By using carbon fiber cloth, Maya blue concave hybrid pigment, poly1,4 butadiene bimodified water-based polyurethane resin and organosiloxane/polyurethane composite coating on the back panel of the mobile phone, it is formed to be scratch-resistant, wear-resistant and anti-resistant The dirty skin-feeling finishing material solves the problems of easy damage and lack of anti-fouling function in the back panel of traditional mobile phones, and achieves high texture and long life.
Patent Information
- Application Number
- CN202411207742.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
The back panel of traditional mobile phones is easy to damage, has single color, has poor touch and lacks anti-fouling functions, making it difficult to achieve comprehensive performance of scratch resistance, wear resistance, stain resistance, beauty and high-quality.
Carbon fiber cloth is used as the base layer, Maya blue concave hybrid pigment and poly1,4 butadiene-bimodified aqueous polyurethane resin as the surface layer, combined with organosiloxane/polyurethane composite coating as the antifouling layer, through Specific preparation methods form skin-feeling finish materials that are scratch-resistant, wear-resistant and stain-resistant.
It realizes the scratch-resistant, wear-resistant and anti-fouling functions of the back panel of the mobile phone, and also has the advantages of high color fastness, good dimensional stability, excellent thermal conductivity, green and environmentally friendly, which improves service life and aesthetics.
Smart Images

Figure CN119061708A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional polymer materials, relates to the manufacture of electronic product back panels, and particularly relates to a skin-feeling antifouling functional finishing material for a mobile phone back panel and a preparation method thereof. Background Art
[0002] Since the emergence of smart phones, people have been accustomed to putting protective cases on their phones to protect the screen and back cover from damage and to beautify the appearance of the phone, because the plastic or metal back panels are not only very easy to damage, but also have a single color and are not beautiful enough. However, traditional mobile phone cases not only increase the weight and volume of the phone during use, but are also made of plastic or rubber, have a poor touch, and lack anti-fouling and other functions. How to develop new materials to achieve the functions of scratch resistance, wear resistance, anti-fouling, beautification, and excellent texture of the back panel of the mobile phone is a problem that needs to be solved urgently. Summary of the invention
[0003] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a skin-feel antifouling functional finishing material for a mobile phone back panel and a preparation method thereof. The skin-feel antifouling functional finishing material uses carbon fiber cloth as a base material layer, a Mayan blue concave clay hybrid pigment and a poly-1,4-butadiene double-modified water-based polyurethane resin as a surface layer, and an organic silicone / polyurethane composite coating as a skin-feel antifouling layer. The finishing material has multiple functions such as scratch resistance, wear resistance, and antifouling. The finishing material prepared by the present invention has the advantages of high color fastness, good dimensional stability, excellent thermal conductivity, and green environmental protection, and has broad market prospects.
[0004] The present invention is achieved through the following technical solutions: A method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel comprises the following steps: Step 1: Add nano kaolin, color paste, defoamer and leveling agent to the Maya blue-like attapulgite hybrid pigment and poly-1,4-butadiene dual-modified waterborne polyurethane resin, and stir evenly to obtain a slurry for a waterborne polyurethane surface layer; Step 2: applying the slurry obtained in step 1 to the surface of the carbon fiber base cloth through a two-roll calender, and drying to form a waterborne polyurethane surface layer; Step three, coating the surface of the waterborne polyurethane surface layer obtained in step two with an organic siloxane / polyurethane composite coating, and drying the coating to obtain the skin-feeling antifouling functional finishing material for the mobile phone back panel.
[0005] A further improvement of the present invention is: The preparation steps of the Maya blue-like attapulgite hybrid pigment and the poly-1,4-butadiene dual-modified waterborne polyurethane resin are as follows: (1) Preparation of a double-modified hydrophilic polyurethane prepolymer: isophorone diisocyanate, hexamethylene diisocyanate and polytetramethylene glycol are mixed and heated at 80-90°C for 1-2 hours with stirring, and then an ethanolamine-type hydrophilic chain extender and a Maya blue attapulgite hybrid pigment are added, and the reaction is continued with stirring for chain extension reaction, and then an organic bismuth catalyst, acetone and terminal hydroxyl poly-1,4-butadiene are added, and the reaction is continued with stirring, and then a diisopropanolamine crosslinker is added, and the reaction is continued with stirring, and then a small molecule acid neutralizer is used for neutralization reaction at 40-60°C for 20-30 minutes; finally, water is added and stirred at high speed for self-emulsification and dispersion to obtain a Maya blue attapulgite hybrid pigment and poly-1,4-butadiene double-modified waterborne polyurethane dispersion; (2) Secondary chain extension: Add a small molecule diamine chain extender to the dispersion obtained in step (1), raise the temperature to 40-50°C, and perform a chain extension reaction for 3-5 hours; (3) Deacetone removal: After the system of step (2) becomes a translucent uniform liquid, deacetone is removed at low pressure at 40-60° C. to obtain a Maya blue-like attapulgite hybrid pigment and a poly-1,4-butadiene dual-modified waterborne polyurethane resin.
