Antistatic aramid fiber textile fabric and preparation method thereof
By grafting acrylic acid on the surface of the aramid fiber and forming a conductive silver layer, the problems of poor storage effect and degradation of antistatic properties in low humidity environments are solved, and high washing resistance and excellent antistatic properties are achieved.
Patent Information
- Application Number
- CN202411242688.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Aramid fabrics have poor storage effect in environments with low humidity and their antistatic properties have greatly decreased after multiple washes, making it difficult to meet the long-term demand for antistatic properties.
Supercritical carbon dioxide technology is used to assist acrylic acid on the surface of aramid fibers, and the reaction of cross-linked hyperbranched polyamide-amine and β-cyclodextrin is formed to improve the antistatic properties.
Without damaging the strength of aramid fiber, the washing resistance and anti-static properties of the anti-static fabric are improved, the moisture absorption effect of the fabric and the chelation of silver ions are enhanced, and the stability of the anti-static properties is significantly improved.
Smart Images

Figure BDA0005029757880000191 
Figure HDA0005029757890000011 
Figure HDA0005029757890000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of clothing fabrics, in particular to an antistatic aramid textile fabric and a preparation method thereof. Background Art
[0002] Aramid fiber, also known as fully aromatic polyamide fiber, is a long-chain polymer formed by directly connecting at least 85% of amide groups to benzene rings. Aramid fiber molecular chains are regularly stacked, with high crystallinity, high mechanical properties, thermal stability, wear resistance and corrosion resistance. Aramid fabrics made of aramid fiber also have the excellent properties of aramid fiber. However, in special occasions where antistatic is required, aramid fabrics are difficult to meet actual needs, so it is very necessary to modify aramid fabrics for antistatic properties.
[0003] In traditional fabric processing technology, antistatic properties are usually achieved by adding antistatic finishing agents during fabric production. However, the fabric produced by traditional production processes has poor storage effect in a low humidity environment, and after multiple washings, the antistatic performance is greatly reduced or even completely lost. Therefore, it is of great practical significance to develop an aramid fabric with long-term antistatic properties. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0005] Step (1) coating a 0.5 mol / L acrylic acid ethanol solution on the surface of the aramid fiber soaked in azobisisobutyronitrile, reacting under CO2 supercritical conditions, purifying, and drying to obtain polyacrylic acid grafted aramid fiber;
[0006] In the above reaction process, the free radicals generated by the decomposition of azobisisobutyronitrile extracted the hydrogen of the amide bonds on the surface of the aramid fiber, and the supercritical carbon dioxide promoted the reaction of the hydrophobic groups with the amide bonds. At the same time, the aramid fiber and the free radicals triggered the free radical polymerization reaction of acrylic acid, and polyacrylic acid was grafted on the aramid fiber.
[0007] Step (2) mixing a hyperbranched polyamide-amine and methanol, stirring, then adding diethylene glycol diglycidyl ether, continuing to stir and react, to obtain a cross-linked hyperbranched polyamide-amine mixed system, adding β-cyclodextrin to the cross-linked hyperbranched polyamide-amine mixed system, heating in an oil bath for reaction, filtering, washing, and drying to obtain a modified hyperbranched polyamide-amine;
[0008] In the above reaction process, diethylene glycol diglycidyl ether is used as a cross-linking agent, and the epoxy group of diethylene glycol diglycidyl ether is opened and combined with the amine group of the hyperbranched polyamide-amine, so that a plurality of hyperbranched polyamide-amine molecules are connected to form a network structure, and hydroxyl groups are introduced into the hyperbranched polyamide-amine molecules to obtain a cross-linked hyperbranched polyamide-amine; the hydroxyl groups in the cross-linked hyperbranched polyamide-amine react with the hydroxyl groups in β-cyclodextrin, and more hydroxyl groups are introduced, while increasing the cross-linking density of the network structure.
[0009] Step (3) adding aqueous ammonia to the silver nitrate aqueous solution until the solution becomes clear and transparent, then adding aqueous KOH solution, and again adding aqueous ammonia until the solution becomes clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing glucose, polyethylene glycol, ethanol and water to obtain a reducing solution;
[0010] Step (4) mixing the modified hyperbranched polyamide-amine, polyacrylic acid grafted aramid fiber and methanol, ultrasonicating, heating and stirring, refluxing in a nitrogen atmosphere, cooling to room temperature, filtering, washing and drying to obtain the modified aramid fiber;
[0011] In the above reaction process, the amine groups in the modified hyperbranched polyamide-amine react with the carboxyl groups of the polyacrylic acid-grafted aramid fiber, and the modified hyperbranched polyamide-amine is grafted on the surface of the aramid fiber in the form of chemical bonds.
[0012] Step (5) soaking the modified aramid fiber in a silver plating bath, then dropping a reducing solution, and after the dropping is completed, ultrasonicating, filtering, washing, and drying to obtain an antistatic modified aramid fiber;
[0013] In the above reaction process, the amino groups, carboxyl groups and hydroxyl groups on the surface of the modified aramid fiber chelate with the silver ions to form a conductive silver layer on the surface of the modified aramid fiber.
