in the manufacturing cost of the enterprise and the accumulation of impurity concentration will affect product quality.

Method used

During the process of drawing gallium-doped single crystal, the attenuation of the axial resistivity of the single crystal is controlled by doping the phosphorus element, and a non-sustaining doping method is adopted to perform phosphorus according to the length of the single crystal, the weight of the residual material or the change in resistivity of the resistivity. The gas or solid doping of elements reduces the concentration of impurities and meets customers' needs for different resistivity.

Benefits of technology

It effectively increases the single crystal pulling length, reduces the impurity concentration, meets customers' demand for different resistivity, improves production efficiency, avoids the accumulation of impurities in phosphorus content, and improves product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004257943500000071
    Figure BDA0004257943500000071
  • Figure BDA0004257943500000081
    Figure BDA0004257943500000081
  • Figure BDA0004257943500000091
    Figure BDA0004257943500000091
Patent Text Reader

Abstract

The invention provides a method for increasing the pulling rod length of a gallium-doped single crystal, which comprises the following steps of: doping phosphorus element in the pulling process of the gallium-doped single crystal so as to control the attenuation of the axial resistivity of the single crystal; wherein the doping mode is as follows: when the single crystal is drawn to a first doping length, doping with a gas containing a phosphorus element or a solid containing the phosphorus element; or, when the weight of the residual material in the crucible reaches the first doping weight, doping the gas containing the phosphorus element or the solid containing the phosphorus element; or when the variation of the axial resistivity of the single crystal reaches the variation of the first doping resistivity, doping the gas containing the phosphorus element or the solid containing the phosphorus element. The method has the beneficial effects that the impurity concentration in the crystal is reduced, and meanwhile, products with different resistivity ratio ranges can be provided according to customer requirements; and the phosphorus-containing gas or solid is non-continuous in the doping process, so that the accumulation increase of the phosphorus content impurity concentration in the direction from the head to the tail of the silicon single crystal is avoided, and the length of the single crystal rod is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicon single crystal production, and in particular relates to a method for increasing the length of a gallium-doped single crystal drawn rod. Background Art

[0002] In the existing technology, gallium-doped single crystals have the advantage of low light attenuation compared to boron-doped single crystals, which has driven the market demand for gallium-doped single crystals. However, due to the extremely small segregation coefficient of Ga (Ga: 0.008, B: 0.8), the resistivity distribution is wider under the same rod length.

[0003] Since gallium has a small segregation coefficient in silicon, in order to meet customers' demand for the resistivity of gallium-doped single crystals, the industry is currently taking measures to reduce the length of gallium-doped single crystal rods and reduce the production of downgraded products. The entry length of gallium-doped products is 30% shorter than that of boron-doped products, which will lead to an increase in the manufacturing costs of enterprises.

[0004] The existing technology emphasizes continuous compensatory pulling, which will lead to the accumulation of high impurity concentration in the production of single crystal silicon. The accumulated concentration after multiple pulling has a negative impact on the quality of client products. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for increasing the length of a gallium-doped single crystal pulled rod to solve the above or other former problems existing in the prior art.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for increasing the length of a gallium-doped single crystal drawn rod, in which phosphorus is doped during the gallium-doped single crystal drawing process to control the attenuation of the axial resistivity of the single crystal; wherein the doping method is:

[0007] When the single crystal is pulled to a first doping length, doping is performed with a gas containing phosphorus or a solid containing phosphorus;

[0008] Or, when the weight of the remaining material in the crucible reaches the first doping weight, doping is performed with a gas containing phosphorus or a solid containing phosphorus;

[0009] Alternatively, when the variation of the axial resistivity of the single crystal reaches the variation of the first doping resistivity, doping is performed with a gas containing phosphorus or a solid containing phosphorus.

[0010] Furthermore, the first doping length is 0-50m.

[0011] Furthermore, when the single crystal is pulled to a second doping length, doping with the gas containing phosphorus or the solid containing phosphorus is stopped, and the second doping length is 0-50m.

[0012] Furthermore, the first doping weight is 0-100kg.

[0013] Furthermore, when the remaining material in the crucible reaches a second doping weight, doping with the gas containing the phosphorus element or the solid containing the phosphorus element is stopped, and the second doping weight is 0-100 kg.

[0014] Furthermore, the variation of the first doping resistivity is 0-20Ω·cm / m.