[0006] Further, the ethanolamine hydrophilic chain extender is selected from one or a combination of N-methyldiethanolamine, N-ethyldiethanolamine, N-propyldiethanolamine, and N-butyldiethanolamine; And / or, the organic bismuth catalyst is selected from bismuth laurate and bismuth isooctanoate; and / or, the small molecule acid neutralizer is selected from one of hydrochloric acid, acetic acid or sulfonic acid; And / or, the small molecule diamine chain extender is selected from one of ethylenediamine and isophoronediamine; Furthermore, the mass ratio of isophorone diisocyanate, hexamethylene diisocyanate, polytetramethylene ether diol, ethanolamine hydrophilic chain extender, Maya blue attapulgite hybrid pigment, organic bismuth catalyst, acetone, hydroxyl-terminated poly 1,4-butadiene, diisopropanolamine crosslinker, small molecule acid neutralizer, and small molecule diamine chain extender is 10-15:10-20:15-30:3-12:1-7:0-1:10-20:3-10:0-1:2-8:3-10.
[0007] Furthermore, in step (1), the temperature of the heating and stirring reaction is 80-90°C and the time is 1-2 hours; the temperature of the neutralization reaction is 40-60°C and the time is 20-30 minutes; in step (2), the temperature of the temperature-raising chain extension is 40-50°C and the time is 3-5 hours; and the temperature of the deacetone in step (3) is 40-60°C.
[0008] Furthermore, the preparation steps of the Maya blue-like attapulgite hybrid pigment are as follows: Take an organic pigment and attapulgite and mix them evenly. Put them in an oven for drying. Take them out and cool them to room temperature, then disperse them in water, add isopropanol, tetraethyl orthosilicate, methacryloxypropyl triethoxysilane and hydrochloric acid, react at 70-90 °C for 20-30h, filter them after cooling to room temperature, wash them with isopropanol, and freeze-dry them at -30--10 °C to obtain an acryloxy-modified Maya blue hybrid pigment; wherein the mass ratio of the organic pigment, attapulgite, tetraethyl orthosilicate and methacryloxypropyl triethoxysilane is 1:10:0.2:1.
[0009] Furthermore, the preparation steps of the organosiloxane / polyurethane composite coating are as follows: At room temperature, a certain proportion of methacryloxypropyl tris(trimethylsiloxane)silane, vinyl-terminated polydimethylsiloxane and polybutadiene rubber modified polyurethane prepolymer are mixed, stirred and mixed evenly, and then azobisisoheptanenitrile is added, stirred and dissolved to obtain an organic siloxane / polyurethane composite coating; wherein the mass ratio of the methacryloxypropyl tris(trimethylsiloxane)silane, vinyl-terminated polydimethylsiloxane, polybutadiene rubber modified polyurethane prepolymer and azobisisoheptanenitrile is 5-10:15-30:55-70:2-6.
[0010] Furthermore, the substrate layer (1) is carbon fiber cloth.
[0011] Furthermore, the drying temperature in step 2 is 110-130° C.; the drying temperature in step 3 is 90-110° C., and the time is 4-8 min.
[0012] A further improvement of the present invention is: The skin-feel antifouling functional finishing material for a mobile phone back panel prepared by the above method comprises a substrate layer (1), a waterborne polyurethane surface layer (2), and an organic silicon skin-feel antifouling layer (3) which are arranged in sequence from bottom to top, wherein the waterborne polyurethane surface layer (2) is an aqueous polyurethane resin double-modified with a Maya blue-like concave clay hybrid pigment and poly-1,4-butadiene, and the organic silicon skin-feel antifouling layer (3) is an organic siloxane / polyurethane composite coating.
