Metal chelating agent and preparation method and application thereof

By using polytanninic acid formed by self-polymerization of tanninic acid to coat cellulose nanofibers as metal chelating agents, combining surfactants and corrosion inhibitors, an efficient silicon wafer cleaning agent was prepared, solving metal contamination in the prior art The problem of low removal efficiency significantly improves the removal rate and cleaning efficiency.

CN119061693AActive Publication Date: 2024-12-03JINWAN GAOJING SOLAR ENERGY TECH CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411194049.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The prior art is relatively low in removing metal contamination on the surface of silicon wafers, especially the lack of removal capacity of metal ions such as Cu, Fe, and Ni, which affects the performance of silicon wafers and the efficiency and stability of solar cells.

Method used

A highly efficient silicon wafer cleaning agent was prepared by using polytannin acid-coated cellulose nanofibers (CNFs@PTA) formed by self-polymerization of tannin acid as metal chelating agent. , significantly improves the removal rate of metal ions.

Benefits of technology

It significantly improves the removal rate of metal ions, reduces the overcorrosion rate, reduces the generation of oxidation sheets, saves water resources and electricity, simplifies the cleaning process, and alleviates the pressure of subsequent water treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061693A_ABST
    Figure CN119061693A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of silicon wafer cleaning agents, in particular to a metal chelating agent and a preparation method and application thereof. The metal chelating agent comprises cellulose nanofibers, namely CNFs (at) PTA, at least part of the surfaces of which are coated with polytannic acid. The nanomaterial has the advantages of small size effect, quantum effect, surface effect and the like, the CNFs is a rod-like nanomaterial, has a large number of hydroxyl groups and is easy for surface modification, and the TA is a polyphenol compound, can be subjected to oxidative self-polymerization reaction under alkaline conditions, can be quickly combined with a matrix and can be deposited on the surface of the matrix to form a polyphenol layer, so that the surface of the matrix is protected. The CNFs (at) PTA has the advantages that the CNFs (at) PTA has excellent metal ion chelation capability, the ortho-phenolic hydroxyl group of the CNFs (at) PTA can be subjected to complexation reaction with metal ions, the surfaces of the CNFs (at) PTA are coated with the polytannic acid through TA auto-polymerization, the obtained CNFs (at) PTA has excellent metal ion chelation capability, and metal pollution can be effectively removed by applying the CNFs (at) PTA to the silicon wafer cleaning agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon wafer cleaning agents, and in particular to a metal chelating agent and a preparation method and application thereof. Background Art

[0002] With the rapid development of solar silicon cells, people's requirements for quality have exploded, which has brought new challenges to the efficiency and stability of silicon cells. Among them, the surface cleanliness of silicon wafers is one of the key factors, which directly affects the power generation efficiency of solar cells. Therefore, for high-efficiency solar cells, the cleaning of silicon wafer surfaces is very important.

[0003] Silicon wafers come from the cutting of silicon rods. There are roughly four types of dirt generated during the cutting process: one is dust pollution; two is organic pollution, which mainly comes from the cutting fluid used in the production process; three is metal pollution, which mainly comes from production equipment and diamond wire; four is silicon powder pollution, which mainly comes from the silicon powder generated during the cutting process.

[0004] Among them, metal pollution is one of the more serious pollution sources in the silicon wafer production process. Metal pollution can cause the structure and performance of the silicon wafer surface to deteriorate. For example, metal ions will form oxides on the surface of the silicon wafer, causing charge loss, affecting electron migration, and causing silicon wafer performance degradation. At present, due to the use of diamond wire cutting, the metal ion pollution introduced during the silicon rod processing process is becoming more and more obvious. In order to remove metal ions, amine cleaning components with chelating effects are often added to the cleaning agent, but their removal power for metal ions is weak, especially the removal of metal ions such as Cu, Fe, and Ni. Therefore, the development of an efficient metal chelating agent and a silicon wafer cleaning agent with efficient removal of metal pollution, as well as a preparation method and a silicon wafer cleaning method, is of great significance for ensuring the quality of silicon wafers and improving the excellence and stability of solar silicon wafer cells.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first object of the present invention is to provide a metal chelating agent, which has a strong chelating ability for metal ions and can be used in a cleaning agent to efficiently remove metal pollution.