[0014] Step (6) The antistatic modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
[0015] Preferably, in the step (1), the preparation method of the aramid fiber soaked in azobisisobutyronitrile is as follows: adding the dried aramid fiber and a 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, blowing the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 16-18 MPa with CO2, and heating it to 75-80°C, soaking for 2-2.5 hours, and stirring at 200-300 rpm for 10-20 minutes; wherein, the drying method of the dried aramid fiber is as follows: washing the aramid fiber with acetone at 65-75°C for 20-24 hours, and vacuum drying it at 50-60°C to constant weight.
[0016] Preferably, in the step (1), the mass ratio of the ethanol solution of acrylic acid to the aramid fiber soaked with azobisisobutyronitrile is 1.8:0.8-1.2; CO2 supercritical conditions: pressure 16-18MPa, heating temperature 75-80°C; reaction time: 3-3.5h; purification method: reducing the system pressure to atmospheric pressure, removing the reacted acrylic acid, azobisisobutyronitrile and the polyacrylic acid polymer remaining on the surface of the aramid fiber by acetone extraction; drying conditions: vacuum drying at 50-60°C to constant weight.
[0017] Preferably, in the step (2), the dosage ratio of the hyperbranched polyamide-amine, methanol, diethylene glycol diglycidyl ether and β-cyclodextrin is 8.2-16.4Kg:100-150L:1.0-10.0Kg:12.0-20.0Kg; the mixing temperature is 50-60°C; the stirring condition is stirring at a speed of 150-250rpm for 20-40min; and the stirring reaction time is 5-6h.
[0018] Preferably, in step (2), the oil bath heating reaction conditions are: 60-70° C. for 1-1.5 h; the washing liquid used for washing is distilled water; and the drying conditions are: 40-50° C. for vacuum drying to constant weight.
[0019] Preferably, in step (3), the concentration of the KOH aqueous solution is 6 g / L; the KOH aqueous solution is added dropwise until the pH of the solution reaches 11.0; the dosage ratio of glucose, polyethylene glycol 2000, ethanol and water is 30 Kg:75 g40 L:1000 L.
[0020] Preferably, in the step (4), the amount ratio of the modified hyperbranched polyamide-amine, the polyacrylic acid grafted aramid fiber, and methanol is 10.0-15.0Kg:20.0-25.0Kg:100-200L; ultrasonic conditions: ultrasound at a frequency of 20-30KHz for 10-20min; heating and stirring conditions: temperature of 140-160°C, stirring speed of 180-250rpm; reflux reaction time: 10-14h; the washing liquid used for washing is distilled water; drying conditions: vacuum drying at 40-50°C to constant weight.
[0021] Preferably, in the step (5), the immersion conditions of the modified aramid fiber are: at room temperature, the modified aramid fiber is immersed in the silver plating bath for 30-40 minutes under 20-30KHz ultrasonic conditions; the reducing solution is added dropwise at a rate of 0.05mL / s at 30-40°C; the ultrasonic conditions are: ultrasonic at 30-40°C for 1-1.5h; the washing conditions are: washing the filter residue with deionized water for 3-5 times; and the drying conditions are: drying at 50-60°C to constant weight.
[0022] Preferably, in step (5), the usage ratio of the modified aramid fiber, the silver plating bath and the reducing solution is 0.5-1.0 Kg:100-200 L:100-200 L.
[0023] Furthermore, the antistatic aramid textile fabric is prepared by the method for preparing the antistatic aramid textile fabric.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention uses supercritical carbon dioxide technology to assist the grafting of acrylic acid on the surface of aramid fiber. Under the premise of not damaging the strength of aramid fiber, active groups are introduced on the surface of aramid fiber in the form of chemical bonds, which is helpful for the development of functional aramid fiber materials.
[0026] 2. The present invention grafts the modified hyperbranched polyamide-amine onto the surface of aramid fiber through chemical bonds, thereby improving the washability of the antistatic aramid fabric; at the same time, the modified hyperbranched polyamide-amine contains a large number of groups that can chelate silver ions, which can make the aramid fabric of the present invention have excellent antistatic properties.
[0027] 3. In the present invention, by cross-linking the hydroxyl groups in the hyperbranched polyamide-amine with the hydroxyl groups in β-cyclodextrin, β-cyclodextrin containing a large number of hydroxyl groups is introduced into the network structure of the hyperbranched polyamide-amine, thereby increasing the cross-linking density of the network and improving the stability of the cross-linking system; at the same time, a large number of hydroxyl groups can increase the moisture absorption effect of the fabric and increase the chelating amount of silver ions, thereby further improving the antistatic performance of the aramid fabric. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a process flow chart of the preparation of the antistatic aramid textile fabric of the present invention;
[0029] Figure 2 It is a comparison chart of the surface resistance test of the antistatic aramid textile fabrics of Examples 1-5 and Comparative Examples 1-3 in the present invention;
[0030] Figure 3 It is a comparison chart of the friction voltage test of the antistatic aramid textile fabrics of Examples 1-5 and Comparative Examples 1-3 in the present invention. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] This embodiment discloses a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0034] Step (1) washing the aramid fiber with acetone at 65°C for 20 hours, and vacuum drying at 50°C to constant weight to obtain dry aramid fiber; adding the dry aramid fiber and 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, purging the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 16-18 MPa with CO2, and heating to 75°C, soaking for 2 hours, and stirring at 200 rpm for 10 minutes to obtain aramid fiber soaked with azobisisobutyronitrile; adding 0.5 mol / L ethanol solution of acrylic acid The liquid is coated on the surface of the aramid fiber soaked in azobisisobutyronitrile, and according to the preparation method of the aramid fiber soaked in azobisisobutyronitrile, the reaction is carried out for 3 hours under CO2 supercritical conditions: pressure 16MPa, heating temperature 75°C, and then the system pressure is reduced to atmospheric pressure, and the reacted acrylic acid, azobisisobutyronitrile and the polyacrylic acid polymer remaining on the surface of the aramid fiber are removed by acetone extraction, and vacuum drying is carried out at 50°C to constant weight to obtain polyacrylic acid grafted aramid fiber; wherein the mass ratio between the ethanol solution of acrylic acid and the aramid fiber soaked in azobisisobutyronitrile is 1.8:0.8.