[0013] Compared with the prior art, the specific beneficial effects of the present invention are as follows: 1. The skin-feel antifouling functional finishing material for the back panel of a mobile phone prepared by the present invention uses a hydrophilic carbon fiber cloth as a base material layer. Firstly, the toughness and strength of the carbon fiber cloth can be used to effectively prevent the shrinkage and deformation of the mixed material layer caused by the different thermal expansion coefficients of the materials due to the temperature difference in the use environment, thereby providing good dimensional stability for the finishing material; secondly, the carbon fiber material is light in weight and is thermally and electrically conductive, thereby providing the finishing layer with certain thermal conductivity and antistatic properties; finally, the large specific surface area and roughness provided by the porosity of the carbon fiber cloth can be used to improve the bonding strength between the finishing layer and the substrate of the back panel of the mobile phone.
[0014] 2. The skin-feel antifouling functional finishing material for the mobile phone back panel prepared by the present invention has a surface layer of a Mayan blue attapulgite hybrid pigment printed with textures or patterns and a poly-1,4-butadiene double-modified waterborne polyurethane resin layer. On the one hand, the modification of the Mayan blue attapulgite hybrid pigment makes the finishing material have excellent weather resistance and beautiful colors, providing good aesthetics; on the other hand, the modification of poly-1,4-butadiene provides the finishing material with a skin-like elastic touch, effectively supporting the skin-like touch of the finishing material. At the same time, the residual double bonds in poly-1,4-butadiene can be cross-linked with the double bonds in the antifouling layer, thereby improving the bonding strength between the finishing layer and the antifouling layer.
[0015] 3. The skin-feel antifouling functional finishing material for the back panel of a mobile phone prepared by the present invention uses an organic siloxane / polyurethane composite coating as a skin-feel antifouling layer. Firstly, after the polymerization of methacryloxypropyl tri(trimethylsiloxy)silane and vinyl-terminated polydimethylsiloxane under the action of an initiator, the finishing material is provided with excellent antifouling and scratch-resistant functions; secondly, the polyurethane prepolymer modified with polybutadiene rubber balances the hardness and touch of the antifouling layer, and improves its skin-feel touch; finally, all the raw materials contain double bonds, which can be copolymerized with the double bonds in the polyurethane surface layer under the action of a free radical initiator, thereby improving the bonding strength between the finishing layer and the antifouling layer, and contributing to improving the overall toughness and strength of the finishing material, thereby increasing its service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a schematic structural diagram of the skin-feel antifouling functional finishing material for the mobile phone back panel prepared by the present invention; Among them, (1) is the base material layer; (2) is the water-based polyurethane surface layer; (3) is the silicone skin-feel anti-fouling layer DETAILED DESCRIPTION
[0017] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods. Example 1
[0018] The present embodiment provides a skin-feel antifouling functional finishing material for a mobile phone back panel, which comprises a substrate layer (1), a water-based polyurethane surface layer (2), and an organosilicon skin-feel antifouling layer (3) arranged in sequence from bottom to top; wherein the water-based polyurethane surface layer is a water-based polyurethane resin double-modified with a Maya blue-like concave clay hybrid pigment and poly-1,4-butadiene, and the organosilicon skin-feel antifouling layer is an organosiloxane / polyurethane composite coating.
[0019] This embodiment also provides a method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel, and the specific steps are as follows: Step 1: Add nano-kaolin, color paste, defoamer, and leveling agent to the Maya blue-like attapulgite hybrid pigment and poly-1,4-butadiene double-modified waterborne polyurethane resin, and stir evenly to obtain a slurry for the waterborne polyurethane surface layer; Step 2: applying the slurry obtained in step 1 to the surface of the carbon fiber base fabric through a two-roll calender and drying it in an oven at 120°C to form a waterborne polyurethane surface layer; Step three: coating the surface of the waterborne polyurethane surface layer obtained in step two with an organic siloxane / polyurethane composite coating, and baking in an oven at 100° C. for 5 minutes to obtain the skin-feel antifouling functional finishing material for the mobile phone back panel.