[0007] The second object of the present invention is to provide a method for preparing the metal chelator as described above, wherein polytannic acid is deposited on the surface of CNFs through self-polymerization of tannic acid, and the obtained CNFs@PTA has excellent metal chelating ability, and the preparation process is simple and controllable.

[0008] The third object of the present invention is to provide a use of the metal chelating agent as described above or the metal chelating agent prepared by the method for preparing the metal chelating agent as described above in preparing a silicon wafer cleaning agent.

[0009] The fourth object of the present invention is to provide a silicon wafer cleaning agent, which can significantly improve the removal rate of metal ions and effectively remove metal pollution.

[0010] The fifth object of the present invention is to provide a method for preparing the silicon wafer cleaning agent as described above, which has a simple preparation process, mild and controllable conditions, and is convenient for mass production.

[0011] A sixth object of the present invention is to provide a method for cleaning a silicon wafer.

[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0013] A metal chelator comprises cellulose nanofibers at least partially coated with polytannic acid, namely CNFs@PTA.

[0014] A method for preparing a metal chelating agent comprises the following steps:

[0015] The cellulose nanofibers and the pH buffer are added to the tannic acid solution to obtain a mixed solution, the pH of the mixed solution is adjusted to 8.6-9.5, the mixture is stirred for reaction, the solid-liquid separation is performed, and the mixture is dried to obtain the CNFs@PTA.

[0016] Use of the metal chelating agent described in the aforementioned embodiment or the metal chelating agent prepared by the preparation method of the metal chelating agent described in the aforementioned embodiment in preparing a silicon wafer cleaning agent.

[0017] A silicon wafer cleaning agent comprises a first metal chelating agent, a surfactant, an alkali, a corrosion inhibitor, an auxiliary agent and water;

[0018] The first metal chelator is the metal chelator described in the above embodiment or a metal chelator prepared by the preparation method of the metal chelator described in the above embodiment.

[0019] A method for preparing a silicon wafer cleaning agent comprises the following steps:

[0020] The surfactant is mixed with water, and the base is added under stirring, and the stirring is continued for 10-20 minutes; the first metal chelating agent and / or the second metal chelating agent, the corrosion inhibitor and the auxiliary agent are added, and the mixture is stirred until they are completely dissolved.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The metal chelating agent provided by the present invention comprises cellulose nanofibers at least partially coated with polytannic acid, i.e., CNFs@PTA. The nanomaterial has the advantages of small size effect, quantum effect and surface effect, and can effectively improve the performance of the material. CNFs is a rod-shaped nanomaterial and contains a large number of hydroxyl groups, which are easy to surface modify. Tannic acid is a polyphenol compound that can undergo oxidative self-polymerization under alkaline conditions and quickly combine with the matrix. At the same time, the ortho-phenolic hydroxyl structure on TA can undergo complexation reaction with metal ions. The present invention deposits polytannic acid on the surface of CNFs to form a polyphenol layer through TA self-polymerization. The obtained CNFs@PTA has excellent metal ion chelating ability and is used in silicon wafer cleaning agents to effectively remove metal pollution.

[0023] (2) The silicon wafer cleaning agent provided by the present invention includes a new high-efficiency metal chelating agent component (CNFs@PTA), a surfactant with strong decontamination ability, a corrosion inhibitor and a defoaming aid. Compared with traditional cleaning agents, the removal rate of metal ions and the metal cleaning efficiency are greatly improved, and the cleaning ability is strong. It can effectively reduce the over-corrosion rate, reduce or prevent the generation of oxide sheets, and produce less cleaning foam, which can not only save water resources, reduce cleaning time and production electricity, but also relieve the pressure of subsequent water treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 is the structural formula of tannic acid;

[0026] Figure 2 The general structural formula of the cellulose nanofibers provided in the embodiments of the present invention;

[0027] Figure 3 A cleaning process flow chart provided for an embodiment of the present invention. DETAILED DESCRIPTION

[0028] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0029] A first aspect of the present invention provides a metal chelator, comprising cellulose nanofibers at least partially coated with polytannic acid, namely CNFs@PTA.