[0035] Step (2) 8.2 kg of hyperbranched polyamide-amine and 100 L of methanol are mixed at 50° C., stirred at a speed of 150 rpm for 20 min, and then 1.0 kg of diethylene glycol diglycidyl ether is added, and the stirring reaction is continued for 5 h to obtain a cross-linked hyperbranched polyamide-amine mixed system, 12.0 kg of β-cyclodextrin is added to the cross-linked hyperbranched polyamide-amine mixed system, and the mixture is heated in an oil bath at 60° C. for 1 h, filtered, and the filter residue is washed with distilled water, and vacuum dried at 40° C. to constant weight to obtain a modified hyperbranched polyamide-amine.
[0036] Step (3) adding aqueous ammonia to 100 L of a 25 g / L silver nitrate aqueous solution until the solution becomes clear and transparent, then adding an aqueous 6 g / L KOH solution until the pH of the solution is 11.0, and then adding aqueous ammonia again until the solution is clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing 30 kg of glucose, 75 g of polyethylene glycol 2000, 40 L of ethanol, and 1000 L of water to obtain a reducing solution.
[0037] Step (4) 10.0 kg of the modified hyperbranched polyamide-amine, 20.0 kg of polyacrylic acid grafted aramid fiber, and 100 L of methanol are mixed, ultrasonicated at 20 kHz for 10 min, refluxed in a nitrogen atmosphere at a temperature of 140° C. and a stirring speed of 180 rpm for 10 h, cooled to room temperature, filtered, washed with distilled water, and vacuum dried at 40° C. to constant weight to obtain modified aramid fiber.
[0038] Step (5) at room temperature, soaking the modified aramid fiber in a silver plating bath under ultrasonic conditions of 20 KHz for 30 minutes, then adding a reducing solution at a rate of 0.05 mL / s at 30° C., and after the addition is completed, ultrasonicating at 30° C. for 1 hour, filtering, washing with deionized water for 3 times, and drying at 50° C. to constant weight to obtain an antistatic modified aramid fiber; wherein the amount ratio of the modified aramid fiber, the silver plating bath, and the reducing solution is 0.5 Kg:100 L:100-L.
[0039] Step (6) The antistatic modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
[0040] Example 2
[0041] This embodiment discloses a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0042] Step (1) washing the aramid fiber with acetone at 75°C for 24 hours, and vacuum drying at 60°C to constant weight to obtain dry aramid fiber; adding the dry aramid fiber and 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, purging the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 18 MPa with CO2, and heating to 80°C, soaking for 2.5 hours, and stirring at 300 rpm for 20 minutes to obtain aramid fiber soaked with azobisisobutyronitrile; adding 0.5 mol / L ethanol solution of acrylic acid The method is applied on the surface of aramid fiber soaked in azobisisobutyronitrile, and reacted for 3.5 hours under supercritical CO2 conditions: pressure of 18 MPa and heating temperature of 80°C, and then the system pressure is reduced to atmospheric pressure. The reacted acrylic acid, azobisisobutyronitrile and the remaining polyacrylic acid polymer on the surface of the aramid fiber are removed by acetone extraction, and the reaction is vacuum dried at 60°C to constant weight to obtain polyacrylic acid grafted aramid fiber; wherein the mass ratio between the ethanol solution of acrylic acid and the aramid fiber soaked in azobisisobutyronitrile is 1.8:1.2.
[0043] Step (2) 16.4 kg of hyperbranched polyamide-amine and 150 L of methanol are mixed at 60° C., stirred at a speed of 250 rpm for 40 min, and then 10.0 kg of diethylene glycol diglycidyl ether is added, and the stirring reaction is continued for 6 h to obtain a cross-linked hyperbranched polyamide-amine mixed system, 20.0 kg of β-cyclodextrin is added to the cross-linked hyperbranched polyamide-amine mixed system, and the mixture is heated in an oil bath at 70° C. for 1.5 h, filtered, and the filter residue is washed with distilled water, and vacuum dried at 50° C. to constant weight to obtain a modified hyperbranched polyamide-amine.
[0044] Step (3) Adding aqueous ammonia to 200 L of a 25 g / L silver nitrate aqueous solution until the solution becomes clear and transparent, then adding an aqueous 6 g / L KOH solution until the pH of the solution is 11.0, and then adding aqueous ammonia again until the solution is clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing 30 kg of glucose, 75 g of polyethylene glycol 2000, 40 L of ethanol, and 1000 L of water to obtain a reducing solution.
