Multicolor yarn and preparation method and application thereof
By adding foaming agent to the masterbatch and adjusting the wire extraction conditions, soft and high color fastness multi-color yarns are prepared, which solves the problems of poor color fastness and fabric performance of existing multi-color yarns at high temperatures. , achieving more efficient production and better physical performance.
Patent Information
- Application Number
- CN202411204767.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing multi-color yarns have poor color fastness at high temperatures, which are prone to color migration. Cloud dyeing and sublimation transfer methods affect the feel and bending resistance of the fabric.
Add foaming agent to the masterbatch, and control the color depth and softness of the yarn by adjusting the foaming ratio and wire drawing rate during wire drawing, and use melt extrusion and wire drawing technology to prepare multi-color yarns.
The obtained multi-color yarns are soft, have good feel and high color fastness, which solves the problems of color migration, bending resistance and poor adhesion, while improving production efficiency.
Smart Images

Figure CN119061516A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of textile technology, and in particular to a multi-color yarn and a preparation method and application thereof. Background Art
[0002] Existing multi-colored yarns are typically produced through cloud dyeing or digital sublimation transfer printing. Both dyeing methods suffer from high-temperature resistance, poor color fastness at high temperatures, and prone to color migration. Sublimation transfer printing, as disclosed in application number 201810535418.0, requires a sequential process of padding, sizing, drying, and printing. The applied sizing forms a thin film on the fabric surface, which not only affects the fabric's feel and flex resistance, but also impairs the coating's adhesion. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to provide a multi-color yarn which is not prone to color migration, and a preparation method and application thereof.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing multi-color yarn, comprising the following steps: melt-extruding a masterbatch containing a foaming agent and then drawing out the yarn, and intermittently changing the foaming ratio by adjusting the drawing temperature during drawing, and when the foaming ratio is x times, the drawing rate is x+1 times the drawing rate when no foaming occurs.
[0005] Another technical solution adopted by the present invention is: a multi-color yarn prepared by adopting the above-mentioned preparation method of the multi-color yarn.
[0006] Another technical solution adopted by the present invention is: application of the above-mentioned multi-color yarn in woven fabrics.
[0007] The beneficial effect of the present invention is that the preparation method of the present invention obtains yarns of different shades of color by adding a foaming agent to the masterbatch and synchronously regulating the foaming ratio and the spinning rate of the yarn during spinning. The yarn is soft, has a good hand feel and has high color fastness. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 The figure shows the multi-color yarn prepared in Example 1 of the present invention;
[0009] Figure 2 Shown is the multi-color yarn prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0010] To illustrate the technical content, achieved objectives and effects of the present invention in detail, the following description is given in conjunction with the embodiments and accompanying drawings.
[0011] A method for preparing multi-color yarn comprises the following steps: melt-extruding a masterbatch containing a foaming agent and then drawing a yarn; during the drawing process, the foaming ratio is intermittently changed by regulating the drawing temperature; when the foaming ratio is x times, the drawing rate is x+1 times the drawing rate when no foaming occurs.
[0012] As can be seen from the above description, the beneficial effects of the present invention are as follows: the present invention adds a foaming agent to the masterbatch, and the higher the foaming ratio, the lighter the yarn color and the thicker the yarn diameter; in order to obtain uniform yarn, the spinning rate is adjusted synchronously, and the faster the spinning rate, the thinner the yarn, and the further lighter the yarn color. The present invention obtains yarns of varying shades by regulating the foaming ratio and spinning rate of the yarn during spinning. The yarn is soft and has high color fastness, and is lightweight, solving the physical performance problems of cloud-dyed fabrics or sublimation transfer fabrics, such as color migration, bending resistance, and poor adhesion. At the same time, this method is easy to adjust, and production conditions can be quickly adjusted to obtain yarn of another color. Compared with the traditional method of replacing dye liquor to produce multi-color yarns, it is more efficient.
[0013] Furthermore, the raw materials of the masterbatch include PET (polyethylene terephthalate plastic) and a foaming agent, and also include a pigment or a dye.
[0014] Furthermore, the pigment or dye has a heat resistance temperature greater than 300°C.
[0015] Furthermore, the raw materials of the masterbatch include 76-80% PET and 0.5-1.5% foaming agent, and also include 18-22% pigment or dye, calculated by weight percentage.
[0016] Preferably, by weight percentage, the raw materials of the masterbatch include 76-80% PET and 1% foaming agent, and also include 20% pigment or dye.
[0017] From the above description, it can be seen that the foaming ratio is controlled by regulating the content of the foaming agent and the spinning rate. If the foaming ratio is too low, the color depth will not change significantly. If the foaming ratio is too high, the yarn may be too hollow and soft, and lack toughness.
[0018] Furthermore, the molecular weight of PET is 3,000 to 30,000 g / mol.
[0019] Preferably, the molecular weight of PET is 10,000 to 15,000 g / mol.