[0030] like Figure 1 As shown in the figure, tannic acid (TA) is a polyphenolic compound rich in catechol and pyrogallol groups. It can undergo oxidative self-polymerization under alkaline conditions, quickly combine with a variety of substrates, and deposit on the substrate surface to form a polyphenol layer. It is an efficient and environmentally friendly surface modification method. In addition, the multiple ortho-phenolic hydroxyl structures of TA can be used as a polyhydroxy ligand to react with metal ions. Two adjacent phenolic hydroxyl groups can form a stable five-membered ring chelate with metal ions in the form of oxygen anions. Although the third phenolic hydroxyl group in the pyrogallol structure does not participate in the complexation, it can promote the dissociation of the other two phenolic hydroxyl groups, thereby promoting the formation and stability of the complex.

[0031] Nanomaterials can effectively improve the performance of materials due to their advantages such as small size effect, quantum effect, and surface effect. Figure 2 As shown in Figure 2, cellulose nanofibers (CNFs) are rod-shaped nanomaterials with a large number of hydroxyl groups. Therefore, CNFs are also a material that is easy to surface modify.

[0032] The CNFs@PTA obtained by coating the surface of CNFs with polytannic acid has excellent metal ion chelating ability and is used in silicon wafer cleaning agents. Compared with conventional amine complexing agents and tannic acid complexing agents, the removal rate of metal ions such as Cu, Fe, and Ni can be significantly improved, and the metal pollution on solar silicon wafers can be effectively removed to improve the performance of silicon wafers.

[0033] The second aspect of the present invention provides a method for preparing the metal chelating agent described in the aforementioned embodiment, comprising the following steps:

[0034] The cellulose nanofibers and the pH buffer are added to the tannic acid solution to obtain a mixed solution, the pH of the mixed solution is adjusted to 8.6-9.5, the mixture is stirred for reaction, the solid-liquid is separated, and the mixture is dried to obtain CNFs@PTA.

[0035] The present invention allows TA to undergo an oxidative self-polymerization reaction under alkaline conditions to form polytannic acid (PTA), which combines with CNFs and is deposited on the surface of CNFs to form a polyphenol layer, thereby obtaining cellulose nanofibers (CNFs@PTA) at least partially coated with polytannic acid on the surface. CNFs@PTA not only has excellent metal chelating ability, but also has a simple and controllable preparation process, which is convenient for mass production and application.

[0036] In some embodiments, typically but not limiting, for example, the pH of the mixed solution can be adjusted to any value among 8.6, 8.8, 9.0, 9.2, 9.5, or a range consisting of any two values.

[0037] In some specific embodiments of the present invention, the mass ratio of cellulose nanofibers to tannic acid in the mixed solution is 0.5-1:10, typically but not restrictively, for example, it can be any point value among 0.5:10, 0.6:10, 0.7:10, 0.8:10, 0.9:10, 1:10 or a range value consisting of any two point values; too large or too small a mass ratio of CNFs to TA will lead to a decrease in the metal ion chelating ability, thereby affecting the metal ion removal rate. This is because when the amount of TA is too large, the small size effect, quantum effect and surface effect of CNFs cannot be reflected; and when the amount of CNFs is too large, the phenolic hydroxyl group of the system is greatly reduced and the chelating effect is reduced, so it is necessary to reasonably control the mass ratio of CNFs to TA.

[0038] In some specific embodiments of the present invention, the tannic acid solution may be an aqueous solution of tannic acid.

[0039] In some specific embodiments of the present invention, the mass concentration of tannic acid in the tannic acid solution is 0.2%-1%, typically but not limitatively, for example, it can be any point value among 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1% or a range value consisting of any two point values.

[0040] In some embodiments of the invention, the pH buffer comprises Tris buffer.

[0041] In some specific embodiments of the present invention, the stirring reaction time of the mixed solution is 20-30h. Typically but not limitatively, for example, the stirring reaction time can be any point value among 20h, 22h, 24h, 26h, 28h, 30h or a range value consisting of any two point values.