[0045] Step (4) 15.0 kg of modified hyperbranched polyamide-amine, 25.0 kg of polyacrylic acid grafted aramid fiber, and 200 L of methanol are mixed, ultrasonicated at 30 kHz for 20 min, refluxed in a nitrogen atmosphere at a temperature of 160° C. and a stirring speed of 250 rpm for 14 h, cooled to room temperature, filtered, washed with distilled water, and vacuum dried at 50° C. to constant weight to obtain modified aramid fiber.
[0046] Step (5) at room temperature, soaking the modified aramid fiber in a silver plating bath under ultrasonic conditions of 30 KHz for 40 minutes, then adding a reducing solution at a rate of 0.05 mL / s at 40° C., and after the addition is completed, ultrasonicating at 40° C. for 1.5 hours, filtering, washing with deionized water for 5 times, and drying at 60° C. to constant weight to obtain an antistatic modified aramid fiber; wherein the amount ratio of the modified aramid fiber, the silver plating bath, and the reducing solution is 1.0 Kg:200 L:200 L.
[0047] Step (6) The antistatic modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
[0048] Example 3
[0049] This embodiment discloses a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0050] Step (1) washing the aramid fiber with acetone at 70°C for 22 hours, and vacuum drying at 55°C to constant weight to obtain dry aramid fiber; adding the dry aramid fiber and 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, purging the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 17 MPa with CO2, and heating to 77°C, soaking for 2.2 hours, and stirring at 250 rpm for 15 minutes to obtain aramid fiber soaked with azobisisobutyronitrile; coating the 0.5 mol / L ethanol solution of acrylic acid on the aramid fiber; On the surface of aramid fiber soaked in azobisisobutyronitrile, according to the preparation method of aramid fiber soaked in azobisisobutyronitrile, react for 3.2 hours under CO2 supercritical conditions: pressure 17MPa, heating temperature 75-80°C, then reduce the system pressure to atmospheric pressure, remove the reacted acrylic acid, azobisisobutyronitrile and the polyacrylic acid polymer remaining on the surface of the aramid fiber by acetone extraction, and vacuum dry at 55°C to constant weight to obtain polyacrylic acid grafted aramid fiber; wherein the mass ratio between the ethanol solution of acrylic acid and the aramid fiber soaked in azobisisobutyronitrile is 1.8:1.0.
[0051] Step (2) 12.4 kg of hyperbranched polyamide-amine and 120 L of methanol are mixed at 55° C., stirred at a speed of 200 rpm for 30 min, and then 5.0 kg of diethylene glycol diglycidyl ether is added, and the stirring reaction is continued for 5.5 h to obtain a cross-linked hyperbranched polyamide-amine mixed system, 16.0 kg of β-cyclodextrin is added to the cross-linked hyperbranched polyamide-amine mixed system, and the mixture is heated in an oil bath at 65° C. for 1.3 h, filtered, and the filter residue is washed with distilled water, and vacuum dried at 45° C. to constant weight to obtain a modified hyperbranched polyamide-amine.
[0052] Step (3) Adding aqueous ammonia to 150 L of a 25 g / L silver nitrate aqueous solution until the solution becomes clear and transparent, then adding an aqueous 6 g / L KOH solution until the pH of the solution is 11.0, and then adding aqueous ammonia again until the solution is clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing 30 Kg of glucose, 75 g of polyethylene glycol 2000, 40 L of ethanol, and 1000 L of water to obtain a reducing solution.
[0053] Step (4) 13.0 kg of modified hyperbranched polyamide-amine, 22.0 kg of polyacrylic acid grafted aramid fiber, and 150 L of methanol are mixed, ultrasonicated at 25 kHz for 15 min, refluxed in a nitrogen atmosphere at a temperature of 150° C. and a stirring speed of 220 rpm for 12 h, cooled to room temperature, filtered, washed with distilled water, and vacuum dried at 45° C. to constant weight to obtain modified aramid fiber.
[0054] Step (5) at room temperature, soaking the modified aramid fiber in a silver plating bath under ultrasonic conditions of 25 kHz for 36 min, then adding a reducing solution at 35° C. at a dropping rate of 0.05 mL / s, and after the addition is completed, ultrasonicating at 35° C. for 1.2 h, filtering, washing with deionized water for 4 times, and drying at 55° C. to constant weight to obtain an antistatic modified aramid fiber; wherein the amount ratio of the modified aramid fiber, the silver plating bath, and the reducing solution is 0.7 Kg:150 L:150 L.
