Anti-ultraviolet fabric and production process thereof
By modifying PA6 polysiloxane and combining nanotitanium dioxide and nanocarbon dots, the problem of degradation of UV-proof fabrics after washing is solved, and efficient UV-proof performance and water-proof performance are achieved.
Patent Information
- Application Number
- CN202411184929.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing UV-proof fabrics have significantly reduced their UV-proof performance after washing, and have poor water-resistant performance, especially their combination with artificial fiber fabrics.
PA6 is functionally modified by polysiloxane-modified nanocomposites, and UV-proof yarns are prepared through melting, spinning, drafting and winding processes, and fabrics are woven through air jet looms, using nanotitanium dioxide and nanocarbon dots. The composition improves the UV resistance and wash resistance of the fabric.
It significantly improves the water-washing and UV-proof properties of UV-proof fabrics, ensuring that the fabric still has good UV-proof properties after multiple washes.
Smart Images

Figure BDA0005013246620000021 
Figure BDA0005013246620000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-ultraviolet fabrics, and in particular relates to an anti-ultraviolet fabric and a production process thereof. Background Art
[0002] Anti-UV fabric is a fabric produced by selecting the best fabric materials and using special processing technology. Anti-UV fabric generally has high light-shielding properties and can effectively block most ultraviolet rays and reduce the damage to the skin caused by direct sunlight.
[0003] It is generally believed that the tightness and thickness of the fabric will affect its UV protection ability. The tighter and thicker the fabric, the better its UV protection ability. With the popularization of sun protection clothing products and the demand for lightweight sun protection clothing, it is necessary to perform UV protection finishing on fabrics with lower gram weight. Commonly used UV protection agents include organic UV absorbers such as benzophenone compounds and benzotriazole compounds, as well as inorganic UV shielding agents such as zinc oxide and titanium dioxide. At present, the methods for UV protection finishing of fabrics mainly include padding, sol-gel method and chemical grafting method, etc., to evenly disperse the UV protection agent on the surface of the fabric.
[0004] Since chemical man-made fibers are lighter, they are more widely used in sun protection clothing than cotton knitted fabrics. However, this also leads to weak bonding between UV protective agents and man-made fiber fabrics. The finished UV-resistant fabrics have poor washing resistance, and their UV-resistant performance is severely reduced after multiple washings. Summary of the invention
[0005] The purpose of the present invention is to provide an anti-ultraviolet fabric and a production process thereof, and to functionally modify PA6 by preparing a polysiloxane-modified nanocomposite with anti-ultraviolet capability, so as to solve the problem of poor water washability of the anti-ultraviolet fabric.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A production process of UV-proof fabrics, comprising the following steps:
[0008] Functionally modified PA6, PA6 and PET are mixed in a mass ratio of 2-3:6-7:1, and anti-UV yarn is prepared through melting, spinning, drawing and winding processes. The anti-UV yarn is woven into fabric through a weft knitting process using a jet loom to obtain the anti-UV fabric, thus completing the production process of the anti-UV fabric.
[0009] Further, the functional modified PA6 is prepared by the following steps:
[0010] Step 1: Add carbon dot composite nano-titanium dioxide, deionized water, tetrahydrofuran and anhydrous potassium carbonate into a reactor, stir for 15-20 minutes at 20-25°C and 500-800r / min, and under nitrogen protection, drop 3-aminopropyltrimethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane into the reactor. After the dropwise addition, stir and react for 100-110 hours at 40°C, let stand to separate the layers, separate the emulsion layer and vacuum dry, dissolve the dried solid with dichloromethane, extract with deionized water and collect the organic phase, dry the organic phase with anhydrous magnesium sulfate, filter, and vacuum dry the filter cake to obtain a polysiloxane-modified nanocomposite.
[0011] The reaction process is as follows:
[0012]
[0013] Furthermore, the usage ratio of carbon dot composite nano-titanium dioxide, deionized water, tetrahydrofuran, anhydrous potassium carbonate, 3-aminopropyltrimethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane is 3.45:4.8:16:0.04:7.17:6.59.
[0014] Step 2: Add PA6 and hexafluoroisopropanol into a reactor, stir for 60-80 minutes at 55±5°C and 200-300r / min to completely dissolve PA6, then add EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride), 4-dimethylaminopyridine and polysiloxane-modified nanocomposite as an activator into the reactor, keep warm and stir under nitrogen protection for 20-24 hours, precipitate the reaction product with anhydrous ethanol, filter, wash the filter cake with anhydrous ethanol 2-3 times, and vacuum dry to obtain functionally modified PA6.