[0042] The third aspect of the present invention provides a use of the metal chelating agent as described in the aforementioned embodiment or the metal chelating agent prepared by the preparation method of the metal chelating agent as described in any one of the aforementioned embodiments in preparing a silicon wafer cleaning agent.

[0043] A fourth aspect of the present invention provides a silicon wafer cleaning agent, comprising a first metal chelating agent, a surfactant, an alkali, a corrosion inhibitor, an auxiliary agent and water.

[0044] The first metal chelator is the metal chelator described in the aforementioned embodiment or a metal chelator prepared by the method for preparing a metal chelator described in any one of the aforementioned embodiments.

[0045] Compared with traditional cleaning agents, the silicon wafer cleaning agent provided by the present invention adopts a new type of metal chelating agent, which greatly improves the removal rate of metal ions; and adds alkali and a surfactant with strong decontamination ability, so it has strong decontamination ability; adds a corrosion inhibitor, which can effectively reduce the over-corrosion rate and reduce or prevent the generation of oxide sheets; adds a defoaming aid, so there is less cleaning foam, which can not only save water resources, reduce cleaning time and production electricity, but also relieve the pressure of subsequent water treatment.

[0046] In some specific embodiments of the present invention, the silicon wafer cleaning agent includes, by mass percentage, 10%-20% of alkylphenol polyoxyethylene ether, 2%-5% of fatty alcohol polyoxyethylene ether, 2%-4% of alkali, 0.5%-5% of the first metal chelating agent, 2%-5.5% of the corrosion inhibitor, 0.1%-0.3% of the auxiliary agent, and the remainder of water. To avoid impurities, the water is preferably deionized water.

[0047] In some embodiments, typically but not limiting, for example, in the silicon wafer cleaning agent, the mass percentage of alkylphenol polyoxyethylene ether can be any point value among 10%, 12%, 14%, 16%, 18%, 20%, or a range value consisting of any two point values; the mass percentage of fatty alcohol polyoxyethylene ether can be any point value among 2%, 3%, 4%, 5%, or a range value consisting of any two point values; the mass percentage of the base can be any point value among 2%, 2.5%, 3%, 3.5%, 4%, or a range value consisting of any two point values; the mass percentage of the first metal chelating agent can be any point value among 0.5%, 1%, 2%, 3%, 4%, 5%, or a range value consisting of any two point values; the mass percentage of the corrosion inhibitor can be any point value among 2%, 3%, 4%, 5%, 5.5%, or a range value consisting of any two point values; the mass percentage of the auxiliary agent can be any point value among 0.1%, 0.2%, 0.3%, or a range value consisting of any two point values.

[0048] In some specific embodiments of the present invention, the silicon wafer cleaning agent also includes a second metal chelating agent, and the second metal chelating agent is selected from disodium ethylenediaminetetraacetic acid and / or diethylenetriaminepentaacetic acid; the first metal chelating agent and the second metal chelating agent can produce a synergistic effect when used in combination, and the metal pollution removal effect is better.

[0049] In some specific embodiments of the present invention, the mass concentration of disodium ethylenediaminetetraacetate in the silicon wafer cleaning agent is 0-1%.

[0050] In some specific embodiments of the present invention, the mass concentration of diethylenetriaminepentaacetic acid in the silicon wafer cleaning agent is 0%-2%.

[0051] In some specific embodiments of the present invention, the mass ratio of the first metal chelating agent, disodium ethylenediaminetetraacetic acid and diethylenetriaminepentaacetic acid is 1-4:1-2:1-4.

[0052] In some specific embodiments of the present invention, the corrosion inhibitor includes at least one of diethanolamine, triethanolamine and ethylenediamine. The organic base corrosion inhibitor is used to reduce the over-corrosion rate and prevent the generation of oxide sheets. The corrosion inhibitors used contain N elements and have a certain ability to complex metal ions, which can assist the metal chelating agent in completing the removal of metal ions.

[0053] In some specific embodiments of the present invention, the mass concentration of diethanolamine in the silicon wafer cleaning agent is 0%-0.5%; and / or, the mass concentration of triethanolamine in the silicon wafer cleaning agent is 0.1%-3%; and / or, the mass concentration of ethylenediamine in the silicon wafer cleaning agent is 0%-2%.

