Packaging paper with surface coated with antibacterial coating
By using bamboo, sisal fiber and modified chitosan to prepare antibacterial coatings, the problem of poor antibacterial performance of traditional packaging paper is solved, the antibacterial and durability of packaging paper is improved, and the stable and efficient antibacterial effect is achieved.
Patent Information
- Application Number
- CN202411445568.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional wrapping paper has poor antibacterial properties, and the compatibility of antibacterial agents with paper is poor, resulting in reduced mechanical properties and oozing of antibacterial agents and whitening.
Using bamboo and sisal fiber as the main raw materials, surface-coated antibacterial coatings are prepared through beating and coating processes, and antibacterial coatings made of modified chitosan and butyl acrylate are enhanced to enhance the antibacterial properties and compatibility of the packaging paper. sex.
It improves the antibacterial, durability and mechanical properties of packaging paper, and the antibacterial coating is environmentally friendly, has long-term and stable performance, and is not easy to fall off.
Smart Images

Figure BDA0005087641530000031 
Figure BDA0005087641530000041 
Figure BDA0005087641530000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of packaging paper, and in particular relates to packaging paper with an antibacterial coating on the surface. Background Art
[0002] Wrapping paper is a kind of paper material used for packaging items. It usually has good strength, toughness, pressure resistance and folding resistance. The quality requirements are slightly simpler than those of cultural printing paper. There are many types of wrapping paper, which can be roughly divided into: ordinary wrapping paper, special wrapping paper, trademark wrapping paper, oil-proof paper, moisture-proof paper, food wrapping paper, etc. Ordinary wrapping paper is strong and tough and is used for general packaging; special wrapping paper is named according to its purpose and its properties are also different; trademark wrapping paper is used for packaging after printing; oil-proof paper has the property of preventing grease penetration; and moisture-proof paper has moisture-proof properties.
[0003] Paper packaging has been widely used in food packaging, milk tea packaging and other fields in recent years due to its green and environmentally friendly characteristics. However, the antibacterial properties of the wrapping paper used in traditional paper packaging are poor. Over time, many microorganisms begin to breed inside the paper, which will not only corrode the wrapping paper, but also have a great impact on the packaged products. The common antibacterial wrapping paper on the market currently has antibacterial agents directly added during the preparation of the wrapping paper. However, the compatibility of antibacterial agents with wrapping paper is poor, which will not only reduce the mechanical properties of the wrapping paper, but also cause the antibacterial agents in the wrapping paper to seep out after long-term use, causing the wrapping paper to turn white. Therefore, it is urgent to solve the above problems to meet the higher demands in the field of wrapping paper technology. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a packaging paper with an antibacterial coating on the surface.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A packaging paper with an antibacterial coating on its surface is prepared by the following steps:
[0007] A1. Add bamboo into a crusher for crushing, then add water, stir and mix thoroughly, add lemon fat and sisal fiber, stir and mix well, then put into a beater, adjust the speed to 1000r / min, mix for 2h, and finally make paper to obtain paper;
[0008] A2. Use a coating machine to apply the antibacterial coating on the upper and lower surfaces of the paper obtained in step A1. After drying and cooling, a packaging paper with the antibacterial coating on the surface is obtained.
[0009] Furthermore, the raw materials are calculated in parts by weight as follows: 60-80 parts of bamboo, 240-320 parts of water, 2-4 parts of lemon fat, and 6-12 parts of sisal fiber.
[0010] Bamboo fiber is a plant fiber with natural antibacterial properties. It not only enhances the antibacterial effect of the wrapping paper, but is also environmentally friendly. The added sisal fiber is a plant fiber with high strength and durability, which can enhance the strength and durability of the wrapping paper.
[0011] Furthermore, the antibacterial coating is prepared by the following steps:
[0012] Butyl acrylate, methyl methacrylate and an emulsifier are added into water and emulsified to obtain an emulsion. Then an initiator is added to initiate a polymerization reaction. After the reaction is completed, an antibacterial agent is added, vigorously stirred, and ultrasonically dispersed for 40 minutes to obtain an antibacterial coating.
[0013] Furthermore, the raw materials are calculated in parts by weight as follows: 30-40 parts of butyl acrylate, 25-35 parts of methyl methacrylate, 3-6 parts of emulsifier, 60-80 parts of water, 1-3 parts of initiator, and 5-15 parts of antibacterial agent.
[0014] Furthermore, the emulsifier is prepared by compounding alkylphenol polyoxyethylene ether and sodium lauryl sulfate in a mass ratio of 1:2.
[0015] Furthermore, the initiator is a water-soluble initiator.