[0015] Further, when the change in the axial resistivity of the single crystal reaches the change in the second doping resistivity, doping with the phosphorus-containing gas or phosphorus-containing solid is stopped, and the change in the second doping resistivity is 0-20Ω·cm / m.

[0016] Furthermore, the flow rate of the gas containing phosphorus element is 0-500 L / min.

[0017] Furthermore, the weight of the solid containing phosphorus element is 0-100kg.

[0018] Furthermore, the phosphorus-containing gas is phosphine gas or a mixed gas of phosphine and argon, and the phosphorus-containing solid is a phosphorus alloy or phosphorus alone.

[0019] Due to the adoption of the above technical scheme, during the process of pulling the gallium-doped single crystal, the gas containing the phosphorus element or the solid containing the phosphorus element is doped, so that the prepared single crystal has gallium and phosphorus. The gas containing the phosphorus element or the solid containing the phosphorus element can be doped at any pulling length of the single crystal, or the gas containing the phosphorus element or the solid containing the phosphorus element can be doped when the weight of the residual material in the crucible is any weight, or the gas containing the phosphorus element or the solid containing the phosphorus element is doped at any axial resistivity change of the single crystal, so as to reduce the impurity concentration in the crystal, and at the same time, products with different resistivity ranges can be provided according to customer needs; the gas containing the phosphorus element or the solid containing the phosphorus element is not continuous during the doping process, so as to avoid the cumulative increase of the phosphorus impurity concentration of the silicon single crystal from the head to the tail direction, resulting in poor performance of the customer product; silicon products with different resistivity ranges can be pulled according to customer needs, so as to achieve phased doping in the production process of silicon single crystals, increase the length of the single crystal rod, and improve production efficiency. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with specific embodiments.

[0021] Some embodiments of the present invention relate to a method for increasing the length of a gallium-doped single crystal pulled rod. During the single crystal pulling process, phosphorus is doped at different single crystal length stages according to the attenuation mode of the gallium alloy corresponding to different single crystal lengths, or phosphorus is doped at different residual material weight stages according to the attenuation mode of the gallium alloy at different residual material weight stages, or phosphorus is doped in different resistivity ranges to increase the resistivity attenuation range and the single crystal pulling length.

[0022] A method for increasing the length of a gallium-doped single crystal drawn rod, wherein phosphorus is doped during the gallium-doped single crystal drawing process to control the attenuation of the axial resistivity of the single crystal; wherein the doping method is:

[0023] When the single crystal is pulled to a first doping length, a gas containing phosphorus or a solid containing phosphorus is doped. In the process of pulling the single crystal, as the length of the single crystal increases, the axial resistivity of the single crystal gradually decreases. According to the attenuation mode of the gallium alloy, in order to reduce the impurity concentration in the single crystal, when the pulled length of the single crystal reaches the first doping length, phosphorus-containing doping is performed to increase the resistivity attenuation range of the single crystal and increase the pulling length of the single crystal.

[0024] Among them, the first doping length is 0-50m, and the doping length can be 0.5m, 1m, 1.5m, 2m, 2.5m, 3m, 3.5m, 4m, 4.5m, 5m, 5.5m, 6m or any length value between 0-50m. It is selected according to actual needs and no specific requirements are made here.

[0025] The flow rate of the above-mentioned phosphorus-containing gas is 0-500L / min. The flow rate of the phosphorus-containing gas can be 500ml / min, 1000ml / min, 1500ml / min, 2000ml / min, 5000ml / min or any flow rate value between 0-500L / min. It is selected according to actual needs and no specific requirements are made here.

[0026] The weight of the above-mentioned solid containing phosphorus element is 0-100kg. The weight of the solid containing phosphorus element can be 10g, 50g, 100g, 150g, 200g, 250g, 300g or any weight value between 0-100kg. The selection is made according to actual needs and no specific requirements are made here.

[0027] After being doped with a gas or solid containing phosphorus, the change in the axial resistivity of the single crystal increases, thereby increasing the resistivity attenuation range of the single crystal and increasing the pulling length of the single crystal.

[0028] Doping with phosphorus-containing gas or doping with phosphorus-containing solid can continue until the single crystal pulling is completed, or, when the length of the single crystal reaches the second doping length, doping with phosphorus-containing gas or doping with phosphorus-containing solid is stopped, and the change in axial resistivity of the single crystal gradually decreases, so that the resistivity of the single crystal naturally decays to the target resistivity, thereby increasing the pulling length of the single crystal.