[0054] In some specific embodiments of the present invention, the alkali used in the silicon wafer cleaning agent includes NaOH and / or KOH.

[0055] In some specific embodiments of the present invention, the auxiliary agent includes at least one of an organosilicon defoamer, a fatty alcohol defoamer and a silicone defoamer. By adding the defoamer, less foam is produced during cleaning, which not only saves water resources, reduces cleaning time and production electricity, but also alleviates the subsequent water treatment pressure.

[0056] A fifth aspect of the present invention provides a method for preparing a silicon wafer cleaning agent as described in any one of the aforementioned embodiments, comprising the following steps:

[0057] The surfactant is mixed with water, and the base is slowly added in small amounts several times under stirring at a speed of 300-500 rpm, and the stirring is continued for 10-20 minutes to fully dissolve and mix the base; then a metal chelating agent (the metal chelating agent here refers to the first metal chelating agent or the combination of the first metal chelating agent and the second metal chelating agent), a corrosion inhibitor and an auxiliary agent are added to the above solution, and the base is stirred until it is completely dissolved.

[0058] In some embodiments, typically but not limitatively, for example, the stirring speed when preparing the cleaning agent can be any point value among 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, or a range value consisting of any two point values; after adding the alkali, the time for continuing stirring and dissolving can be any point value among 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, or a range value consisting of any two point values.

[0059] Some embodiments of the present invention are described in detail below in conjunction with specific examples. The CNFs used in the examples were purchased from CNFs prepared by mechanical method of SCIENCEK; the other raw materials used can be purchased from the market unless otherwise specified.

[0060] Example 1

[0061] Preparation of CNFs@PTA:

[0062] Weigh 0.6 g of TA powder, add 99.4 g of deionized water to prepare a 0.6% TA aqueous solution, add 0.04 g of CNFs, and make the mass ratio of CNFs to TA 1:15;

[0063] An appropriate amount of pH buffer Tris (trishydroxymethylaminomethane) was added to adjust the pH value of the above solution to about 9. After stirring and reacting at room temperature for 24 hours, the solution was centrifuged and dried to obtain CNFs@PTA.

[0064] Calculated by mass percentage, the silicon wafer cleaning agent includes the following components:

[0065] Alkylphenol polyoxyethylene ether (OP-9) 15%, fatty alcohol polyoxyethylene ether (AEO-9) 3%, NaOH 3%, CNFs@PTA 2%, disodium ethylenediaminetetraacetic acid 0.5%, diethylenetriaminepentaacetic acid 0.5%, diethanolamine 0.5%, triethanolamine 2%, ethylenediamine 1.5%, isopropanol 0.2%, and the balance is water.

[0066] The preparation method of the above cleaning agent is as follows:

[0067] Mix the surfactant alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and deionized water, slowly add NaOH in small amounts several times at a stirring speed of 400 rpm, continue stirring at room temperature for 15 minutes, add metal chelating agents (first metal chelating agent and second metal chelating agent), corrosion inhibitor and isopropanol auxiliary agent in sequence, stir until completely dissolved, and obtain a cleaning agent.

[0068] Example 2

[0069] Synthesis of CNFs@PTA:

[0070] Weigh 0.6 g of TA powder, add 99.4 g of deionized water to prepare a 0.6% TA aqueous solution, add 0.04 g of CNFs, and make the mass ratio of CNFs to TA 1:15;

[0071] An appropriate amount of pH buffer Tris (trishydroxymethylaminomethane) was added to adjust the pH value of the above solution to about 9. After stirring and reacting at room temperature for 24 hours, the solution was centrifuged and dried to obtain CNFs@PTA.

[0072] Calculated by mass percentage, the silicon wafer cleaning agent includes the following components:

[0073] Alkylphenol polyoxyethylene ether (OP-9) 20%, fatty alcohol polyoxyethylene ether (AEO-9) 5%, NaOH 4%, CNFs@PTA 2%, disodium ethylenediaminetetraacetic acid 1%, diethylenetriaminepentaacetic acid 2%, diethanolamine 0.5%, triethanolamine 3%, ethylenediamine 2%, isopropanol 0.3%, and the balance is water.