[0015] Further, the dosage ratio of PA6, hexafluoroisopropanol, EDC, 4-dimethylaminopyridine, polysiloxane-modified nanocomposite and dimethyl sulfoxide is 2 g: 30-40 mL: 0.038 g: 0.024 g: 0.08 g.
[0016] Furthermore, the carbon dot composite nano-titanium dioxide is prepared by the following steps:
[0017] Step 1: Add citric acid, ethylenediamine, boric acid and deionized water into a reactor in a mass ratio of 1:1.1:4.1:180-200, stir and mix, keep warm at 170-180°C for 8-10 hours, cool naturally, filter through a 0.22 μm water system microporous filter membrane, centrifuge the filtrate at 10000 r / min for 10 minutes, separate the precipitate and dry it to obtain nanocarbon dots.
[0018] Step 2: Prepare the nano-carbon dots into a carbon dot dispersion with a concentration of 1 mg / mL using anhydrous ethanol, add nano-titanium dioxide, deionized water and anhydrous ethanol into a reactor, stir at 300-500 r / min for 3-5 min, then add the carbon dot dispersion into the reactor, ultrasonically disperse for 5-10 min, stir the reaction at 140-145°C for 4-5 h, cool naturally, vacuum dry the reaction product, grind and crush to obtain carbon dot composite nano-titanium dioxide.
[0019] Furthermore, the dosage ratio of titanium dioxide, deionized water, anhydrous ethanol and carbon dot dispersion is 0.4-0.45 g: 20 mL: 6 mL: 8-9 mL.
[0020] Beneficial effects of the present invention:
[0021] The anti-ultraviolet fabric of the present invention has good anti-ultraviolet performance. Compared with the method of post-processing and finishing the artificial fiber fabric, the polysiloxane-modified nanocomposite with anti-ultraviolet ability is used to functionally modify PA6, and the anti-ultraviolet fabric is blended to produce the anti-ultraviolet fabric, thereby improving the water washing resistance of the anti-ultraviolet fabric and ensuring the anti-ultraviolet performance of the fabric after washing.
[0022] The polysiloxane modified nanocomposite of the present invention uses nano titanium dioxide as a matrix, and nano carbon dots are loaded on its surface. The nano carbon dots are hydrothermally prepared using citric acid, ethylenediamine and boric acid as raw materials, have a large number of oxygen-containing functional groups, have good ultraviolet absorption performance, and are combined with nano titanium dioxide to increase its light absorption range and significantly improve its ultraviolet protection performance. 3-Aminopropyltrimethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane are hydrolyzed to form silanol groups. During polymerization, some of the silanol groups can also react with the hydroxyl groups on the carbon-dot composite nano-titanium dioxide, so that the polysiloxane containing aminopropyl and trifluoropropyl groups is coated on the surface of the carbon-dot composite nano-titanium dioxide, and a polysiloxane-modified nano-composite is prepared and uniformly mixed with PA6 by solvent dispersion. The polysiloxane-modified nano-composite has good dispersibility in the solvent, and the amino group contained can react and graft with the terminal hydroxyl group in PA6 to increase its dispersibility and stability in PA6, which helps to improve the breaking strength of the yarn, while the trifluoropropyl group helps to improve the waterproof and oil-proof properties of the fabric, and further improves the water-washing resistance of the UV-proof fabric. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Embodiment 1: This embodiment provides an anti-ultraviolet fabric, which is produced by the following production process:
[0025] S1: Add citric acid, ethylenediamine, boric acid and deionized water into a reactor in a mass ratio of 1:1.1:4.1:180, stir and mix, keep warm at 170°C for 8 hours, cool naturally, pass through a 0.22 μm water-based microporous filter membrane, centrifuge the filtrate at 10,000 r / min for 10 minutes, separate the precipitate and dry it, and prepare nano-carbon dots with good ultraviolet absorption ability.
[0026] S2: Prepare the nano-carbon dots into a carbon dot dispersion with a concentration of 1 mg / mL using anhydrous ethanol, add 4 kg of nano-titanium dioxide, 200 L of deionized water and 60 L of anhydrous ethanol into a reactor, stir at 300 r / min for 3 min, then add 80 L of the carbon dot dispersion into the reactor, ultrasonically disperse for 5 min, stir and react at 140 ° C for 4 h to load the nano-carbon dots on the surface of the nano-titanium dioxide, cool naturally, vacuum dry the reaction product, grind and crush to obtain carbon dot composite nano-titanium dioxide.