[0055] Step (6) The antistatic modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
[0056] Example 4
[0057] This embodiment discloses a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0058] Step (1) washing the aramid fiber with acetone at 68° C. for 22 hours, and vacuum drying at 52° C. to constant weight to obtain dry aramid fiber; adding the dry aramid fiber and 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, purging the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 17 MPa with CO2, and heating to 76° C., soaking for 2.1 hours, and stirring at 220 rpm for 13 minutes to obtain aramid fiber soaked with azobisisobutyronitrile; coating the 0.5 mol / L ethanol solution of acrylic acid on the aramid fiber; On the surface of aramid fiber soaked in azobisisobutyronitrile, according to the preparation method of aramid fiber soaked in azobisisobutyronitrile, react for 3.1 hours under CO2 supercritical conditions: pressure 17MPa, heating temperature 75-80°C, then reduce the system pressure to atmospheric pressure, remove the reacted acrylic acid, azobisisobutyronitrile and the polyacrylic acid polymer remaining on the surface of the aramid fiber by acetone extraction, and vacuum dry to constant weight at 52°C to obtain polyacrylic acid grafted aramid fiber; wherein the mass ratio between the ethanol solution of acrylic acid and the aramid fiber soaked in azobisisobutyronitrile is 1.8:0.9.
[0059] Step (2) 10.4 kg of hyperbranched polyamide-amine and 110 L of methanol are mixed at 52° C., stirred at a speed of 180 rpm for 25 min, and then 3.0 kg of diethylene glycol diglycidyl ether is added, and the stirring reaction is continued for 5.2 h to obtain a cross-linked hyperbranched polyamide-amine mixed system, 14.0 kg of β-cyclodextrin is added to the cross-linked hyperbranched polyamide-amine mixed system, and the mixture is heated in an oil bath at 62° C. for 1.1 h, filtered, and the filter residue is washed with distilled water, and vacuum dried at 42° C. to constant weight to obtain a modified hyperbranched polyamide-amine.
[0060] Step (3) Adding aqueous ammonia to 130 L of a 25 g / L silver nitrate aqueous solution until the solution becomes clear and transparent, then adding an aqueous 6 g / L KOH solution until the pH of the solution is 11.0, and then adding aqueous ammonia again until the solution is clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing 30 Kg of glucose, 75 g of polyethylene glycol 2000, 40 L of ethanol, and 1000 L of water to obtain a reducing solution.
[0061] Step (4) 11.0 kg of modified hyperbranched polyamide-amine, 21.0 kg of polyacrylic acid grafted aramid fiber, and 120 L of methanol are mixed, ultrasonicated at 22 kHz for 12 min, refluxed in a nitrogen atmosphere at a temperature of 145° C. and a stirring speed of 200 rpm for 11 h, cooled to room temperature, filtered, washed with distilled water, and vacuum dried at 42° C. to constant weight to obtain modified aramid fiber.
[0062] Step (5) at room temperature, soaking the modified aramid fiber in a silver plating bath under ultrasonic conditions of 22 kHz for 33 minutes, then adding a reducing solution at 33°C at a dropping rate of 0.05 mL / s, and after the addition is completed, ultrasonicating at 32°C for 1.1 hours, filtering, washing with deionized water for 3 times, and drying at 52°C to constant weight to obtain an antistatic modified aramid fiber; wherein the amount ratio of the modified aramid fiber, the silver plating bath, and the reducing solution is 0.6 Kg:120 L:120 L.
[0063] Step (6) The antistatic modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
[0064] Example 5
[0065] This embodiment discloses a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0066] Step (1) washing the aramid fiber with acetone at 72° C. for 23 h, and vacuum drying at 58° C. to constant weight to obtain dry aramid fiber; adding the dry aramid fiber and 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, purging the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 18 MPa with CO2, and heating to 78° C., soaking for 2.4 h, and stirring at 280 rpm for 18 min to obtain aramid fiber soaked with azobisisobutyronitrile; adding 0.5 mol / L ethanol solution of acrylic acid The method is as follows: the reaction is carried out under supercritical conditions of CO2: a pressure of 18 MPa and a heating temperature of 78°C for 3.4 hours, and the system pressure is then reduced to atmospheric pressure. The reacted acrylic acid, azobisisobutyronitrile and the remaining polyacrylic acid polymer on the surface of the aramid fiber are removed by acetone extraction, and the reaction is vacuum dried at 58°C to a constant weight to obtain polyacrylic acid grafted aramid fiber; wherein the mass ratio between the ethanol solution of acrylic acid and the aramid fiber soaked in azobisisobutyronitrile is 1.8:1.1.
[0067] Step (2) 14.1 kg of hyperbranched polyamide-amine and 130 L of methanol are mixed at 58° C., stirred at a speed of 220 rpm for 35 min, and then 8.0 kg of diethylene glycol diglycidyl ether is added, and the stirring reaction is continued for 5.8 h to obtain a cross-linked hyperbranched polyamide-amine mixed system, 18.0 kg of β-cyclodextrin is added to the cross-linked hyperbranched polyamide-amine mixed system, and the mixture is heated in an oil bath at 68° C. for 1.4 h, filtered, and the filter residue is washed with distilled water, and vacuum dried at 47° C. to constant weight to obtain a modified hyperbranched polyamide-amine.
[0068] Step (3) Adding aqueous ammonia to 180 L of a 25 g / L silver nitrate aqueous solution until the solution becomes clear and transparent, then adding an aqueous 6 g / L KOH solution until the pH of the solution is 11.0, and then adding aqueous ammonia again until the solution is clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing 30 kg of glucose, 75 g of polyethylene glycol 2000, 40 L of ethanol, and 1000 L of water to obtain a reducing solution.