[0029] The above-mentioned second doping length is 0-50m, and the second doping length can be 0.5m, 1m, 1.5m, 3m, 5m or any length value between 0-50m. It is selected according to actual needs and no specific requirements are made here.

[0030] Alternatively, when the weight of the remaining material in the crucible reaches a first doping weight, doping is performed with a gas containing phosphorus or a solid containing phosphorus. During the process of pulling a single crystal, as the remaining material in the crucible gradually decreases and the length of the single crystal increases, the axial resistivity of the single crystal gradually decreases. According to the attenuation mode of the gallium alloy, in order to reduce the impurity concentration in the single crystal, when the weight of the remaining material in the crucible reaches the doping weight, doping with phosphorus is performed to increase the attenuation range of the single crystal resistivity and increase the pulling length of the single crystal.

[0031] Among them, the first doping weight is 0-100kg, and the doping weight can be 0.5kg, 3kg, 5kg or any weight value between 0-100kg. It is selected according to actual needs and no specific requirements are made here.

[0032] The flow rate of the above-mentioned phosphorus-containing gas is 0-500L / min. The flow rate of the phosphorus-containing gas can be 500ml / min, 1000ml / min, 1500ml / min, 2000ml / min, 5000ml / min or any flow rate value between 0-500L / min. It is selected according to actual needs and no specific requirements are made here.

[0033] The weight of the solid containing phosphorus element is 0-100kg. The weight of the solid containing phosphorus element can be 10g, 50g, 100g, 150g, 200g, 250g, 300g or any weight value between 0-100kg. The selection is made according to actual needs and no specific requirements are made here.

[0034] After being doped with a gas or solid containing phosphorus, the change in the axial resistivity of the single crystal increases, thereby increasing the resistivity attenuation range of the single crystal and increasing the pulling length of the single crystal.

[0035] Doping with phosphorus-containing gas or doping with phosphorus-containing solid can continue until the single crystal pulling is completed, or, when the weight of the remaining material in the crucible reaches the second doping weight, doping with phosphorus-containing gas or doping with phosphorus-containing solid is stopped, and the change in axial resistivity of the single crystal gradually decreases, so that the resistivity of the single crystal naturally decays to the target resistivity, thereby increasing the pulling length of the single crystal.

[0036] The above-mentioned second doping weight is 0-100kg. The second doping weight can be 0.5kg, 3kg, 5kg or any weight value of 0-100kg. It is selected according to actual needs and no specific requirements are made here.

[0037] Alternatively, when the change in the axial resistivity of the single crystal reaches the change in the first doping resistivity, a gas containing phosphorus or a solid containing phosphorus is doped. According to the attenuation mode of the gallium alloy, in order to reduce the impurity concentration in the single crystal, phosphorus-containing elements are doped in different resistivity ranges to increase the resistivity attenuation range of the single crystal and increase the pulling length of the single crystal.

[0038] Among them, the change in the above-mentioned first doping resistivity is 0-20Ω·cm / m, and the doping change can be 0.3Ω·cm / m, 0.5Ω·cm / m, 1Ω·cm / m, 1.5Ω·cm / m or any doping change value between 0-20Ω·cm / m. It is selected according to actual needs and no specific requirements are made here.

[0039] The flow rate of the gas containing phosphorus element is 0-500L / min. The flow rate of the gas containing phosphorus element can be 500ml / min, 1000ml / min, 1500ml / min, 2000ml / min, 5000ml / min or any flow rate value between 0-100L / min. It is selected according to actual needs and no specific requirements are made here.

[0040] The weight of the solid containing phosphorus element is 0-100kg. The weight of the solid containing phosphorus element can be 0.5kg, 3kg, 5kg, 10kg or any weight value between 0-100kg. The selection is made according to actual needs and no specific requirements are made here.

[0041] After doping with the gas containing the phosphorus element or the solid containing the phosphorus element, the change in the axial resistivity of the single crystal increases, and the doping with the gas containing the phosphorus element or the solid containing the phosphorus element can be continued until the single crystal pulling is completed, or, when the change in the axial resistivity of the single crystal is the change in the second doping resistivity, the doping with the gas containing the phosphorus element or the solid containing the phosphorus element is stopped, and the change in the axial resistivity of the single crystal gradually decreases, so that the resistivity of the single crystal naturally decays to the target resistivity, thereby increasing the pulling length of the single crystal.

