Outdoor home furnishing fabric fluoride-free processing technology

Through the antibacterial treatment of fluorine-free waterproofing agent and crosslinking agent finishing solution and the antibacterial treatment of the jumbled polyurethane microcapsules, the environmental and health hazards of organic fluorine finishing agent in the fabric are solved, and the water repellent, wear resistance and antibacterial properties of the fabric are achieved, improving the water repellent, wear resistance and antibacterial properties of the fabric. The weather resistance and ease of use of fabrics.

CN119061698APending Publication Date: 2024-12-03GLEN RAVEN TEXTILE TECH SUZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411315833.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The organic fluorine finishing agent used in existing fabrics is difficult to decompose, resulting in environmental pollution and human health hazards, and it is difficult to achieve good weather resistance and antibacterial properties.

Method used

The finishing solution without fluorine-free waterproofing agent and crosslinking agent is used for impregnation and baking treatment, combined with the antibacterial treatment of the jumbled polyurethane microcapsules, and the liquid spraying and spraying technology are used to fully enter the fabric to form a water-repellent and antibacterial layer.

Benefits of technology

The fabric is water repellent, wear-resistant and antibacterial properties are achieved, the total fluorine content is reduced, the fabric is weather-resistant and convenient to use, and the heat consumed in drying is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052161220000081
    Figure BDA0005052161220000081
  • Figure BDA0005052161220000091
    Figure BDA0005052161220000091
  • Figure BDA0005052161220000101
    Figure BDA0005052161220000101
Patent Text Reader

Abstract

The invention relates to the technical field of fabric finishing, and particularly discloses a fluoride-free processing technology for an outdoor home fabric. The fluoride-free processing technology for the outdoor home furnishing fabric comprises the following steps: (1) padding: adopting a continuous finishing technology, uniformly dipping the fabric in a finishing liquid through liquid spraying and a dipping tank, then carrying out compression roller treatment to enable the liquid carrying rate of the fabric to be 57-63%, and carrying out vacuum suction to enable the liquid carrying rate of the fabric to be 23-27%; after preliminary pre-drying, the fabric is uniformly coated with the antibacterial and wear-resistant finishing liquid in a mist spraying or spraying mode; (2) baking: the fabric is placed in a baking oven, the temperature of the baking oven is 170-180 DEG C, the temperature of the fabric cover is 170-173 DEG C, and the baking time is 10-20 s; in addition, the preparation method provided by the invention has the advantage of reducing the harm to the environment and human body caused by fluorine contained in the fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of fabric finishing, and more specifically, to a fluorine-free processing technology for outdoor home fabrics. Background Art

[0002] With the improvement of living standards and quality of life, people have higher and higher functional requirements for textiles. For example, if the fabrics of outdoor household items have water-repellent properties, the fabrics of household items can be easy to clean, and at the same time have good weather resistance and water washability, making them more convenient to use.

[0003] Currently, the water-repellent properties of fabrics are usually achieved using organic fluorine finishing agents, such as PFAS, PFOS, etc., but PFAS is difficult to decompose and will affect the human immune system, sex hormone levels, thyroid function, etc., and because it is difficult to degrade, it will persist in the environment and accumulate through the food chain, causing harm to human health and the natural world. Summary of the invention

[0004] In order to reduce the harm of fluorine in fabrics to the environment and human body, the present application provides a fluorine-free processing technology for outdoor home fabrics, which adopts the following technical solutions: A fluorine-free processing technology for outdoor home fabrics comprises the following steps: (1) Padding and vacuum suction: A continuous finishing process is adopted, the fabric is evenly impregnated with finishing liquid through a liquid spray and an impregnation tank, and then processed by a pressing roller, so that the fabric liquid carrying rate is 57-63%. After vacuum suction, the fabric liquid carrying rate is 23-27%; the finishing liquid includes 50-100g / L fluorine-free waterproofing agent, 5-25g / L cross-linking agent, 5-10g / L wear resistance improving agent and pH value adjusting agent, and the pH value of the finishing liquid is 5-6; (2) Pre-drying: The impregnated fabric is sent to a drying oven for treatment, so that the fabric liquid content is 15-20%; (3) Post-treatment: Apply post-treatment liquid to the fabric by spraying or coating; (4) Baking: Place the fabric in an oven at a temperature of 170-180°C, a surface temperature of 170-173°C, and a baking time of 10-20 seconds.