[0069] Step (4) 14.0 kg of modified hyperbranched polyamide-amine, 24.0 kg of polyacrylic acid grafted aramid fiber, and 180 L of methanol are mixed, ultrasonicated at 28 kHz for 18 min, refluxed in a nitrogen atmosphere at a temperature of 155° C. and a stirring speed of 220 rpm for 13 h, cooled to room temperature, filtered, washed with distilled water, and vacuum dried at 48° C. to constant weight to obtain modified aramid fiber.
[0070] Step (5) at room temperature, soaking the modified aramid fiber in a silver plating bath under ultrasonic conditions of 28 kHz for 38 minutes, then adding a reducing solution at 37°C at a dropping rate of 0.05 mL / s, and after the addition is completed, ultrasonicating at 37°C for 1.3 hours, filtering, washing with deionized water for 4 times, and drying at 58°C to constant weight to obtain an antistatic modified aramid fiber; wherein the amount ratio of the modified aramid fiber, the silver plating bath, and the reducing solution is 0.9 Kg:180 L:180 L.
[0071] Step (6) The antistatic modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
[0072] Comparative Example 1
[0073] This comparative example discloses a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0074] Step (1) 10.4 kg of a hyperbranched polyamide-amine and 110 L of methanol are mixed at 52° C., stirred at a rotation speed of 180 rpm for 25 min, and then 3.0 kg of diethylene glycol diglycidyl ether is added, and the stirring reaction is continued for 5.2 h to obtain a cross-linked hyperbranched polyamide-amine mixed system, 14.0 kg of β-cyclodextrin is added to the cross-linked hyperbranched polyamide-amine mixed system, and the mixture is heated in an oil bath at 62° C. for 1.1 h, filtered, and the filter residue is washed with distilled water, and vacuum dried at 42° C. to constant weight to obtain a modified hyperbranched polyamide-amine.
[0075] Step (2) adding aqueous ammonia to 130 L of a 25 g / L silver nitrate aqueous solution until the solution becomes clear and transparent, then adding aqueous 6 g / L KOH until the pH of the solution is 11.0, and then adding aqueous ammonia again until the solution is clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing 30 Kg of glucose, 75 g of polyethylene glycol 2000, 40 L of ethanol, and 1000 L of water to obtain a reducing solution.
[0076] Step (3) 11.0 kg of modified hyperbranched polyamide-amine, 21.0 kg of aramid fiber, and 120 L of methanol are mixed, ultrasonicated at 22 kHz for 12 min, refluxed in a nitrogen atmosphere at a temperature of 145 ° C and a stirring speed of 200 rpm for 11 h, cooled to room temperature, filtered, washed with distilled water, and vacuum dried at 42 ° C to constant weight to obtain modified aramid fiber.
[0077] Step (4) at room temperature, soaking the modified aramid fiber in a silver plating bath under ultrasonic conditions of 22 kHz for 33 minutes, then adding a reducing solution at 33°C at a dropping rate of 0.05 mL / s, and after the addition is completed, ultrasonicating at 32°C for 1.1 hours, filtering, washing with deionized water for 3 times, and drying at 52°C to constant weight to obtain an antistatic modified aramid fiber; wherein the amount ratio of the modified aramid fiber, the silver plating bath, and the reducing solution is 0.6 Kg:120 L:120 L.
[0078] Step (5) spins, weaves, and dyes the antistatic modified aramid fiber to obtain an antistatic aramid fabric.
[0079] Comparative Example 2
[0080] This comparative example discloses a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0081] Step (1) washing the aramid fiber with acetone at 68° C. for 22 hours, and vacuum drying at 52° C. to constant weight to obtain dry aramid fiber; adding the dry aramid fiber and 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, purging the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 17 MPa with CO2, and heating to 76° C., soaking for 2.1 hours, and stirring at 220 rpm for 13 minutes to obtain aramid fiber soaked with azobisisobutyronitrile; coating the 0.5 mol / L ethanol solution of acrylic acid on the aramid fiber; On the surface of aramid fiber soaked in azobisisobutyronitrile, according to the preparation method of aramid fiber soaked in azobisisobutyronitrile, react for 3.1 hours under CO2 supercritical conditions: pressure 17MPa, heating temperature 75-80°C, then reduce the system pressure to atmospheric pressure, remove the reacted acrylic acid, azobisisobutyronitrile and the polyacrylic acid polymer remaining on the surface of the aramid fiber by acetone extraction, and vacuum dry to constant weight at 52°C to obtain polyacrylic acid grafted aramid fiber; wherein the mass ratio between the ethanol solution of acrylic acid and the aramid fiber soaked in azobisisobutyronitrile is 1.8:0.9.
[0082] Step (2) 10.4 kg of a hyperbranched polyamide-amine and 110 L of methanol are mixed at 52° C., stirred at a speed of 180 rpm for 25 min, and then 3.0 kg of diethylene glycol diglycidyl ether is added, and the stirring reaction is continued for 5.2 h to obtain a cross-linked hyperbranched polyamide-amine mixed system, which is filtered, the filter residue is washed with distilled water, and vacuum dried at 42° C. to constant weight to obtain a cross-linked hyperbranched polyamide-amine.