[0042] The above-mentioned change in the second doping resistivity is 0-20Ω·cm / m. The change in the second doping resistivity can be 0.3Ω·cm / m, 0.5Ω·cm / m, 1Ω·cm / m, 1.5Ω·cm / m or any doping change value between 0-20Ω·cm / m. It is selected according to actual needs and no specific requirements are made here.

[0043] The phosphorus-containing gas is phosphine gas or a mixed gas of phosphine and argon, which is selected according to actual needs; the phosphorus-containing solid is a phosphorus alloy or phosphorus element, which is selected according to actual needs.

[0044] Embodiment 1

[0045] During the single crystal pulling process, when the length of the single crystal increases from 0 to 1 m, without doping with phosphorus-containing gas or phosphorus-containing solid, the axial resistivity change per unit length of the single crystal decreases from 1 Ω·cm / m to 0.9 Ω·cm / m;

[0046] When the length of the single crystal increases from 1 to 2 m, without doping with phosphorus-containing gas or phosphorus-containing solid, the change in axial resistivity per unit length of the single crystal decreases from 0.9 Ω·cm / m to 0.8 Ω·cm / m;

[0047] When the length of the single crystal increases from 2 to 3 m, without doping with phosphorus-containing gas or phosphorus-containing solid, the change in axial resistivity per unit length of the single crystal decreases from 0.8 Ω·cm / m to 0.7 Ω·cm / m;

[0048] When the length of the single crystal increases from 3m to 4m, doping with phosphorus-containing gas at a flow rate of 1000ml / min or doping with phosphorus-containing solid at a weight of 500g is performed, and the change in axial resistivity per unit length of the single crystal increases from 0.7Ω·cm / m to 0.8Ω·cm / m;

[0049] When the length of the single crystal increases from 4m to 5m, the doping of phosphorus-containing gas with a flow rate of 1000ml / min or the doping of phosphorus-containing solid with a weight of 500g is performed, and the change of the axial resistivity per unit length of the single crystal increases from 0.8Ω·cm / m to 1Ω·cm / m.

[0050] When the length of the single crystal increases from 5 to 6 m, without doping with phosphorus-containing gas or phosphorus-containing solid, the change in axial resistivity per unit length of the single crystal decreases from 1 Ω·cm / m to 0.9 Ω·cm / m;

[0051] When the length of the single crystal increases from 6 to 7 m, without doping with phosphorus-containing gas or phosphorus-containing solid, the change in axial resistivity per unit length of the single crystal decreases from 0.9 Ω·cm / m to 0.8 Ω·cm / m;

[0052] When the length of the single crystal increases from 7 to 8 m, without doping with phosphorus-containing gas or phosphorus-containing solid, the change in axial resistivity per unit length of the single crystal decreases from 0.8 Ω·cm / m to 0.7 Ω·cm / m;

[0053] The above data are sorted out as shown in the following table:

[0054]

[0055] From the above content, it can be known that when the axial resistivity change per unit length of the single crystal decays to 0.7Ω·cm / m, doping with phosphorus-containing gas or phosphorus-containing solid is carried out. When the axial resistivity change per unit length of the single crystal is 1Ω·cm / m, doping with phosphorus-containing gas or phosphorus-containing solid is stopped to increase the axial resistivity change per unit length of the single crystal, increase the resistivity attenuation range, and increase the single crystal pulling length.

[0056] Embodiment 2

[0057] During the single crystal pulling process, when the weight of the residual material in the crucible is 800 kg, no doping with phosphorus-containing gas or phosphorus-containing solid is performed, and the axial resistivity change per unit length of the single crystal is 1Ω·cm / m;

[0058] When the weight of the remaining material in the crucible is 700 kg, and no phosphorus-containing gas or phosphorus-containing solid doping is performed, the change in axial resistivity per unit length of the single crystal is 0.9 Ω·cm / m;

[0059] When the weight of the residual material in the crucible is 600 kg, no doping with gas or solid containing phosphorus is performed, and the change in axial resistivity per unit length of the single crystal is 0.8 Ω·cm / m;