[0005] By adopting the above technical solution, after the fabric is sprayed and impregnated with the finishing liquid, the finishing liquid fully enters the interior of the fabric, so that the fabric has water-repellent properties and good wear resistance. The finishing liquid is a fluorine-free waterproof agent, which can reduce the total fluorine content of the fabric after finishing. By squeezing and vacuum suction, the liquid carrying rate of the fabric is reduced, thereby reducing the heat consumed in the subsequent drying of the fabric, and controlling the baking time and temperature so that the finishing liquid has the best finishing effect on the fabric, and the fabric can be kept dry.

[0006] By controlling the concentration of fluorine-free waterproofing agent and cross-linking agent and the pH of the finishing liquid, the finishing liquid can have a better finishing effect on the fabric. The finished fabric has a relatively good water-repellent effect, and the total fluorine content is less than 50ppm. The wear-resistant enhancer can further improve the wear resistance of the fabric, thereby improving the weather resistance of the fabric.

[0007] Preferably, the finishing liquid comprises 80-90 g / L of fluorine-free waterproofing agent, 10-15 g / L of cross-linking agent, 5-10 g / L of wear resistance improving agent and pH value adjusting agent, and the pH value of the finishing liquid is 5-6.

[0008] By adopting the above technical solution, the concentration of the fluorine-free waterproofing agent and the cross-linking agent is further limited, so that the comprehensive properties such as water repellency formed by the waterproofing agent on the fabric are better.

[0009] Preferably, the fluorine-free waterproofing agent is selected from one of polyurethane fluorine-free waterproofing agent emulsion, acrylic fluorine-free waterproofing agent emulsion, and silicone fluorine-free waterproofing agent emulsion, the cross-linking agent is selected from a blocked isocyanate compound dispersion, and the wear-resistant enhancer is selected from a high-density polyethylene dispersion.

[0010] By adopting the above technical scheme, polyurethane-based fluorine-free waterproofing agent emulsion, acrylic-based fluorine-free waterproofing agent emulsion, and silicone-based fluorine-free waterproofing agent emulsion can all be cross-linked under the action of a blocked isocyanate compound dispersion to form a water-repellent layer on the surface of the fabric, thereby improving the water-repellent performance and weather resistance of the fabric. High-density polyethylene has good wear resistance, which can enable the finishing liquid to improve the wear resistance of the fabric.

[0011] Preferably, the post-treatment liquid is an antibacterial and wear-resistant finishing liquid with an active ingredient concentration of 0.7-1.5 g / L, and the active ingredient is gallnut polyurethane microcapsules.

[0012] By adopting the above technical solution, the gallnut polyurethane microcapsules are dispersed in the post-treatment liquid, and are attached to the surface of the fabric by spraying or coating. Gallnut is a natural antibacterial substance, and the gallnut polyurethane microcapsules can slowly release gallnut, so that the fabric used outdoors has antibacterial properties.

[0013] Preferably, the preparation method of the gallnut polyurethane microcapsule comprises the following steps: mixing sodium alginate, polyethylene and water, heating and stirring until dissolved, cooling to 30°C, adding polyethylene glycol, stirring and emulsifying for 10-15 minutes to obtain an emulsion, uniformly mixing toluene-2,4-diisocyanate and gallnut essential oil, and dripping them into the emulsion, adding dibutyltin dilaurate, stirring and reacting for 1-1.2 hours, heating to 70°C, adding ethylene glycol aqueous solution to obtain a mixed solution, stirring for 1-1.3 hours, cooling to room temperature, centrifuging, and drying to obtain the gallnut polyurethane microcapsule.

[0014] By adopting the above technical scheme, polyethylene glycol is polymerized with toluene-2,4-diisocyanate, and in the case of ethylene glycol as a chain extender, polyurethane is polymerized to form polyurethane, and the polyurethane is coated with gallnut essential oil by interfacial polymerization to form a core-shell structure, thereby preparing gallnut polyurethane microcapsules.

[0015] Preferably, the mass ratio of sodium alginate to polyethylene is 1:(1.28-1.36), and the total concentration of sodium alginate and polyethylene in the mixed solution is 0.170-0.185wt%.

[0016] By adopting the above technical scheme, sodium alginate and polyethylene are used as dispersants to emulsify the mixture of gallnut essential oil and dibutyltin dilaurate, thereby affecting the particle size and dispersibility of gallnut polyurethane microcapsules.

[0017] Preferably, the concentration of dibutyltin dilaurate in the mixed solution is 0.12-0.18 wt %.

[0018] By adopting the above technical solution, dibutyltin dilaurate is used as a catalyst to accelerate the polymerization of polyethylene glycol and toluene-2,4-diisocyanate. Controlling the dosage of dibutyltin dilaurate can effectively control the polymerization reaction rate, thereby affecting the particle size of the gallnut polyurethane microcapsules.