[0027] S3: Add 3.45kg of carbon dot composite nano-titanium dioxide, 4.8kg of deionized water, 16kg of tetrahydrofuran and 0.04kg of anhydrous potassium carbonate to the reactor, stir at 20°C and 500r / min for 15min, and add 7.17kg of 3-aminopropyltrimethoxysilane and 6.59kg (3,3,3-trifluoropropyl) trimethoxysilane were added dropwise and stirred for reaction at 40°C for 100h. 3-aminopropyltrimethoxysilane and (3,3,3-trifluoropropyl) trimethoxysilane were hydrolyzed to form silanol groups. During polymerization, some silanol groups could also react with hydroxyl groups on the carbon dot composite nano-titanium dioxide, so that the polysiloxane containing aminopropyl and trifluoropropyl groups was coated on the surface of the carbon dot composite nano-titanium dioxide. The emulsion layer was separated and vacuum dried. The dried solid was dissolved with dichloromethane, and the organic phase was collected after extraction with deionized water. The organic phase was dried with anhydrous magnesium sulfate, filtered, and the filter cake was vacuum dried to obtain a polysiloxane-modified nano-composite.
[0028] S4: 20 kg of PA6 and 300 L of hexafluoroisopropanol were added to a reactor, and stirred at 50 ° C and 200 r / min for 60 minutes to completely dissolve the PA6. Then, 0.38 kg of EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) as an activator, 0.24 kg of 4-dimethylaminopyridine and 0.8 kg of polysiloxane-modified nanocomposite were added to the reactor. The reaction was stirred and kept warm for 20 hours under nitrogen protection. The polysiloxane-modified nanocomposite has good dispersibility in the solvent, and the amino group in the polysiloxane on its surface can react and graft with the terminal hydroxyl group in PA6 to increase its dispersibility and stability in PA6. The reaction product was precipitated with anhydrous ethanol, filtered, and the filter cake was washed twice with anhydrous ethanol and vacuum dried to obtain functionally modified PA6.
[0029] S5: Functionally modified PA6, PA6 and PET are mixed in a mass ratio of 2:6:1, and anti-UV yarn is prepared through melting, spinning, drawing and winding processes. The anti-UV yarn is woven by a jet loom through a weft knitting process to obtain an anti-UV fabric.
[0030] Embodiment 2: This embodiment provides an anti-ultraviolet fabric, which is produced by the following production process:
[0031] S1: Add citric acid, ethylenediamine, boric acid and deionized water into a reactor in a mass ratio of 1:1.1:4.1:190, stir and mix, keep warm at 175°C for 9 hours, cool naturally, pass through a 0.22 μm water-based microporous filter membrane, centrifuge the filtrate at 10,000 r / min for 10 minutes, separate the precipitate and dry it, and prepare nano-carbon dots with good ultraviolet absorption ability.
[0032] S2: Prepare the nano-carbon dots into a carbon dot dispersion with a concentration of 1 mg / mL using anhydrous ethanol, add 4.25 kg of nano-titanium dioxide, 200 L of deionized water and 60 L of anhydrous ethanol into a reactor, stir at 400 r / min for 4 min, then add 85 L of the carbon dot dispersion into the reactor, ultrasonically disperse for 8 min, stir the reaction at 142 ° C for 4.5 h to load the nano-carbon dots on the surface of the nano-titanium dioxide, cool naturally, vacuum dry the reaction product, grind and crush to obtain carbon dot composite nano-titanium dioxide.
[0033] S3: Add 3.45kg of carbon dot composite nano-titanium dioxide, 4.8kg of deionized water, 16kg of tetrahydrofuran and 0.04kg of anhydrous potassium carbonate to the reactor, stir at 22°C and 650r / min for 18min, and add 7.17kg of 3-aminopropyltrimethoxysilane and 6.59kg (3,3,3-trifluoropropyl) trimethoxysilane were added dropwise and stirred for reaction at 40°C for 105h. 3-aminopropyltrimethoxysilane and (3,3,3-trifluoropropyl) trimethoxysilane were hydrolyzed to form silanol groups. During polymerization, some silanol groups could also react with hydroxyl groups on the carbon dot composite nano-titanium dioxide, so that the polysiloxane containing aminopropyl and trifluoropropyl groups was coated on the surface of the carbon dot composite nano-titanium dioxide. The emulsion layer was separated and vacuum dried. The dried solid was dissolved with dichloromethane, and the organic phase was collected after extraction with deionized water. The organic phase was dried with anhydrous magnesium sulfate, filtered, and the filter cake was vacuum dried to obtain a polysiloxane-modified nano-composite.