[0083] Step (3) Adding aqueous ammonia to 130 L of a 25 g / L silver nitrate aqueous solution until the solution becomes clear and transparent, then adding an aqueous 6 g / L KOH solution until the pH of the solution is 11.0, and then adding aqueous ammonia again until the solution is clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing 30 Kg of glucose, 75 g of polyethylene glycol 2000, 40 L of ethanol, and 1000 L of water to obtain a reducing solution.
[0084] Step (4) 11.0 kg of cross-linked hyperbranched polyamide-amine, 21.0 kg of polyacrylic acid grafted aramid fiber, and 120 L of methanol are mixed, ultrasonicated at 22 kHz for 12 min, refluxed in a nitrogen atmosphere at a temperature of 145° C. and a stirring speed of 200 rpm for 11 h, cooled to room temperature, filtered, washed with distilled water, and vacuum dried at 42° C. to constant weight to obtain modified aramid fiber.
[0085] Step (5) at room temperature, soaking the modified aramid fiber in a silver plating bath under ultrasonic conditions of 22 kHz for 33 minutes, then adding a reducing solution at 33°C at a dropping rate of 0.05 mL / s, and after the addition is completed, ultrasonicating at 32°C for 1.1 hours, filtering, washing with deionized water for 3 times, and drying at 52°C to constant weight to obtain an antistatic modified aramid fiber; wherein the amount ratio of the modified aramid fiber, the silver plating bath, and the reducing solution is 0.6 Kg:120 L:120 L.
[0086] Step (6) The antistatic modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
[0087] Comparative Example 3
[0088] This comparative example discloses a method for preparing an antistatic aramid textile fabric, comprising the following steps:
[0089] Step (1) washing the aramid fiber with acetone at 68° C. for 22 hours, and vacuum drying at 52° C. to constant weight to obtain dry aramid fiber; adding the dry aramid fiber and 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, purging the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 17 MPa with CO2, and heating to 76° C., soaking for 2.1 hours, and stirring at 220 rpm for 13 minutes to obtain aramid fiber soaked with azobisisobutyronitrile; coating the 0.5 mol / L ethanol solution of acrylic acid on the aramid fiber; On the surface of aramid fiber soaked in azobisisobutyronitrile, according to the preparation method of aramid fiber soaked in azobisisobutyronitrile, react for 3.1 hours under CO2 supercritical conditions: pressure 17MPa, heating temperature 75-80°C, then reduce the system pressure to atmospheric pressure, remove the reacted acrylic acid, azobisisobutyronitrile and the polyacrylic acid polymer remaining on the surface of the aramid fiber by acetone extraction, and vacuum dry to constant weight at 52°C to obtain polyacrylic acid grafted aramid fiber; wherein the mass ratio between the ethanol solution of acrylic acid and the aramid fiber soaked in azobisisobutyronitrile is 1.8:0.9.
[0090] Step (2) 10.4 kg of hyperbranched polyamide-amine and 110 L of methanol are mixed at 52° C., stirred at a speed of 180 rpm for 25 min, and then 3.0 kg of diethylene glycol diglycidyl ether is added, and the stirring reaction is continued for 5.2 h to obtain a cross-linked hyperbranched polyamide-amine mixed system, 14.0 kg of β-cyclodextrin is added to the cross-linked hyperbranched polyamide-amine mixed system, and the mixture is heated in an oil bath at 62° C. for 1.1 h, filtered, and the filter residue is washed with distilled water, and vacuum dried at 42° C. to constant weight to obtain a modified hyperbranched polyamide-amine.
[0091] Step (3) 11.0 kg of modified hyperbranched polyamide-amine, 21.0 kg of polyacrylic acid grafted aramid fiber, and 120 L of methanol are mixed, ultrasonicated at 22 kHz for 12 min, refluxed in a nitrogen atmosphere at a temperature of 145° C. and a stirring speed of 200 rpm for 11 h, cooled to room temperature, filtered, washed with distilled water, and vacuum dried at 42° C. to constant weight to obtain modified aramid fiber.
[0092] Step (4) The modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
[0093] Experimental example
[0094] The performance tests were performed on the antistatic aramid fabrics in Examples 1-5 and Comparative Examples 1-3:
[0095] Surface resistance: Detect the surface resistance of antistatic aramid fabrics according to GB / T 12703-91 "Test method for electrostatic discharge of textiles";
[0096] Friction voltage: Test the friction voltage of antistatic aramid fabrics according to GB 12014-2009 Antistatic Clothing.
[0097] The test results are shown in Table 1:
[0098] Table 1
[0099]
[0100] From the test results in Table 1, it can be seen that the antistatic aramid fabrics of Examples 1-5 of the present invention not only have excellent antistatic properties, but also have very good washability. From Comparative Example 1, it can be seen that when the aramid fiber is not grafted with acrylic acid, it is connected to the modified hyperbranched polyamide-amine through hydrogen bonds, and the washability will be greatly affected.