[0019] Preferably, the gallnut polyurethane microcapsules are treated as follows: dopamine hydrochloride is dissolved in tris(hydroxymethylaminomethane)-hydrochloric acid buffer, the gallnut polyurethane microcapsules are added, ultrasonically dispersed for 10-15 minutes, copper sulfate and hydrogen peroxide are added, reacted for 60 minutes, centrifuged and freeze-dried.

[0020] By adopting the above technical solution, dopamine has good viscosity and self-polymerization effect, and can self-polymerize and deposit on the surface of the gallnut polyurethane microcapsule, thereby enhancing the adhesion of the gallnut polyurethane microcapsule, thereby increasing the deposition and adhesion amount of the gallnut polyurethane microcapsule on the fabric.

[0021] Preferably, the mass ratio of dopamine hydrochloride to the gallnut polyurethane microcapsule is 1:(1.68-2.01), and the concentration of dopamine hydrochloride is 1.8-2.2 g / L.

[0022] By adopting the above technical solution, the mass ratio of dopamine hydrochloride to the gallnut polyurethane microcapsule directly affects the self-polymerization of dopamine on the surface of the gallnut polyurethane microcapsule, thereby affecting the adhesion of the treated gallnut polyurethane microcapsule.

[0023] In summary, this application has the following beneficial effects: 1. Since the present application adopts fluorine-free waterproofing agent and cross-linking agent, after the fabric is sprayed and impregnated with the finishing liquid, the finishing liquid fully enters the interior of the fabric, making the fabric water-repellent and having good wear resistance. The finishing liquid is a fluorine-free waterproofing agent, which can reduce the total fluorine content of the fabric after finishing. By squeezing the liquid, the liquid carrying rate of the fabric is reduced, thereby reducing the heat consumed in the subsequent drying of the fabric, controlling the baking time and temperature, so that the finishing effect of the finishing liquid on the fabric is optimal, and the fabric can be kept dry.

[0024] 2. In the present application, the post-treatment liquid is preferably used for antibacterial treatment. The gallnut polyurethane microcapsules are dispersed in the post-treatment liquid. The gallnut polyurethane microcapsules are attached to the surface of the fabric by spraying or coating. Gallnut is a natural antibacterial substance. The gallnut polyurethane microcapsules can slowly release gallnut, so that the fabric used outdoors has antibacterial properties. DETAILED DESCRIPTION

[0025] The present application is further described in detail below in conjunction with embodiments.

[0026] Preparation Examples 1-14 of Gallnut Polyurethane Microcapsules Preparation Example 1 The preparation method of gallnut polyurethane microcapsules comprises the following steps: mixing sodium alginate, 1g polyethylene and 200mL water, heating and stirring until dissolved, cooling to 30°C, adding 3.05g polyethylene glycol, stirring and emulsifying for 10min to obtain an emulsion, uniformly mixing toluene-2,4-diisocyanate and gallnut essential oil, dripping into the emulsion, stirring while dripping, adding dibutyltin dilaurate, stirring and reacting for 1h, heating to 70°C, adding ethylene glycol aqueous solution to obtain a microcapsule. A mixed solution was obtained, stirred for 1 hour, cooled to room temperature, centrifuged and dried to obtain gallnut polyurethane microcapsules; the mass ratio of sodium alginate to polyethylene was 1:1.28, the total concentration of sodium alginate and polyethylene in the mixed solution was 0.170wt%, the concentration of dibutyltin dilaurate in the mixed solution was 0.12wt%, the mass ratio of polyethylene glycol to toluene-2,4-diisocyanate was 1:3, and the mass ratio of gallnut essential oil to toluene-2,4-diisocyanate was 8:3.

[0027] Preparation Example 2 The preparation method of gallnut polyurethane microcapsules comprises the following steps: mixing sodium alginate, 1g polyethylene and 200mL water, heating and stirring until dissolved, cooling to 30°C, adding 3.05g polyethylene glycol, stirring and emulsifying for 15min to obtain an emulsion, uniformly mixing toluene-2,4-diisocyanate and gallnut essential oil, dripping into the emulsion, stirring while dripping, adding dibutyltin dilaurate, stirring and reacting for 1.2h, heating to 70°C, adding ethylene glycol aqueous solution, and preparing A mixed solution was obtained, stirred for 1.3 hours, cooled to room temperature, centrifuged and dried to obtain gallnut polyurethane microcapsules; the mass ratio of sodium alginate to polyethylene was 1:1.36, the total concentration of sodium alginate and polyethylene in the mixed solution was 0.185wt%, the concentration of dibutyltin dilaurate in the mixed solution was 0.18wt%, the mass ratio of polyethylene glycol to toluene-2,4-diisocyanate was 1:3, and the mass ratio of gallnut essential oil to toluene-2,4-diisocyanate was 8:3.