[0034] S4: 20kg PA6 and 350L hexafluoroisopropanol were added to the reactor, and stirred at 55°C and 250r / min for 70min to completely dissolve the PA6. Then, 0.38kg EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) as an activator, 0.24kg 4-dimethylaminopyridine and 0.8kg polysiloxane-modified nanocomposite were added to the reactor. The reaction was stirred and kept warm for 22h under nitrogen protection. The polysiloxane-modified nanocomposite had good dispersibility in the solvent, and the amino groups in the polysiloxane on its surface could react and graft with the terminal hydroxyl groups in PA6 to increase its dispersibility and stability in PA6. The reaction product was precipitated with anhydrous ethanol, filtered, and the filter cake was washed twice with anhydrous ethanol and vacuum dried to obtain functionally modified PA6.
[0035] S5: Functionally modified PA6, PA6 and PET are mixed in a mass ratio of 2.5:6.5:1, and anti-UV yarn is prepared through melting, spinning, drawing and winding processes. The anti-UV yarn is woven by a jet loom through a weft knitting process to obtain an anti-UV fabric.
[0036] Embodiment 3: This embodiment provides an anti-ultraviolet fabric, which is produced by the following production process:
[0037] S1: Add citric acid, ethylenediamine, boric acid and deionized water into a reactor in a mass ratio of 1:1.1:4.1:200, stir and mix, keep warm at 180°C for 10 hours, cool naturally, filter through a 0.22 μm water-based microporous filter membrane, centrifuge the filtrate at 10,000 r / min for 10 minutes, separate the precipitate and dry it, and prepare nano-carbon dots with good ultraviolet absorption ability.
[0038] S2: Prepare the nano-carbon dots into a carbon dot dispersion with a concentration of 1 mg / mL using anhydrous ethanol, add 4.5 kg of nano-titanium dioxide, 200 L of deionized water and 60 L of anhydrous ethanol into a reactor, stir at 500 r / min for 5 min, then add 90 L of the carbon dot dispersion into the reactor, ultrasonically disperse for 10 min, stir and react at 145 ° C for 5 h to load the nano-carbon dots on the surface of the nano-titanium dioxide, cool naturally, vacuum dry the reaction product, grind and crush to obtain carbon dot composite nano-titanium dioxide.
[0039] S3: Add 3.45kg of carbon dot composite nano-titanium dioxide, 4.8kg of deionized water, 16kg of tetrahydrofuran and 0.04kg of anhydrous potassium carbonate to the reactor, stir at 25°C and 800r / min for 20min, and add 7.17kg of 3-aminopropyltrimethoxysilane and 6.59kg (3,3,3-trifluoropropyl) trimethoxysilane were added dropwise and stirred for reaction at 40°C for 110h. 3-aminopropyltrimethoxysilane and (3,3,3-trifluoropropyl) trimethoxysilane were hydrolyzed to form silanol groups. During polymerization, some silanol groups could also react with hydroxyl groups on the carbon dot composite nano-titanium dioxide, so that the polysiloxane containing aminopropyl and trifluoropropyl groups was coated on the surface of the carbon dot composite nano-titanium dioxide. The emulsion layer was separated and vacuum dried. The dried solid was dissolved with dichloromethane, and the organic phase was collected after extraction with deionized water. The organic phase was dried with anhydrous magnesium sulfate, filtered, and the filter cake was vacuum dried to obtain a polysiloxane-modified nano-composite.
[0040] S4: 20kg PA6 and 400L hexafluoroisopropanol were added to the reactor, and stirred at 60°C and 300r / min for 80min to completely dissolve the PA6. Then, 0.38kg EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) as an activator, 0.24kg 4-dimethylaminopyridine and 0.8kg polysiloxane-modified nanocomposite were added to the reactor, and the mixture was stirred and reacted for 24h under nitrogen protection. The polysiloxane-modified nanocomposite had good dispersibility in the solvent, and the amino groups in the polysiloxane on its surface could react and graft with the terminal hydroxyl groups in PA6 to increase its dispersibility and stability in PA6. The reaction product was precipitated with anhydrous ethanol, filtered, and the filter cake was washed with anhydrous ethanol for 3 times and vacuum dried to obtain functionally modified PA6.