[0074] The preparation method of the above cleaning agent is as follows:

[0075] Mix the surfactant alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and deionized water, slowly add NaOH in small amounts several times at a stirring speed of 500 rpm, continue stirring at room temperature for 20 minutes, add metal chelating agents (first metal chelating agent and second metal chelating agent), corrosion inhibitor and isopropanol auxiliary agent in sequence, stir until completely dissolved, and obtain a cleaning agent.

[0076] Example 3

[0077] Synthesis of CNFs@PTA:

[0078] Weigh 0.6 g of TA powder, add 99.4 g of deionized water to prepare a 0.6% TA aqueous solution, add 0.04 g of CNFs, and make the mass ratio of CNFs to TA 1:15;

[0079] An appropriate amount of pH buffer Tris (trishydroxymethylaminomethane) was added to adjust the pH value of the above solution to about 9. After stirring and reacting at room temperature for 24 hours, the solid-liquid was separated and dried to obtain CNFs@PTA.

[0080] Calculated by mass percentage, the silicon wafer cleaning agent includes the following components:

[0081] Alkylphenol polyoxyethylene ether (OP-9) 10%, fatty alcohol polyoxyethylene ether (AEO-9) 3%, NaOH 2%, CNFs@PTA 0.5%, diethanolamine 0.5%, triethanolamine 0.5%, ethylenediamine 1%, isopropanol 0.1%, and the balance is water.

[0082] The preparation method of the above cleaning agent is as follows:

[0083] Mix the surfactant alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and deionized water, slowly add NaOH in small amounts several times at a stirring speed of 300 rpm, continue stirring at room temperature for 10 minutes, add metal chelating agent, corrosion inhibitor and isopropanol auxiliary agent in sequence, stir until completely dissolved, and the cleaning agent is obtained.

[0084] Example 4

[0085] The difference between Example 4 and Example 1 is that during the synthesis of CNFs@PTA, the amount of CNFs is changed so that the mass ratio of CNFs to TA is 1:10, and the other conditions are the same as in Example 1.

[0086] Example 5

[0087] The difference between Example 5 and Example 1 is that during the synthesis of CNFs@PTA, the amount of CNFs is changed so that the mass ratio of CNFs to TA is 1:20, and the other conditions are the same as in Example 1.

[0088] Example 6

[0089] The difference between Example 6 and Example 1 is that the metal chelating agent in the cleaning agent component is all CNFs@PTA, no disodium ethylenediaminetetraacetic acid and diethylenetriaminepentaacetic acid are added, the total amount of the metal chelating agent remains unchanged, and the other conditions are the same as Example 1.

[0090] Comparative Example 1

[0091] The difference between Comparative Example 1 and Example 1 is that the CNFs@PTA in Example 1 is replaced with an equal amount of tannic acid, and the other conditions are the same as Example 1.

[0092] Comparative Example 2

[0093] The difference between Comparative Example 2 and Example 1 is that the metal chelating agent in the cleaning agent component is all diethylenetriaminepentaacetic acid, CNFs@PTA and disodium ethylenediaminetetraacetate are not added, the total amount of the metal chelating agent remains unchanged, and the other conditions are the same as Example 1.

[0094] Comparative Example 3

[0095] The difference between Comparative Example 3 and Example 1 is that the metal chelating agent in the cleaning agent component is all disodium ethylenediaminetetraacetic acid, CNFs@PTA and diethylenetriaminepentaacetic acid are not added, the total amount of the metal chelating agent remains unchanged, and the other conditions are the same as Example 1.

[0096] Test example

[0097] The cleaning agents prepared in the embodiments and comparative examples were used to clean the silicon wafers, and the cleaning effects were statistically analyzed. The cleaning process is as follows:

[0098] like Figure 3 As shown, slots 1-2 are pure water slots, slots 3-5 are reagent slots, 3 L of the cleaning agent in the example needs to be added to each reagent slot, slots 6-8 are the same as slots 1-2, slots 9-10 are pure water slots without ultrasound, the ultrasonic power of slots 1-8 is about 1.2 KW, the water volume of each slot in slots 1-10 is about 500 L, and the time is 180 s, slot 11 is a slow pulling slot, the time is 120 s, and slots 12-13 are drying slots, the temperature is set to 110 ° C, and the time is 300 s.