[0028] Preparation Example 3 The difference between Preparation Example 3 and Preparation Example 1 is that the mass ratio of sodium alginate to polyethylene is 1:0.8.

[0029] Preparation Example 4 The difference between Preparation Example 4 and Preparation Example 1 is that the mass ratio of sodium alginate to polyethylene is 1:1.8.

[0030] Preparation Example 5 The difference between Preparation Example 5 and Preparation Example 1 is that the total concentration of sodium alginate and polyethylene in the mixed solution is 0.1 wt %.

[0031] Preparation Example 6 The difference between Preparation Example 6 and Preparation Example 1 is that the total concentration of sodium alginate and polyethylene in the mixed solution is 0.25 wt %.

[0032] Preparation Example 7 The difference between Preparation Example 7 and Preparation Example 1 is that the concentration of dibutyltin dilaurate in the mixed solution is 0.08 wt %.

[0033] Preparation Example 8 The difference between Preparation Example 8 and Preparation Example 1 is that the concentration of dibutyltin dilaurate in the mixed solution is 0.25 wt %.

[0034] Preparation Example 9 The difference between Preparation Example 9 and Preparation Example 1 is that the gallnut polyurethane microcapsules are also treated as follows: dopamine hydrochloride is dissolved in tris(hydroxymethylaminomethane)-hydrochloric acid buffer, the pH of the buffer is 8.5, the concentration of dopamine hydrochloride is 1.8 g / L, gallnut polyurethane microcapsules are added, the mass ratio of dopamine hydrochloride to gallnut polyurethane microcapsules is 1:1.68, ultrasonic dispersion is performed for 10 minutes, copper sulfate and hydrogen peroxide are added, the concentration of copper sulfate is 5 mmol / L, the concentration of hydrogen peroxide is 10 mmol / L, the reaction is continued for 60 minutes, centrifugation and freeze-drying are performed.

[0035] Preparation Example 10 The difference between Preparation Example 10 and Preparation Example 1 is that the gallnut polyurethane microcapsules are further treated as follows: dopamine hydrochloride is dissolved in tris(hydroxymethylaminomethane)-hydrochloric acid buffer, the pH of the buffer is 8.5, the concentration of dopamine hydrochloride is 2.2 g / L, gallnut polyurethane microcapsules are added, the mass ratio of dopamine hydrochloride to gallnut polyurethane microcapsules is 1:2.01, ultrasonic dispersion is performed for 15 minutes, copper sulfate and hydrogen peroxide are added, the concentration of copper sulfate is 5 mmol / L, the concentration of hydrogen peroxide is 10 mmol / L, the reaction is continued for 60 minutes, centrifugation and freeze-drying are performed.

[0036] Preparation Example 11 The difference between Preparation Example 11 and Preparation Example 9 is that the mass ratio of dopamine hydrochloride to the gallnut polyurethane microcapsule is 1:1.2.

[0037] Preparation Example 12 The difference between Preparation Example 12 and Preparation Example 9 is that the mass ratio of dopamine hydrochloride to the gallnut polyurethane microcapsule is 1:2.5.

[0038] Preparation Example 13 The difference between Preparation Example 13 and Preparation Example 9 is that the concentration of dopamine hydrochloride is 0.5 g / L.

[0039] Preparation Example 14 The difference between Preparation Example 14 and Preparation Example 9 is that the concentration of dopamine hydrochloride is 2.8 g / L. Example

[0040] Example 1 A fluorine-free processing technology for outdoor home fabrics, characterized by comprising the following steps: (1) Dipping and vacuum suction: A continuous finishing process is adopted. The fabric is evenly impregnated with the finishing liquid through a spray and an impregnation tank, and then treated with a roller, so that the fabric has a liquid carrying rate of 57%. After vacuum suction, the fabric has a liquid carrying rate of 23%. The finishing liquid includes 40g / L fluorine-free waterproofing agent, 5g / L cross-linking agent, 5g / L wear resistance enhancer and pH value adjuster. The pH value of the finishing liquid is 5. The fluorine-free waterproofing agent is a polyurethane fluorine-free waterproofing agent emulsion, which is X-702MA from Shanghai Fuke. The cross-linking agent is a blocked isocyanate compound dispersion, which is Huntsman's EXTENDER UAN, wear-resistant enhancer uses high-density polyethylene dispersion, and uses AP-35 from Glen Raven USA.