[0041] S5: Functionally modified PA6, PA6 and PET are mixed in a mass ratio of 3:7:1, and anti-UV yarn is prepared through melting, spinning, drawing and winding processes. The anti-UV yarn is woven by a jet loom through a weft knitting process to obtain an anti-UV fabric.
[0042] Comparative Example 1: Based on Example 3, in step S3, the carbon dot composite nano-titanium dioxide is replaced by nano-titanium dioxide, and the other steps remain unchanged to prepare an anti-ultraviolet fabric.
[0043] Comparative Example 2: Based on Example 3, in step S3, (3,3,3-trifluoropropyl)trimethoxysilane is replaced with 3-aminopropyltrimethoxysilane of the same molar mass, and the other steps remain unchanged to prepare an anti-ultraviolet fabric.
[0044] Comparative Example 3: Based on Example 3, in step S3, 3-aminopropyltrimethoxysilane is replaced with (3,3,3-trifluoropropyl)trimethoxysilane of the same molar mass, and the other steps remain unchanged to prepare an anti-ultraviolet fabric.
[0045] Comparative Example 4: On the basis of Example 3, the carbon dot composite nano-titanium dioxide in step S2 is prepared into a 50 g / L slurry with deionized water, PA6 and PET are mixed in a mass ratio of 10:1, and the fabric is prepared by the method of step S5. The fabric is dipped and rolled in the slurry to prepare an anti-ultraviolet fabric with a carbon dot composite nano-titanium dioxide loading of 0.05wt%.
[0046] When preparing the anti-ultraviolet yarn in the examples and comparative examples, a single screw extruder is used, the screw diameter is 150mm, the aspect ratio is 30, the melting temperature of the raw material is 300°C, the melt is metered by a metering pump and extruded through the spinneret of the spinning equipment, the spinning speed is 600mm / min, after spraying spinning oil, it is stretched according to a draft ratio of 5.5, and after high temperature relaxation and heat setting at 245°C, it is wound into shape. The obtained anti-ultraviolet yarn contains 96 monofilaments per strand. The ZAX9100 air jet loom is used in the weaving process, and its process parameters are: speed 600r / min, opening time 300°, upper machine tension 3200N, and the woven anti-ultraviolet fabric weight ≈85g / m 2 .
[0047] In the examples and comparative examples, nano titanium dioxide was purchased from Nanjing Tianxing New Materials Co., Ltd. and had a diameter of 5-10 nm; PA6 was J2400F spinning-grade nylon chip resin from Hangzhou Polyshun; and PET was 608S spinning-grade polyester pure resin from Shanghai Yuanfang.
[0048] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 4. The breaking strength of different anti-ultraviolet yarns was measured using an electronic tensile testing machine. The anti-ultraviolet performance of different anti-ultraviolet fabrics was evaluated according to GB / T 18830-2009, and the UPF values, UVA transmittance, and UVB transmittance of different anti-ultraviolet fabrics were recorded. The fabrics were washed according to the 5A procedure of GB / T 8629-2001 "Household Washing and Drying Procedures for Textile Testing", and tumble dried at a drying temperature of 55°C. After cooling for 5 minutes, the anti-ultraviolet performance of the anti-ultraviolet fabrics washed 50 times was measured. The results are shown in Table 1:
[0049] Table 1
[0050]
[0051] As can be seen from Table 1, the anti-ultraviolet fabrics in Examples 1 to 3 have higher UPF values, lower UVA transmittance and UVB transmittance. Compared with the direct padding loading of anti-ultraviolet substances in Comparative Example 4, the anti-ultraviolet fabrics in the examples still have good anti-ultraviolet performance after 50 washings. Comparative Example 1 shows that the anti-ultraviolet performance of the fabric can be significantly improved after loading nano-carbon dots with nano-titanium dioxide; the anti-ultraviolet performance in Comparative Example 2 decreases after washing because the lack of trifluoropropyl in polysiloxane reduces the washing resistance of the anti-ultraviolet fabric; the decrease in the breaking strength of the yarn in Comparative Example 3 is due to the lack of aminopropyl in polysiloxane, which reduces the chemical grafting of the anti-ultraviolet nanofiller with PA6 and reduces the dispersibility and compatibility.