[0020] It should be noted that the specific preparation method of the above-mentioned Maya blue attapulgite hybrid pigment is: Take 2g of organic pigment and mix it with 20g of attapulgite. After mixing thoroughly, put it in an oven at 130°C for 48 hours. After cooling to room temperature, disperse it in 200ml of water, add 100ml of isopropanol, 0.4g of tetraethyl orthosilicate, 2g of methacryloyloxypropyltriethoxysilane and 0.4ml of hydrochloric acid, react at 80°C for 24h, cool to room temperature, filter, wash with isopropanol, and freeze-dry at -20°C to obtain an acryloyloxy-modified Maya blue hybrid pigment.
[0021] The specific preparation method of the above-mentioned Maya blue-like attapulgite hybrid pigment and poly-1,4-butadiene dual-modified waterborne polyurethane resin is as follows: 12 g of isophorone diisocyanate, 15 g of hexamethylene diisocyanate and 23 g of polytetramethylene ether glycol were stirred and reacted at 85° C. for 1.5 hours, 6 g of 2,2'-dihydroxydiethylamine and 4 g of Maya blue attapulgite hybrid pigment were added, and the reaction was continued for 1 hour. Then, 0.5 g of organic bismuth catalyst, 14 g of acetone and 4 g of hydroxy-terminated poly 1,4-butadiene were added, and the reaction was continued for 1.5 hours. Then, 0.6 g of diisopropanolamine crosslinking agent was added, and the reaction was continued for 1 hour. Then, 3 g of small molecule acid neutralizer was used for neutralization reaction at 50° C. for 20-30 minutes. Finally, 100 g of water was added and stirred at high speed for self-emulsification dispersion to obtain Maya blue attapulgite hybrid pigment and poly 1,4-butadiene double-modified waterborne polyurethane dispersion. (2) Secondary chain expansion: 5 g of a small molecule diamine chain extender was added to the Maya blue attapulgite hybrid pigment modified aqueous polyurethane dispersion, and then the temperature was raised to 45°C for chain extension for 4 hours; (3) Deacetone removal: After the system becomes a translucent uniform liquid, acetone is removed at 50° C. under low pressure to obtain a Maya blue attapulgite hybrid pigment and a poly-1,4-butadiene dual-modified waterborne polyurethane resin.
[0022] The specific preparation method of the above-mentioned organosiloxane / polyurethane composite coating is as follows: At room temperature, 5 g of methacryloxypropyl tris(trimethylsiloxy)silane, 30 g of vinyl-terminated polydimethylsiloxane and 62 g of polybutadiene rubber-modified polyurethane prepolymer were mixed and stirred until uniformly mixed, and then 3 g of azobisisoheptanenitrile was added and stirred to dissolve to obtain an organosiloxane / polyurethane composite coating. Example 2
[0023] This embodiment is substantially the same as the embodiment 1, except that the waterborne polyurethane surface layer (2) in this embodiment uses a different formula of a Maya blue attapulgite-like hybrid pigment and a poly-1,4-butadiene-modified waterborne polyurethane resin. Specifically, 12 g of isophorone diisocyanate, 15 g of hexamethylene diisocyanate and 20 g of polytetramethylene ether glycol are stirred and reacted at 85° C. for 1.5 hours, 6 g of 2,2'-dihydroxydiethylamine and 4 g of Maya blue attapulgite-like hybrid pigment are added, and the stirring reaction is continued for 1 hour, 0.5 g of an organic bismuth catalyst, 14 g of acetone and 9 g of hydroxy-terminated poly-1,4-butadiene are added, and the stirring reaction is continued for 1.5 hours, and then 0.6 g of a diisopropanolamine crosslinking agent is added, and the stirring reaction is continued for 1 hour, and then 3 g of the diisopropanolamine crosslinking agent is added at 50° C. g small molecule acid neutralizer for neutralization reaction for 20-30 minutes; finally, 100 g water is added for high-speed stirring for self-emulsification and dispersion to obtain a Maya blue attapulgite hybrid pigment and poly-1,4-butadiene dual-modified waterborne polyurethane dispersion; (2) Secondary chain expansion: 5 g of a small molecule diamine chain extender was added to the Maya blue attapulgite hybrid pigment modified aqueous polyurethane dispersion, and then the temperature was raised to 45°C for chain extension for 4 hours; (3) Deacetone removal: After the system becomes a translucent uniform liquid, acetone is removed at 50° C. under low pressure to obtain a Maya blue attapulgite hybrid pigment and a poly-1,4-butadiene dual-modified waterborne polyurethane resin.