[0041] (2) Pre-drying: The impregnated fabric is sent to a drying oven for treatment, so that the fabric liquid content is 15%; (3) Post-treatment: applying a post-treatment liquid onto the fabric by spraying or coating, wherein the post-treatment liquid is an antibacterial and wear-resistant finishing liquid having an active ingredient concentration of 0.7 g / L, the mass ratio of the fabric to the post-treatment liquid is 1:15, the active ingredient is gallnut polyurethane microcapsules, and the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 1; (4) Baking: Place the fabric in an oven at 170°C, the surface temperature at 170°C, and the baking time for 20 seconds.

[0042] Example 2 A fluorine-free processing technology for outdoor home fabrics, characterized by comprising the following steps: (1) Dipping and vacuum suction: A continuous finishing process is adopted. The fabric is evenly impregnated with the finishing liquid through a spray and an impregnation tank, and then treated with a roller, so that the fabric has a liquid carrying rate of 63%. After vacuum suction, the fabric has a liquid carrying rate of 27%. The finishing liquid includes 100 g / L fluorine-free waterproofing agent, 20 g / L cross-linking agent, 10 g / L wear-resistant enhancer and pH value adjuster. The pH value of the finishing liquid is 6. The fluorine-free waterproofing agent is an acrylic fluorine-free waterproofing agent emulsion, which is UNIYNE XF-5005 of Daikin Company. The cross-linking agent is a blocked isocyanate compound dispersion, which is Huntsman Company. EXTENDER UAN, wear-resistant enhancer uses high-density polyethylene dispersion, and uses AP-35 from Glen Raven USA.

[0043] (2) Pre-drying: The impregnated fabric is sent to a drying oven for treatment, so that the fabric liquid content is 20%; (3) Post-treatment: applying a post-treatment liquid onto the fabric by spraying or coating, wherein the post-treatment liquid is an antibacterial and wear-resistant finishing liquid having an active ingredient concentration of 1.5 g / L, the mass ratio of the fabric to the post-treatment liquid is 1:15, the active ingredient is gallnut polyurethane microcapsules, and the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 2; (4) Baking: Place the fabric in an oven at 180°C, the surface temperature at 173°C, and the baking time for 10 seconds.

[0044] Example 3 A fluorine-free processing technology for outdoor home fabrics, characterized by comprising the following steps: (1) Dipping and vacuum suction: A continuous finishing process is adopted. The fabric is evenly impregnated with the finishing liquid through a spray and an impregnation tank, and then treated with a roller to make the fabric liquid-carrying rate 60%. After vacuum suction, the fabric liquid-carrying rate is 25%. The finishing liquid includes 80g / L fluorine-free waterproofing agent, 10g / L cross-linking agent, 8g / L wear-resistance improving agent and pH value adjusting agent. The pH value of the finishing liquid is 5. The fluorine-free waterproofing agent is a silicone-based fluorine-free waterproofing agent emulsion, Dowsil IE-8749 from Dow Chemical Company, and the cross-linking agent is a blocked isocyanate compound dispersion, selected from Huntsman Company. EXTENDER UAN, wear-resistant enhancer uses high-density polyethylene dispersion, and uses AP-35 from Glen Raven USA.

[0045] (2) Pre-drying: The impregnated fabric is sent to a drying oven for treatment, so that the fabric liquid content is 17%; (3) Post-treatment: applying a post-treatment liquid onto the fabric by spraying or coating, wherein the post-treatment liquid is an antibacterial and wear-resistant finishing liquid having an active ingredient concentration of 1.5 g / L, the mass ratio of the fabric to the post-treatment liquid is 1:15, the active ingredient is gallnut polyurethane microcapsules, and the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 2; (4) Baking: Place the fabric in an oven at 180°C, the surface temperature at 173°C, and the baking time for 10 seconds.

[0046] Example 4 The difference between Example 4 and Example 1 is that the finishing liquid includes 80 g / L fluorine-free waterproofing agent, 10 g / L cross-linking agent, 5 g / L wear resistance improving agent and pH adjuster, and the pH of the finishing liquid is 5.

[0047] Example 5 The difference between Example 5 and Example 1 is that the finishing liquid includes 90 g / L fluorine-free waterproofing agent, 15 g / L cross-linking agent, 10 g / L wear resistance improving agent and pH adjuster, and the pH of the finishing liquid is 6.