[0020] Furthermore, the raw materials of the masterbatch also include antioxidants, dispersants and coupling agents.
[0021] From the above description, it can be seen that the coupling agent is used to enhance the bonding effect between the pigment or dye and the resin carrier; the antioxidant is used to enhance the anti-yellowing performance of the PET resin.
[0022] Furthermore, the raw materials of the masterbatch include, by weight percentage, 0.1-1% antioxidant, 0.9-4% dispersant and 0.5-1% coupling agent.
[0023] Furthermore, the antioxidant is a phosphite antioxidant.
[0024] Furthermore, the rate of temperature change during spinning is 9-11°C / s.
[0025] From the above description, it can be seen that the rate of change when the spinning temperature changes is faster and the yarn color is more stable.
[0026] Furthermore, the temperature of the melt extrusion is lower than the foaming temperature.
[0027] Furthermore, the temperature of the melt extrusion is greater than or equal to 250°C.
[0028] From the above description, it can be seen that 250°C is the conventional melting and extrusion temperature of the spinning machine. A temperature lower than this may cause extrusion blockage.
[0029] Furthermore, the expansion ratio is 1 to 10 times.
[0030] From the above description, it can be seen that a foaming ratio exceeding 10 times may cause the yarn to be too hollow and soft and lack toughness.
[0031] Another technical solution adopted by the present invention is: a multi-color yarn prepared by adopting the above-mentioned preparation method of the multi-color yarn.
[0032] Another technical solution adopted by the present invention is: application of the above-mentioned multi-color yarn in woven fabrics.
[0033] As can be seen from the above description, the fabric woven with the multi-colored yarn of the present invention has a single-color effect with different brightness, and the softness of the fabric is improved and the weight is reduced.
[0034] Furthermore, the multi-color yarn is used in weaving gradient fabrics.
[0035] The raw materials in the following examples include:
[0036] Antioxidant: Jiaxing Zhongcheng's antioxidant ZG203, dispersant: Lubrizol DP310 (polyester modified polyphosphate dispersant), coupling agent: silane coupling agent kh560, dye: Ningbo Longxin SR122 transparent navy R (heat resistant temperature greater than 300°C), foaming agent: Sekisui Chemical EM406.
[0037] Embodiment 1 of the present invention is: a method for preparing multi-color yarn, comprising the following steps:
[0038] S1. Preparation of masterbatch: 76.5 kg of PET with a molecular weight of 10,000 g / mol, 20 kg of dye, 1 kg of foaming agent, 0.7 kg of antioxidant, 1 kg of dispersant and 0.8 kg of coupling agent were mixed and melted at 250° C. and granulated to obtain masterbatch.
[0039] S2. Wire drawing: The masterbatch is melt-extruded at 250°C and then wire drawing is performed. The wire drawing is divided into two states. The first state switches to the second state after walking 100 cm, and the second state switches to the first state after walking 200 cm. The temperature change rate when the two states switch is 10°C / s; the first state is a non-foaming state, the wire drawing temperature is 250°C, and the wire drawing rate is 10cm / s; the second state is a foaming state, the foaming ratio is 1 times, and the wire drawing rate is 20cm / s.
[0040] The effect of the multi-color yarn obtained in Example 1 is shown in FIG. Figure 1 shown.
[0041] Comparative Example 1 of the present invention is: a method for preparing ordinary yarn, the steps are as follows:
[0042] S1. Preparation of masterbatch: 77.5 kg of PET with a molecular weight of 10,000 g / mol, 20 kg of dye, 0.7 kg of antioxidant, 1 kg of dispersant and 0.8 kg of coupling agent were mixed and melted at 250° C. and granulated to obtain masterbatch.
[0043] S2. Thread drawing: The masterbatch was melt-extruded at 250°C and then thread drawing was performed. The thread drawing temperature was 250°C and the thread drawing rate was 10 cm / s.
[0044] The second embodiment of the present invention is a method for preparing multi-color yarn, comprising the following steps:
[0045] S1. Preparation of masterbatch: 80 kg of PET with a molecular weight of 3000 g / mol, 18 kg of dye, 0.5 kg of foaming agent, 0.1 kg of antioxidant, 0.9 kg of dispersant and 0.5 kg of coupling agent were mixed and melted at 250° C. and granulated to obtain masterbatch.
[0046] S2. Wire drawing: The masterbatch is melt-extruded at 250°C and then drawn. The wire drawing is divided into four states. Each time the line is 100 cm, it switches to the next state. The temperature change rate when the four states are switched is 9°C / s; the first state is the non-foaming state, the wire drawing temperature is 250°C, and the wire drawing rate is 5cm / s; the second state is the foaming state, the foaming ratio is 1 times, and the wire drawing rate is 10cm / s; the third state is the foaming state, the foaming ratio is 3 times, and the wire drawing rate is 20cm / s; the fourth state is the foaming state, the foaming ratio is 5 times, and the wire drawing rate is 30cm / s.