[0016] The prepared antibacterial coating is an acrylic water-based coating, which is not only environmentally friendly but also has good pollution resistance. It can isolate the packaging paper from the external environment and protect the packaging paper. In addition, two soft monomers, butyl acrylate and ethyl acrylate, are selected to make the prepared coating more flexible. The emulsifier is an anionic and non-ionic composite emulsifier, which has a better emulsification effect.
[0017] Furthermore, the antibacterial agent is prepared by the following steps:
[0018] S1. Dissolve 5,5-dimethylhydantoin in acetone in a flask, add anhydrous potassium carbonate (acid binding agent), heat to 70°C, reflux for 0.5h, add 1,3-dichloropropane, continue to heat to 80°C, reflux for 4h, complete, filter with diatomaceous earth column chromatography to remove inorganic salts, wash with ethyl acetate 2-3 times, and then purify by column chromatography (eluent uses a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 3:2), remove the eluent by rotary evaporation to obtain intermediate 1; the ratio of 5,5-dimethylhydantoin, acetone, anhydrous potassium carbonate, and 1,3-dichloropropane is 12.8g:150mL:13.8g:12.4g;
[0019] Under the catalysis of anhydrous potassium carbonate, 5,5-dimethylhydantoin and 1,3-dichloropropane undergo a nucleophilic substitution reaction. By controlling the molar ratio of the two to be close to 1:1 and a slight excess of 1,3-dichloropropane, intermediate 1 is obtained. The specific reaction process is shown below:
[0020]
[0021] S2, dissolving intermediate 1 in a mixed solvent of tert-butanol and water (the volume ratio of tert-butanol and water is 4:1), stirring and mixing evenly, adding tert-butyl hypochlorite, reacting at room temperature for 8h under light-proof conditions, after the reaction is completed, removing the solvent by distillation under reduced pressure to obtain intermediate 2; the ratio of the amount of intermediate 1, the mixed solvent of tert-butanol and water, and tert-butyl hypochlorite is 20.4g:150mL:15mL;
[0022] The specific reaction process is as follows:
[0023]
[0024] S3, add intermediate 2 and N, N-dimethylformamide to a three-necked flask equipped with a stirring device, stir and mix evenly, then add 4-pyridinecarboxaldehyde dropwise, control the reaction temperature to 70°C, keep the reaction for 6 hours, and after the reaction is completed, remove part of the solvent by distillation under reduced pressure, and then purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two is 4:3), and remove the eluent by rotary evaporation to obtain intermediate 3; the ratio of the amount of intermediate 2, N, N-dimethylformamide, and 4-pyridinecarboxaldehyde is 23.8g:150mL:10.7g;
[0025] Intermediate 2 undergoes quaternization reaction with 4-pyridinecarboxaldehyde to obtain intermediate 3; the specific reaction process is as follows:
[0026]
[0027] S4, chitosan was added to a mixed solution of acetic acid and toluene (the mass fraction of acetic acid was 28%), stirred until completely dissolved, then intermediate 3 and piperidine (condensation agent) were added, stirred and reacted at room temperature for 30 min, sodium hydroxide solution was added dropwise to adjust the pH to 5.5, and the reaction was continued for 2 h. After the reaction was completed, the mixture was allowed to stand for precipitation, filtered, washed with ethanol and water in turn, and dried in an oven to obtain modified chitosan; the ratio of the mixed solution of acetic acid and toluene, chitosan, intermediate 3, and piperidine was 100 mL: 1 g: 8.5 g: 15 mL;
[0028] Under the action of the condensing agent, the aldehyde group on the intermediate 3 condenses with the amino group on the chitosan to form an imine group (C=N Schiff base structure) to obtain modified chitosan; the specific reaction process is as follows:
[0029]
[0030] Chitosan is a natural antibacterial material with biodegradability. Chitosan is also a high molecular compound with good film-forming properties, which can enhance the mechanical properties of acrylic matrix. By modifying chitosan and connecting it with organic molecular chains through C=N, the hydrogen bonding effect of chitosan amino groups is weakened, the biological activity and antibacterial properties of chitosan are improved, and the surface hydrophobicity of the modified chitosan is improved, which enhances the compatibility with the matrix and promotes the dispersion of the modified chitosan, so that the performance of the modified chitosan is fully exerted, and the antibacterial properties of the matrix are greatly enhanced. In addition, the modified chitosan molecule also contains pyridinium quaternary ammonium salt and chloramine structure, among which pyridinium quaternary ammonium salt is a new type of quaternary ammonium salt with more concentrated positive charge and stronger bactericidal ability, which avoids the problem of bacterial resistance caused by the long-term use of quaternary ammonium salt antibacterial agents and can greatly enhance the antibacterial properties of the matrix. The introduced chloramine is an excellent antibacterial structure with certain regeneration, which can release strong oxidizing Cl + It destroys the bacterial structure and works synergistically with the C=N group and quaternary ammonium salt of pyridinium, significantly improving the antibacterial properties of the matrix;
[0031] It should be added that the organic molecular chains are connected to the chitosan molecules through chemical bonding, which can improve the migration and exudation resistance of the organic molecular chains and make the antibacterial properties of the modified chitosan long-term and stable.