[0048] Example 6 The difference between Example 6 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 3.

[0049] Example 7 The difference between Example 7 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 4.

[0050] Example 8 The difference between Example 8 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 5.

[0051] Example 9 The difference between Example 9 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 6.

[0052] Example 10 The difference between Example 10 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 7.

[0053] Embodiment 11 The difference between Example 11 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 8.

[0054] Example 12 The difference between Example 12 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 9.

[0055] Example 13 The difference between Example 13 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 10.

[0056] Embodiment 14 The difference between Example 14 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 11.

[0057] Embodiment 15 The difference between Example 15 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 12.

[0058] Example 16 The difference between Example 16 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 13.

[0059] Embodiment 17 The difference between Example 17 and Example 1 is that the gallnut polyurethane microcapsules are the gallnut polyurethane microcapsules prepared in Preparation Example 14.

[0060] Embodiment 18 The difference between Example 18 and Example 1 is that the finishing liquid includes 35 g / L fluorine-free waterproofing agent, 25 g / L cross-linking agent, 15 g / L wear resistance improving agent and pH adjuster, and the pH of the finishing liquid is 5.

[0061] Embodiment 19 The difference between Example 19 and Example 1 is that the finishing liquid includes 120 g / L fluorine-free waterproofing agent, 3 g / L cross-linking agent, 2 g / L wear resistance improving agent and pH adjuster, and the pH of the finishing liquid is 5.

[0062] Embodiment 20 The difference between Example 20 and Example 1 is that the pH of the finishing liquid is 4.

[0063] Embodiment 21 The difference between Example 21 and Example 1 is that the pH of the finishing liquid is 8.

[0064] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the fabric is not post-treated.

[0065] Detection Methods 1. According to the preparation process of Examples 1-5 and Examples 18-21, the acrylic fabric was finished, and the finished fabric was tested for water repellency, and the results were recorded in Table 1. The water repellency test was rated according to the "Test Method for Surface Moisture Resistance of Textile Fabrics-Water Test Method" GB / T4745-2012, and the rating standard was: Level 5-the upper surface of the sample was not wet or stained; Level 4-the upper surface of the sample was slightly, randomly wet or stained; Level 3-the upper surface of the sample was wet at the spray point; Level 2-the entire upper surface of the sample was partially wet; Level 1-the entire upper surface of the sample was completely wet; Level 0-the entire upper surface and lower surface of the sample were completely wet.

[0066] Table 1 Water repellency of the finished fabric According to Table 1 and Examples 1-2, it can be seen that the fabric of Example 1-2 has good water repellency after finishing, indicating that the use of the finishing liquid and the corresponding process of Example 1-2 can give the fabric good water repellency. The finishing liquid used in Example 1-2 contains a fluorine-free waterproofing agent, a cross-linking agent, and a wear resistance enhancing agent, and the pH of the finishing liquid is adjusted to between 5 and 6 using a pH adjuster, so that the finishing liquid can form a water repellent layer on the surface of the fabric during the fabric immersion period, so that the fabric has good water repellency after being soaked, dried and baked, and the total fluorine content of the fabric is less than 50ppm, which greatly reduces the total fluorine content in the fabric, and the water repellency and wear resistance are relatively good, meeting the product requirements.

[0067] The polyurethane fluorine-free waterproofing agent emulsion, acrylic fluorine-free waterproofing agent emulsion, and silicone fluorine-free waterproofing agent emulsion used in Examples 1-2 can all be cross-linked under the action of the blocked isocyanate compound dispersion to form a water-repellent layer on the surface of the fabric, thereby improving the water-repellent and weather resistance of the fabric. High-density polyethylene can improve the wear resistance of the fabric and has a good improvement effect on the wear resistance, weather resistance, water-repellent and other properties of the fabric.

[0068] Compared with Example 1, the fabric after finishing in Example 4-5 has better water-repellent properties, which shows that the composition and content of the finishing liquid selected in Example 4-5 have better synergistic effect than that in Example 1. After the fabric is impregnated, the water-repellent layer formed by the finishing liquid components on the surface of the fabric has better water-repellent effect and can effectively reduce the situation of fabric getting wet. Among them, the composition and content of the finishing liquid selected in Example 3 have the best water-repellent effect of the water-repellent layer formed by the finishing liquid components on the surface of the fabric. The prepared fabric still shows good water-repellent properties during the test and after the test time is extended.