[0101] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing an antistatic aramid textile fabric, characterized in that: The following steps are involved: Step (1) coating a 0.5 mol / L acrylic acid ethanol solution on the surface of the aramid fiber soaked in azobisisobutyronitrile, reacting under CO2 supercritical conditions, purifying, and drying to obtain polyacrylic acid grafted aramid fiber; Step (2) mixing a hyperbranched polyamide-amine and methanol, stirring, then adding diethylene glycol diglycidyl ether, continuing to stir and react, to obtain a cross-linked hyperbranched polyamide-amine mixed system, adding β-cyclodextrin to the cross-linked hyperbranched polyamide-amine mixed system, heating in an oil bath for reaction, filtering, washing, and drying to obtain a modified hyperbranched polyamide-amine; Step (3) adding aqueous ammonia to the silver nitrate aqueous solution until the solution becomes clear and transparent, then adding aqueous KOH solution, and again adding aqueous ammonia until the solution becomes clear, and finally, adding 0.5 wt % polyvinyl pyrrolidone to the mixture to obtain a silver plating bath; mixing glucose, polyethylene glycol, ethanol and water to obtain a reducing solution; Step (4) mixing the modified hyperbranched polyamide-amine, polyacrylic acid grafted aramid fiber and methanol, ultrasonicating, heating and stirring, refluxing in a nitrogen atmosphere, cooling to room temperature, filtering, washing and drying to obtain the modified aramid fiber; Step (5) soaking the modified aramid fiber in a silver plating bath, then dropping a reducing solution, and after the dropping is completed, ultrasonicating, filtering, washing, and drying to obtain an antistatic modified aramid fiber; Step (6) The antistatic modified aramid fiber is spun, weaved, dyed and finished to obtain an antistatic aramid fabric.
2. The method for preparing the antistatic aramid textile fabric according to claim 1, characterized in that: In the step (1), the preparation method of the aramid fiber soaked in azobisisobutyronitrile is as follows: adding the dried aramid fiber and 0.04 mol / L ethanol solution of azobisisobutyronitrile into a high-pressure stainless steel container, blowing the air space in the stainless steel container with a CO2 gas flow, pressurizing the stainless steel container to 16-18 MPa with CO2, and heating it to 75-80°C, soaking it for 2-2.5 hours, and stirring it at 200-300 rpm for 10-20 minutes; wherein the drying method of the dried aramid fiber is as follows: washing the aramid fiber with acetone at 65-75°C for 20-24 hours, and vacuum drying it at 50-60°C to constant weight.
3. The method for preparing the antistatic aramid textile fabric according to claim 1, characterized in that: In the step (1), the mass ratio of the ethanol solution of acrylic acid to the aramid fiber soaked with azobisisobutyronitrile is 1.8:0.8-1.2; CO2 supercritical conditions: pressure 16-18MPa, heating temperature 75-80°C; reaction time: 3-3.5h; purification method: reducing the system pressure to atmospheric pressure, removing the reacted acrylic acid, azobisisobutyronitrile and the polyacrylic acid polymer remaining on the surface of the aramid fiber by acetone extraction; drying conditions: vacuum drying at 50-60°C to constant weight.
4. The method for preparing the antistatic aramid textile fabric according to claim 1, characterized in that: In the step (2), the dosage ratio of the hyperbranched polyamide-amine, methanol, diethylene glycol diglycidyl ether and β-cyclodextrin is 8.2-16.4Kg:100-150L:1.0-10.0Kg:12.0-20.0Kg; the mixing temperature is 50-60°C; the stirring condition is stirring at a speed of 150-250rpm for 20-40min; and the stirring reaction time is 5-6h.
5. The method for preparing the antistatic aramid textile fabric according to claim 1, characterized in that: In the step (2), the oil bath heating reaction conditions are: 60-70° C. for 1-1.5 h; the washing liquid used for washing is distilled water; and the drying conditions are: 40-50° C. vacuum drying to constant weight.
6. The method for preparing the antistatic aramid textile fabric according to claim 1, characterized in that: In the step (3), the concentration of the KOH aqueous solution is 6 g / L; the KOH aqueous solution is added dropwise until the pH of the solution reaches 11.0; the dosage ratio of glucose, polyethylene glycol 2000, ethanol, and water is 30 Kg:75 g40 L:1000 L.
7. The method for preparing the antistatic aramid textile fabric according to claim 1, characterized in that: In the step (4), the amount ratio of the modified hyperbranched polyamide-amine, the polyacrylic acid grafted aramid fiber, and methanol is 10.0-15.0Kg:20.0-25.0Kg:100-200L; the ultrasonic condition is 10-20min at a frequency of 20-30KHz; the heating and stirring conditions are 140-160°C and 180-250rpm; the reflux reaction time is 10-14h; the washing liquid used for washing is distilled water; and the drying conditions are vacuum drying at 40-50°C to constant weight.
8. The method for preparing the antistatic aramid textile fabric according to claim 1, characterized in that: In the step (5), the modified aramid fiber is immersed in the silver plating bath for 30-40 minutes under the ultrasonic condition of 20-30KHz at room temperature; the reducing solution is added dropwise at a rate of 0.05mL / s at 30-40°C; Ultrasonic conditions: ultrasonic at 30-40°C for 1-1.5h; washing conditions: wash the filter residue with deionized water 3-5 times; drying conditions: dry at 50-60°C to constant weight.
9. The method for preparing the antistatic aramid textile fabric according to claim 1, characterized in that: In the step (5), the usage ratio of the modified aramid fiber, the silver plating bath solution and the reducing solution is 0.5-1.0 Kg:100-200 L:100-200 L.
10. An antistatic aramid textile fabric prepared by the method according to any one of claims 1 to 9.