[0024] Apart from this, this embodiment is exactly the same as Embodiment 1 and will not be described in detail here. Example 3
[0025] This embodiment is substantially the same as the embodiment 1, except that the formula of the organosilicone skin-feel antifouling layer (3) used in this embodiment is different. Specifically, 10 g of methacryloxypropyl tris(trimethylsiloxy)silane, 26 g of vinyl-terminated polydimethylsiloxane and 60 g of polybutadiene rubber-modified polyurethane prepolymer are mixed at room temperature, stirred and mixed evenly, and then 4 g of azobisisoheptonitrile is added and stirred to dissolve to obtain the organosilicone / polyurethane composite coating.
[0026] Apart from this, this embodiment is exactly the same as Embodiment 1 and will not be described in detail here.
[0027] The skin-feel antifouling functional finishing material for the mobile phone back panel prepared by the above embodiments 1 to 3 has a soft, plump and elastic surface, has a certain hydrophobicity, and has good antifouling and wear resistance. The method for testing the hydrophobicity, antifouling and wear resistance of the prepared skin-feel antifouling functional finishing material for the mobile phone back panel is as follows: Hydrophobicity: The hydrophobicity of the skin-feel antifouling functional finishing material for the back panel of the mobile phone is measured by the water contact angle. A volume of 5.0 μL of deionized water is dropped on the surface of the material and measured using a JC2000C2 contact angle meter. The contact angle is measured at different positions of the finishing material using the angle measurement method and the average value is taken.
[0028] Stain resistance: Refer to JG / T304-2011 to test the stain resistance of the surface of the finishing material with skin-feel anti-fouling function; use a marker pen to draw a circle on the surface of the finishing material, and then erase it with a lint-free cotton cloth. This is a cycle test (counted as one time) to test its stain resistance against marker pen writing until the oily marker pen writing cannot be wiped clean.
[0029] Wear resistance: The prepared mobile phone back panel skin-feel antifouling functional finishing material was tested on a TABER friction tester using an H22 grinding wheel to test the number of circles at which the material surface began to wear.
[0030] The skin-feel antifouling functional finishing materials for mobile phone back panels prepared in Examples 1 to 3 were tested for water contact angle, stain resistance and abrasion resistance. The results are shown in the following table:
[0031] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel, characterized in that: The following steps are involved: Step 1: Add nano kaolin, color paste, defoamer and leveling agent to the Maya blue-like attapulgite hybrid pigment and poly-1,4-butadiene dual-modified waterborne polyurethane resin, and stir evenly to obtain a slurry for a waterborne polyurethane surface layer; Step 2: applying the slurry obtained in step 1 to the surface of the carbon fiber base cloth through a two-roll calender, and drying to form a waterborne polyurethane surface layer; Step three, coating the surface of the waterborne polyurethane surface layer obtained in step two with an organic siloxane / polyurethane composite coating, and drying the coating to obtain the skin-feeling antifouling functional finishing material for the mobile phone back panel.
2. The method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel according to claim 1, characterized in that: The preparation steps of the Maya blue-like attapulgite hybrid pigment and the poly-1,4-butadiene dual-modified waterborne polyurethane resin are as follows: (1) Preparation of a double-modified hydrophilic polyurethane prepolymer: isophorone diisocyanate, hexamethylene diisocyanate and polytetramethylene glycol are mixed and heated at 80-90°C for 1-2 hours with stirring, and then an ethanolamine-type hydrophilic chain extender and a Maya blue attapulgite hybrid pigment are added, and the reaction is continued with stirring for chain extension reaction, and then an organic bismuth catalyst, acetone and terminal hydroxyl poly-1,4-butadiene are added, and the reaction is continued with stirring, and then a diisopropanolamine cross-linking agent is added, and the reaction is continued with stirring, and then a small molecule acid neutralizer is used for neutralization reaction at 40-60°C for 20-30 minutes; finally, water is added and stirred at high speed for self-emulsification and dispersion to obtain a Maya blue attapulgite hybrid pigment and poly-1,4-butadiene double-modified waterborne polyurethane dispersion; (2) Secondary chain extension: Add a small molecule diamine chain extender to the dispersion obtained in step (1), raise the temperature to 40-50°C, and perform a chain extension reaction for 3-5 hours; (3) Deacetone removal: After the system of step (2) becomes a translucent uniform liquid, deacetone is removed at low pressure at 40-60° C. to obtain a Maya blue-like attapulgite hybrid pigment and a poly-1,4-butadiene dual-modified waterborne polyurethane resin.