[0069] Compared with Example 1, the water repellent performance of the fabric after finishing in Example 18-19 is lower than that in Example 1. In Example 18-19, the components and their contents in the finishing liquid are adjusted, indicating that the content of each component in the finishing liquid affects the treatment effect of the finishing liquid, indicating that there is a synergistic effect between the contents of each component. The fluorine-free waterproofing agent and the cross-linking agent need to have suitable concentrations and mass ratios to form a water-repellent layer with excellent performance, giving the fabric good weather resistance and water washability. A reduction in the content of the fluorine-free waterproofing agent will reduce the water repellent performance of the fabric, and a reduction in the content of high-density polyethylene will reduce the wear resistance of the fabric.

[0070] Compared with Example 1, the water repellency of the fabric after finishing in Example 20-21 is lower than that in Example 1. The pH of the finishing liquid is adjusted in Example 20-21, indicating that the pH of the finishing liquid has an effect on the treatment effect of the finishing liquid. The pH of the finishing liquid affects the reaction between the fluorine-free water repellent and the cross-linking agent in the finishing liquid, thereby affecting the performance of the water repellent layer formed on the surface of the fabric.

[0071] 2. According to the preparation process of Example 1, Examples 6-17 and Comparative Example 1, acrylic fabrics were finished, and the finished fabrics were subjected to antibacterial tests. The tests were conducted in accordance with "GB / T 20944.3-2008 Evaluation of Antibacterial Properties of Textiles Part 3: Oscillation Method", and Staphylococcus aureus was selected as the test strain, and the results were recorded in Table 2 Table 2 Antibacterial properties of the finished fabrics According to Table 2, Example 1 and Comparative Example 1, it can be seen that the antibacterial property of the fabric after finishing in Comparative Example 1 is lower than that in Example 1. The fabric in Comparative Example 1 is not post-treated, which shows that the post-treatment liquid can effectively improve the antibacterial property of the fabric. The gallnut polyurethane microcapsules are dispersed in the post-treatment liquid, and the gallnut polyurethane microcapsules are adhered to the surface of the fabric by spraying or spraying. The gallnut polyurethane microcapsules can slowly release gallnut, so that when the fabric is used for outdoor use, in addition to having water repellency and good weather resistance, it can also have good antibacterial property, further improving the durability of the fabric and reducing the number of times the fabric is washed.

[0072] Compared with Example 1, the antibacterial property of the fabric after finishing in Example 6-9 is lower than that in Example 1. When preparing the gallnut polyurethane microcapsules used in Example 6-7, the mass ratio of sodium alginate to polyethylene is adjusted. When preparing the gallnut polyurethane microcapsules used in Example 8-9, the total addition amount of sodium alginate and polyethylene in the mixed solution is adjusted. Sodium alginate and polyethylene are used as dispersants to improve the emulsification of gallnut essential oil and dibutyltin dilaurate in the mixed solution, so that the mixing of polyethylene glycol, toluene-2,4-diisocyanate and gallnut essential oil is more uniform, which is conducive to the moderate particle size and uniform dispersion of the gallnut polyurethane microcapsules. Sodium alginate and polyethylene have a synergistic effect. Changing the mass ratio and total addition amount of the two is likely to affect their dispersion effect.

[0073] Compared with Example 1, the antibacterial property of the fabric after finishing in Example 10-11 is lower than that in Example 1. When preparing the gallnut polyurethane microcapsules used in Example 10-11, the concentration of dibutyltin dilaurate is adjusted. Dibutyltin dilaurate is used as a catalyst to promote the polymerization reaction of polyethylene glycol and toluene-2,4-diisocyanate. If the addition amount of dibutyltin dilaurate is too high or too low, it is easy to affect the capsule shell of the gallnut polyurethane microcapsule, that is, the formation speed and polymerization degree of the polyurethane, thereby affecting the particle size and capsule shell morphology of the gallnut polyurethane microcapsule, and further affecting the antibacterial property of the fabric.

[0074] Compared with Example 1, the antibacterial property of the fabric after finishing in Example 12-13 is improved compared with that in Example 1. During the preparation of the gallnut polyurethane microcapsules used in Examples 12-13, the surface of the gallnut polyurethane microcapsules was treated with dopamine. Dopamine has good viscosity and self-polymerization effect, and can self-polymerize and deposit on the surface of the gallnut polyurethane microcapsules, thereby enhancing the adhesion of the gallnut polyurethane microcapsules, thereby increasing the deposition and adhesion amount of the gallnut polyurethane microcapsules on the fabric.