[0099] The over-corrosion rate of the silicon wafer surface after cleaning is obtained from the sorting results of the sorting machine, and the metal ion content test standard is determined using GB / T 39145-2020.

[0100] The experimental results are shown in Table 1.

[0101] Table 1

[0102]

[0103]

[0104] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A metal chelating agent, characterized in that: The invention comprises cellulose nanofibers at least part of which are coated with polytannic acid, namely CNFs@PTA.

2. The method for preparing a metal chelating agent according to claim 1, wherein The following steps are involved: The cellulose nanofibers and the pH buffer are added to the tannic acid solution to obtain a mixed solution, the pH of the mixed solution is adjusted to 8.6-9.5, the mixture is stirred for reaction, the solid-liquid separation is performed, and the mixture is dried to obtain the CNFs@PTA.

3. The method for preparing a metal chelating agent according to claim 2, characterized in that: Contains at least one of the following characteristics: (1) The mass ratio of the cellulose nanofibers to tannic acid is 0.5-1:10; (2) The mass concentration of tannic acid in the tannic acid solution is 0.2%-1%; (3) The pH buffer comprises a Tris buffer; (4) The stirring reaction time is 20-30 hours.

4. Use of the metal chelating agent according to claim 1 or the metal chelating agent prepared by the preparation method of the metal chelating agent according to claim 2 or 3 in preparing a silicon wafer cleaning agent.

5. A silicon wafer cleaning agent, characterized in that: comprising a first metal chelating agent, a surfactant, an alkali, a corrosion inhibitor, an additive and water; The first metal chelator is the metal chelator according to claim 1 or a metal chelator prepared by the preparation method of the metal chelator according to claim 2 or 3.

6. The silicon wafer cleaning agent according to claim 5, characterized in that: Measured by mass percentage, the silicon wafer cleaning agent includes 10%-20% of alkylphenol polyoxyethylene ether, 2%-5% of fatty alcohol polyoxyethylene ether, 2%-4% of the alkali, 0.5%-5% of the first metal chelating agent, 2%-5.5% of the corrosion inhibitor, 0.1%-0.3% of the auxiliary agent, and the balance of water.

7. The silicon wafer cleaning agent according to claim 5 or 6, characterized in that: The silicon wafer cleaning agent further comprises a second metal chelating agent, wherein the second metal chelating agent is selected from disodium ethylenediaminetetraacetic acid and / or diethylenetriaminepentaacetic acid; Preferably, the mass concentration of disodium edetate is 0-1%; Preferably, the mass concentration of the diethylenetriaminepentaacetic acid is 0-2%.

8. The silicon wafer cleaning agent according to claim 5, characterized in that: Meet at least one of the following characteristics: (1) The corrosion inhibitor comprises at least one of diethanolamine, triethanolamine and ethylenediamine; (2) the base comprises NaOH and / or KOH; (3) The auxiliary agent includes at least one of an organic silicon defoamer, a fatty alcohol defoamer and a silicone defoamer.

9. The method for preparing a silicon wafer cleaning agent according to any one of claims 5 to 8, characterized in that: The following steps are involved: The surfactant is mixed with water, and the base is added under stirring, and the stirring is continued for 10-20 minutes; the first metal chelating agent and / or the second metal chelating agent, the corrosion inhibitor and the auxiliary agent are added, and the mixture is stirred until they are completely dissolved.

10. A method for cleaning a silicon wafer, characterized in that: The silicon wafer surface is cleaned using the silicon wafer cleaning agent described in any one of claims 5 to 8.

Citation Information

Patent Citations

  • Cleaning agent used for solar grade silicon wafers and preparing method thereof

    CN105039006A

  • Cellulose / tannin micro-nano fibers and preparation method thereof

    CN105536727A

  • Conductive glass fiber and preparation method thereof

    CN112010572A

  • Tannic acid coated nanocellulose / polyacrylic acid adhesive hydrogel and preparation method thereof

    CN112266486A

  • Preparation method of PVA composite hydrogel

    CN115894967A