3. The method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel according to claim 2, characterized in that: The ethanolamine hydrophilic chain extender is selected from one or a combination of N-methyldiethanolamine, N-ethyldiethanolamine, N-propyldiethanolamine, and N-butyldiethanolamine; And / or, the organic bismuth catalyst is selected from bismuth laurate and bismuth isooctanoate; and / or, the small molecule acid neutralizer is selected from one of hydrochloric acid, acetic acid or sulfonic acid; And / or, the small molecule diamine chain extender is selected from one of ethylenediamine and isophoronediamine.
4. The method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel according to claim 2, characterized in that: The mass ratio of the isophorone diisocyanate, hexamethylene diisocyanate, polytetramethylene ether diol, ethanolamine hydrophilic chain extender, Maya blue attapulgite hybrid pigment, organic bismuth catalyst, acetone, hydroxyl-terminated poly 1,4-butadiene, diisopropanolamine crosslinking agent, small molecule acid neutralizer, and small molecule diamine chain extender is 10-15:10-20:15-30:3-12:1-7:0-1:10-20:3-10:0-1:2-8:3-10.
5. The method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel according to claim 2, characterized in that: In step (1), the temperature of the heating and stirring reaction is 80-90°C and the time is 1-2 hours; the temperature of the neutralization reaction is 40-60°C and the time is 20-30 minutes; in step (2), the temperature of the temperature-raising chain extension is 40-50°C and the time is 3-5 hours; in step (3), the temperature of the deacetone is 40-60°C.
6. The method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel according to claim 2, characterized in that: The preparation steps of Maya blue attapulgite hybrid pigment are as follows: Take an organic pigment and attapulgite and mix them evenly. Put them in an oven for drying. Take them out and cool them to room temperature, then disperse them in water, add isopropanol, tetraethyl orthosilicate, methacryloxypropyl triethoxysilane and hydrochloric acid, react at 70-90 °C for 20-30h, filter them after cooling to room temperature, wash them with isopropanol, and freeze-dry them at -30--10 °C to obtain an acryloxy-modified Maya blue hybrid pigment; wherein the mass ratio of the organic pigment, attapulgite, tetraethyl orthosilicate and methacryloxypropyl triethoxysilane is 1:10:0.2:
1.
7. The method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel according to claim 1, characterized in that: The preparation steps of the organosiloxane / polyurethane composite coating are as follows: At room temperature, a certain proportion of methacryloxypropyl tris(trimethylsiloxane)silane, vinyl-terminated polydimethylsiloxane and polybutadiene rubber modified polyurethane prepolymer are mixed, stirred and mixed evenly, and then azobisisoheptanenitrile is added, stirred and dissolved to obtain an organic siloxane / polyurethane composite coating; wherein the mass ratio of the methacryloxypropyl tris(trimethylsiloxane)silane, vinyl-terminated polydimethylsiloxane, polybutadiene rubber modified polyurethane prepolymer and azobisisoheptanenitrile is 5-10:15-30:55-70:2-6.
8. The method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel according to claim 1, characterized in that: The substrate layer (1) is carbon fiber cloth.
9. The method for preparing a skin-feeling antifouling functional finishing material for a mobile phone back panel according to claim 1, characterized in that: The drying temperature in step 2 is 110-130°C; the drying temperature in step 3 is 90-110°C and the time is 4-8 minutes.
10. A skin-feeling antifouling functional finishing material for a mobile phone back panel, characterized in that: Prepared by the method according to any one of claims 1 to 9, the finishing material is composed of a substrate layer (1), a waterborne polyurethane surface layer (2), and a silicone skin-feel antifouling layer (3) arranged in sequence from bottom to top, wherein the waterborne polyurethane surface layer (2) is a waterborne polyurethane resin double-modified with a Maya blue-like concave clay hybrid pigment and poly-1,4-butadiene, and the silicone skin-feel antifouling layer (3) is an organosiloxane / polyurethane composite coating.