[0060] When the weight of the residual material in the crucible is 500 kg, the phosphorus-containing gas is doped at a flow rate of 1000 ml / min, or the phosphorus-containing solid is doped at a weight of 500 g, and the axial resistivity change per unit length of the single crystal is 0.9 Ω·cm / m;

[0061] When the weight of the residual material in the crucible is 400 kg, doping with a gas containing phosphorus element is performed, and the flow rate of the gas containing phosphorus element is 1000 ml / min, or doping with a solid containing phosphorus element is performed, and the weight of the solid containing phosphorus element is 500 g, and the change of the axial resistivity per unit length of the single crystal is 1 Ω·cm / m;

[0062] When the weight of the remaining material in the crucible is 300 kg, no doping with phosphorus-containing gas or phosphorus-containing solid is performed, and the change in axial resistivity per unit length of the single crystal is 0.9 Ω·cm / m;

[0063] When the weight of the residual material in the crucible is 200 kg, no doping with gas or solid containing phosphorus is performed, and the change in axial resistivity per unit length of the single crystal is 0.8 Ω·cm / m;

[0064] When the weight of the remaining material in the crucible is 100 kg, no doping with gas or solid containing phosphorus is performed, and the change in axial resistivity per unit length of the single crystal is 0.7 Ω·cm / m;

[0065] When the weight of the remaining material in the crucible is 50 kg, no doping with the gas containing phosphorus or the solid containing phosphorus is performed, and the change in the axial resistivity per unit length of the single crystal is 0.6 Ω·cm / m.

[0066] The above data are sorted out as shown in the following table:

[0067]

[0068]

[0069] From the above content, it can be known that when the axial resistivity change per unit length of the single crystal decays to 0.8Ω·cm / m, doping with phosphorus-containing gas or phosphorus-containing solid is carried out. When the axial resistivity change per unit length of the single crystal reaches 1Ω·cm / m, doping with phosphorus-containing gas or phosphorus-containing solid is stopped to increase the axial resistivity change per unit length of the single crystal, increase the resistivity attenuation range, and increase the single crystal pulling length.

[0070] Embodiment 3

[0071] In the single crystal pulling process, when the unit axial resistivity change of the single crystal is 1Ω·cm / m, no doping of phosphorus gas or phosphorus-containing solid is performed, and the unit length axial resistivity change of the single crystal is 1Ω·cm / m;

[0072] When the unit axial resistivity change of the single crystal is 0.9Ω·cm / m, without doping with phosphorus gas or phosphorus-containing solid, the unit length axial resistivity change of the single crystal is 0.9Ω·cm / m;

[0073] When the unit axial resistivity change of the single crystal is 0.8Ω·cm / m, without doping with phosphorus gas or phosphorus-containing solid, the unit length axial resistivity change of the single crystal is 0.8Ω·cm / m;

[0074] When the unit axial resistivity change of the single crystal is 0.7Ω·cm / m, phosphorus gas is doped, and the flow rate of the phosphorus-containing gas is 1000ml / min, or phosphorus-containing solid is doped, and the weight of the phosphorus-containing solid is 500g, and the unit length axial resistivity change of the single crystal is 0.8Ω·cm / m;

[0075] When the unit axial resistivity change of the single crystal is 0.8Ω·cm / m, phosphorus gas is doped, and the flow rate of the phosphorus-containing gas is 1000ml / min, or phosphorus-containing solid is doped, and the weight of the phosphorus-containing solid is 500g, and the unit length axial resistivity change of the single crystal is 1Ω·cm / m;

[0076] The pulling of the single crystal is continued, and the doping of phosphorus gas or phosphorus-containing solid is stopped. The axial resistivity of the single crystal gradually decays, and the change of axial resistivity per unit length of the single crystal gradually decays to 0.9Ω·cm / m, 0.8Ω·cm / m, 0.7Ω·cm / m, and 0.6Ω·cm / m.

[0077] The above data are sorted out as shown in the following table:

[0078]

[0079] From the above content, it can be known that when the axial resistivity change per unit length of the single crystal decays to 0.8Ω·cm / m, doping with phosphorus-containing gas or phosphorus-containing solid is carried out. When the axial resistivity change per unit length of the single crystal reaches 1Ω·cm / m, doping with phosphorus-containing gas or phosphorus-containing solid is stopped to increase the axial resistivity change per unit length of the single crystal, increase the resistivity attenuation range, and increase the single crystal pulling length.