[0075] Compared with Example 12, the antibacterial properties of the fabrics treated with Examples 14-17 are lower than that of Example 12. When the gallnut polyurethane microcapsules used in Examples 14-15 are treated with dopamine, the mass ratio of dopamine hydrochloride to the gallnut polyurethane microcapsules is adjusted. When the gallnut polyurethane microcapsules used in Examples 16-17 are treated with dopamine, the concentration of dopamine hydrochloride is adjusted. The amount of dopamine hydrochloride directly affects the degree and amount of polymerization of dopamine on the surface of the gallnut polyurethane microcapsules, thereby affecting the adhesion of the gallnut polyurethane microcapsules.

[0076] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A fluorine-free processing technology for outdoor home fabrics, characterized by: The following steps are involved: (1) Padding and vacuum suction: A continuous finishing process is adopted, the fabric is evenly impregnated with the finishing liquid through a spray and an impregnation tank, and then processed by a pressing roller, so that the fabric has a liquid carrying rate of 57-63%. After vacuum suction, the fabric has a liquid carrying rate of 23-27%; the finishing liquid includes 40-100g / L fluorine-free waterproofing agent, 5-25g / L cross-linking agent, 5-10g / L wear resistance enhancer and pH value adjuster, and the pH value of the finishing liquid is 5-6; (2) Pre-drying: The impregnated fabric is sent into a drying oven for treatment, so that the fabric liquid content is 15-20%; (3) Post-treatment: Apply post-treatment liquid to the fabric by spraying or coating; (4) Baking: Place the fabric in an oven at a temperature of 170-180°C, a surface temperature of 170-173°C, and a baking time of 10-20 seconds.

2. The fluorine-free processing technology for outdoor home fabrics according to claim 1, characterized in that: The finishing liquid comprises 80-90 g / L of fluorine-free waterproofing agent, 10-15 g / L of cross-linking agent, 5-10 g / L of wear resistance improving agent and pH value adjusting agent, and the pH value of the finishing liquid is 5-6.

3. A fluorine-free processing technology for outdoor home fabrics according to claim 1 or 2, characterized in that: The fluorine-free waterproofing agent is selected from one of polyurethane fluorine-free waterproofing agent emulsion, acrylic fluorine-free waterproofing agent emulsion, and silicone fluorine-free waterproofing agent emulsion, the cross-linking agent is selected from blocked isocyanate compound dispersion, and the wear-resistant enhancer is selected from high-density polyethylene dispersion.

4. The fluorine-free processing technology for outdoor home fabrics according to claim 1, characterized in that: The post-treatment liquid is an antibacterial and wear-resistant finishing liquid with an effective component concentration of 0.7-1.5 g / L, and the effective component is gallnut polyurethane microcapsule.

5. The fluorine-free processing technology for outdoor home fabrics according to claim 4, characterized in that: The preparation method of the gallnut polyurethane microcapsule comprises the following steps: mixing sodium alginate, polyethylene and water, heating and stirring until dissolved, cooling to 30°C, adding polyethylene glycol, stirring and emulsifying for 10-15 minutes to obtain an emulsion, uniformly mixing toluene-2,4-diisocyanate and gallnut essential oil, dripping into the emulsion, adding dibutyltin dilaurate, stirring and reacting for 1-1.2 hours, heating to 70°C, adding ethylene glycol aqueous solution to obtain a mixed solution, stirring for 1-1.3 hours, cooling to room temperature, centrifuging, and drying to obtain the gallnut polyurethane microcapsule.

6. The fluorine-free processing technology for outdoor home fabrics according to claim 5, characterized in that: The mass ratio of sodium alginate to polyethylene is 1:(1.28-1.36), and the total concentration of sodium alginate and polyethylene in the mixed solution is 0.170-0.185wt%.

7. The fluorine-free processing technology for outdoor home fabrics according to claim 5, characterized in that: The concentration of dibutyltin dilaurate in the mixed solution is 0.12-0.18 wt %.

8. The fluorine-free processing technology for outdoor home fabrics according to claim 5, characterized in that: The gallnut polyurethane microcapsules are treated as follows: dopamine hydrochloride is dissolved in tris(hydroxymethylaminomethane)-hydrochloric acid buffer, the gallnut polyurethane microcapsules are added, ultrasonically dispersed for 10-15 minutes, copper sulfate and hydrogen peroxide are added, reacted for 60 minutes, centrifuged and freeze-dried.

9. The fluorine-free processing technology for outdoor home fabrics according to claim 8, characterized in that: The mass ratio of dopamine hydrochloride to gallnut polyurethane microcapsules is 1:(1.68-2.01), and the concentration of dopamine hydrochloride is 1.8-2.2 g / L.