[0047] The effect of the multi-color yarn obtained in Example 2 is shown in FIG. Figure 2 shown.
[0048] The third embodiment of the present invention is a method for preparing multi-color yarn, comprising the following steps:
[0049] S1. Preparation of masterbatch: 76 kg of PET with a molecular weight of 30,000 g / mol, 21 kg of dye, 0.5 kg of foaming agent, 1 kg of antioxidant, 1 kg of dispersant and 0.5 kg of coupling agent were mixed, melted and granulated at 250° C. to obtain masterbatch.
[0050] S2. Wire drawing: The masterbatch is melt-extruded at 250°C and then drawn. The wire drawing is divided into two states. The first state switches to the second state after walking 100 cm, and the second state switches to the first state after walking 200 cm. The temperature change rate when switching between the two states is 11°C / s; the first state is a non-foaming state, the wire drawing temperature is 250°C, and the wire drawing rate is 10cm / s; the second state is a foaming state, the foaming ratio is 2 times, and the wire drawing rate is 20cm / s.
[0051] The fourth embodiment of the present invention is: a multi-color yarn, which is obtained by the preparation method of the first embodiment, and its effect is shown in FIG. Figure 1 shown.
[0052] The fifth embodiment of the present invention is: a gradient fabric woven with the multi-color yarn of the fourth embodiment.
[0053] The yarns of Example 1 and Comparative Example 1 are respectively used to weave A4-sized fabrics 1 and 1', and the weight of fabric 1 is 8.12 g / m 2 The warp density is 50 threads / inch and the weft density is 40 threads / inch; the weight of fabric 1' is 9.97g / m 2 The warp density was 50 threads / inch and the weft density was 40 threads / inch. The softness of fabrics 1 and 1' was tested using the following method: the fabrics were placed face-down on a flat surface and the warping angle was measured. The lower the warping angle, the better the softness. The test results are shown in Table 1. The color fastness of fabrics 1 and 1' was tested using the ISO105-P01 standard (180s at 190°C). The test results are shown in Table 1.
[0054] Table 1
[0055] Softness Color fastness Fabric 1 10° Level 4-5 Fabric 1' 30° Level 4-5
[0056] In summary, the multi-color yarn provided by the present invention and its preparation method and application have the following advantages:
[0057] 1. By regulating the yarn foaming ratio and spinning speed during spinning, yarns with different shades of color can be obtained. The yarns are soft and have high color fastness.
[0058] 2. The foaming ratio is controlled by adjusting the content of the foaming agent and the spinning rate. The foaming ratio does not exceed 10 times to maintain a certain toughness.
[0059] 3. The rate of change of spinning temperature is faster and the yarn color is more stable.
[0060] 4. The multi-color yarn of the present invention can be directly woven into a gradient fabric.
[0061] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's description and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing multicolor yarn, characterized in that: The following steps are involved: The masterbatch containing the foaming agent is melt-extruded and then drawn. During the drawing, the foaming ratio is intermittently changed by adjusting the drawing temperature. When the foaming ratio is x times, the drawing rate is x+1 times the drawing rate when there is no foaming.
2. The method for preparing multicolor yarn according to claim 1, characterized in that: The raw materials of the masterbatch include PET and a foaming agent, and also include a pigment or a dye.
3. The method for preparing multicolor yarn according to claim 2, characterized in that: Calculated by weight percentage, the raw materials of the masterbatch include 76-80% PET and 0.5-1.5% foaming agent, and also include 18-22% pigment or dye.
4. The method for preparing multicolor yarn according to claim 2, characterized in that: The raw materials of the masterbatch also include antioxidant, dispersant and coupling agent.
5. The method for preparing multicolor yarn according to claim 4, characterized in that: Calculated by weight percentage, the raw materials of the masterbatch include 0.1-1% antioxidant, 0.9-4% dispersant and 0.5-1% coupling agent.
6. The method for preparing multicolor yarn according to claim 1, characterized in that: The speed of changing the spinning temperature is 9-11°C / s.
7. The method for preparing multicolor yarn according to claim 1, characterized in that: The temperature of the melt extrusion is lower than the foaming temperature.
8. The method for preparing multicolor yarn according to claim 1, characterized in that: The foaming ratio is 1 to 10 times.
9. A multicolor yarn prepared by the method for preparing a multicolor yarn according to any one of claims 1 to 8.
10. Use of the multi-color yarn as claimed in claim 9 in woven fabrics.
Citation Information
Patent Citations
Microporous foaming polypropylene fiber and preparation method thereof
CN102174717A
Multicolor anti-static foaming polypropylene bead particle and preparation method thereof
CN109401055A
Multicolor wood-plastic profile, manufacturing method thereof and wood-plastic plate
CN115516026A
Processing method of color-changing silk
CN116676676A
Multicolor wood-plastic profile, manufacturing method thereof and wood-plastic plate
CN117264308A