[0080] Due to the adoption of the above technical scheme, during the process of pulling the gallium-doped single crystal, the gas containing the phosphorus element or the solid containing the phosphorus element is doped, so that the prepared single crystal has gallium and phosphorus. The gas containing the phosphorus element or the solid containing the phosphorus element can be doped at any pulling length of the single crystal, or the gas containing the phosphorus element or the solid containing the phosphorus element can be doped when the weight of the residual material in the crucible is any weight, or the gas containing the phosphorus element or the solid containing the phosphorus element is doped at any axial resistivity change of the single crystal, so as to reduce the impurity concentration in the crystal, and at the same time, products with different resistivity ranges can be provided according to customer needs; the gas containing the phosphorus element or the solid containing the phosphorus element is not continuous during the doping process, so as to avoid the cumulative increase of the phosphorus impurity concentration of the silicon single crystal from the head to the tail direction, resulting in poor performance of the customer product; silicon products with different resistivity ranges can be pulled according to customer needs, so as to achieve phased doping in the production process of silicon single crystals, increase the length of the single crystal rod, and improve production efficiency.

[0081] The embodiments of the present invention are described in detail above, but the contents described are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for increasing the length of a gallium-doped single crystal drawn rod, characterized in that: During the gallium-doped single crystal pulling process, phosphorus is doped to control the attenuation of the axial resistivity of the single crystal; wherein the doping method is: When the single crystal is pulled to a first doping length, doping is performed with a gas containing phosphorus or a solid containing phosphorus; Or, when the weight of the remaining material in the crucible reaches the first doping weight, doping is performed with a gas containing phosphorus or a solid containing phosphorus; Alternatively, when the variation of the axial resistivity of the single crystal reaches the variation of the first doping resistivity, doping is performed with a gas containing phosphorus or a solid containing phosphorus.

2. The method for increasing the length of a gallium-doped single crystal drawn rod according to claim 1, characterized in that: The first doping length is 0-50m.

3. The method for increasing the length of a gallium-doped single crystal drawn rod according to claim 2, characterized in that: When the single crystal is pulled to a second doping length, doping with the gas containing phosphorus or the solid containing phosphorus is stopped, and the second doping length is 0-50m.

4. The method for increasing the length of a gallium-doped single crystal drawn rod according to any one of claims 1 to 3, characterized in that: The first doping weight is 0-100kg.

5. The method for increasing the length of a gallium-doped single crystal drawn rod according to claim 4, characterized in that: When the remaining material in the crucible reaches a second doping weight, doping with the gas containing phosphorus element or the solid containing phosphorus element is stopped, and the second doping weight is 0-100kg.

6. The method for increasing the length of a gallium-doped single crystal drawn rod according to any one of claims 1 to 3 and 5, characterized in that: The variation of the first doping resistivity is 0-20Ω·cm / m.

7. The method for increasing the length of a gallium-doped single crystal drawn rod according to claim 6, characterized in that: When the change in the axial resistivity of the single crystal reaches the change in the second doping resistivity, doping with the gas or solid containing phosphorus is stopped, and the change in the second doping resistivity is 0-20Ω·cm / m.

8. The method for increasing the length of a gallium-doped single crystal drawn rod according to any one of claims 1 to 3, characterized in that: The flow rate of the phosphorus-containing gas is 0-500 L / min.

9. The method for increasing the length of a gallium-doped single crystal drawn rod according to claim 8, characterized in that: The weight of the solid containing phosphorus element is 0-100kg.

10. The method for increasing the length of a gallium-doped single crystal drawn rod according to claim 1, characterized in that: The phosphorus-containing gas is phosphine gas or a mixed gas of phosphine and argon gas, and the phosphorus-containing solid is a phosphorus alloy or phosphorus element.

Citation Information

Patent Citations

  • Growth method of gallium-doped czochralski silicon, gallium-doped monocrystalline silicon and application

    CN112831828A

  • Silicon single crystal and preparation method thereof, silicon wafer, solar cell and assembly

    CN114622278A

  • Method for automatically controlling resistivity of monocrystalline silicon

    CN115341266A

  • Method for controlling axial attenuation rate of resistivity of single crystal

    CN115341271A

  • Method for controlling resistivity and n-type silicon single crystal

    US20170260645A1