[0052] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0053] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process for anti-ultraviolet fabric, characterized in that: The steps include: Functionally modified PA6, PA6 and PET are mixed in a mass ratio of 2-3:6-7:1, and anti-ultraviolet yarn is prepared through melting, spinning, drawing and winding processes, and the anti-ultraviolet yarn is woven into anti-ultraviolet fabric through weft knitting process using an air jet loom; The modified PA6 is prepared by the following steps: Add PA6 and hexafluoroisopropanol into a reactor, stir at 55±5°C and 200-300r / min for 60-80min, add EDC, 4-dimethylaminopyridine and polysiloxane modified nanocomposite into the reactor, keep warm and stir under nitrogen protection for 20-24h, precipitate the reaction product with anhydrous ethanol, filter, wash the filter cake with anhydrous ethanol 2-3 times, and vacuum dry to obtain functional modified PA6.
2. The production process of a UV-proof fabric according to claim 1, characterized in that: The dosage ratio of PA6, hexafluoroisopropanol, EDC, 4-dimethylaminopyridine, polysiloxane-modified nanocomposite and dimethyl sulfoxide is 2g:30-40mL:0.038g:0.024g:0.08g.
3. The production process of a UV-proof fabric according to claim 1, characterized in that: The polysiloxane-modified nanocomposite is prepared by the following steps: Add carbon dot composite nano titanium dioxide, deionized water, tetrahydrofuran and anhydrous potassium carbonate into a reaction kettle, stir at 20-25° C. and 500-800 r / min for 15-20 min, add 3-aminopropyltrimethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane dropwise into the reaction kettle under nitrogen protection, stir and react at 40° C. for 100-110 h after the addition is complete, stand and separate, separate the emulsion layer and vacuum dry, dissolve the dried solid with dichloromethane and add deionized water, extract and collect the organic phase, dry the organic phase with anhydrous magnesium sulfate, filter, and vacuum dry the filter cake to obtain a polysiloxane modified nanocomposite.
4. The production process of a UV-proof fabric according to claim 3, characterized in that: The usage ratio of the carbon dot composite nano titanium dioxide, deionized water, tetrahydrofuran, anhydrous potassium carbonate, 3-aminopropyltrimethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane is 3.45:4.8:16:0.04:7.17:6.
59.
5. The production process of a UV-proof fabric according to claim 3, characterized in that: The carbon dot composite nano titanium dioxide is prepared by the following steps: The nano-carbon dots are prepared into a carbon dot dispersion with a concentration of 1 mg / mL using anhydrous ethanol, and nano-titanium dioxide, deionized water and anhydrous ethanol are added into a reactor, stirred at 300-500 r / min for 3-5 min, and then the carbon dot dispersion is added into the reactor, ultrasonically dispersed for 5-10 min, stirred at 140-145° C. for 4-5 h, cooled naturally, and the reaction product is vacuum dried and ground to obtain carbon dot composite nano-titanium dioxide.
6. The production process of a UV-proof fabric according to claim 5, characterized in that: The dosage ratio of the titanium dioxide, deionized water, anhydrous ethanol and carbon dot dispersion is 0.4-0.45 g: 20 mL: 6 mL: 8-9 mL.
7. The production process of a UV-proof fabric according to claim 5, characterized in that: The nano carbon dots are prepared by the following steps: Citric acid, ethylenediamine, boric acid and deionized water were added into a reaction kettle in a mass ratio of 1:1.1:4.1:180-200, stirred and mixed, kept at 170-180°C for 8-10 hours, cooled naturally, filtered through a 0.22 μm water system microporous filter membrane, and the filtrate was centrifuged at 10000 r / min for 10 minutes. The precipitate was collected and dried to obtain nanocarbon dots.
8. An anti-ultraviolet fabric, characterized in that: It is prepared by the production process described in any one of claims 1 to 7.
Citation Information
Patent Citations
Application of carbon dot @ inorganic oxide to preparation of anti-ultraviolet product
CN106521679A
Preparation method of fluorescent carbon dots capable of rapidly detecting survival state of yeast cells and application of fluorescent carbon dots
CN111978959A
Preparation method of anti-ultraviolet textile fabric
CN112030255A
Antibacterial moisture-permeable multilayer composite fabric and preparation method thereof
CN117656619A
Natural plant-based fiber and preparation method thereof
CN117845355A