[0032] Beneficial effects of the present invention:
[0033] 1. The main raw material of the packaging paper prepared by the present invention is bamboo, and the bamboo fiber in the bamboo gives the packaging paper a certain antibacterial property;
[0034] 2. The added sisal fiber is a natural plant fiber that can improve the strength and durability of the wrapping paper;
[0035] 3. The antibacterial coating prepared is an acrylic water-based coating, which can protect the packaging paper and is environmentally friendly;
[0036] 4. Compared with ordinary chitosan, the prepared modified chitosan has better compatibility with acrylic matrix. Various groups in the molecule play a synergistic role, which can greatly enhance the antibacterial property of packaging paper, and the performance is long-lasting and stable, and it is not easy to fall off;
[0037] Therefore, the packaging paper prepared by the present invention has stable and efficient antibacterial properties, good durability, excellent mechanical properties, is green and environmentally friendly, and has important application value in the field of packaging paper technology. DETAILED DESCRIPTION
[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Embodiment 1
[0040] Preparation of antimicrobial agent:
[0041] S1. Dissolve 12.8 g of 5,5-dimethylhydantoin in 150 mL of acetone in a flask, add 13.8 g of anhydrous potassium carbonate, heat to 70 ° C, reflux for 0.5 h, add 12.4 g of 1,3-dichloropropane, continue to heat to 80 ° C, reflux for 4 h, complete, filter with diatomaceous earth column chromatography to remove inorganic salts, wash with ethyl acetate 3 times, and then purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 3:2), and remove the eluent by rotary evaporation to obtain intermediate 1;
[0042] S2, 20.4g of intermediate 1 was dissolved in 150mL of a mixed solvent of tert-butyl alcohol and water (the volume ratio of tert-butyl alcohol to water was 4:1), and after stirring and mixing evenly, 15mL of tert-butyl hypochlorite was added, and the mixture was reacted at room temperature for 8h under light-proof conditions. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate 2;
[0043] S3, in a three-necked flask equipped with a stirring device, 23.8g of intermediate 2 and 150mL of N,N-dimethylformamide were added and stirred and mixed uniformly, and then 10.7g of 4-pyridinecarboxaldehyde was added dropwise, and the reaction temperature was controlled to 70°C. The reaction was kept warm for 6 hours. After the reaction was completed, part of the solvent was removed by distillation under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 4:3), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0044] S4. Add 1 g of chitosan to a mixed solution of 100 mL of acetic acid and toluene (the mass fraction of acetic acid is 28%), stir until completely dissolved, then add 8.5 g of intermediate 3 and 15 mL of piperidine, stir and react at room temperature for 30 min, add dropwise sodium hydroxide solution to adjust the pH to 5.5, continue the reaction for 2 h, and after the reaction is completed, let it stand and precipitate, filter, wash with ethanol and water in turn, and dry in an oven to obtain modified chitosan.
[0045] Embodiment 2
[0046] Preparation of antimicrobial agent:
[0047] S1. Dissolve 25.6 g of 5,5-dimethylhydantoin in 300 mL of acetone in a flask, add 27.6 g of anhydrous potassium carbonate, heat to 70°C, reflux for 0.5 h, add 24.8 g of 1,3-dichloropropane, continue to heat to 80°C, reflux for 4 h, complete, filter with diatomaceous earth column chromatography to remove inorganic salts, wash twice with ethyl acetate, and then purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 3:2), and remove the eluent by rotary evaporation to obtain intermediate 1;
[0048] S2, 40.8g of intermediate 1 was dissolved in 300mL of a mixed solvent of tert-butyl alcohol and water (the volume ratio of tert-butyl alcohol to water was 4:1), and after stirring and mixing evenly, 30mL of tert-butyl hypochlorite was added, and the mixture was reacted at room temperature for 8h under light-proof conditions. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate 2;
[0049] S3, in a three-necked flask equipped with a stirring device, 47.6g of intermediate 2 and 300mL of N,N-dimethylformamide were added and stirred and mixed uniformly, and then 21.4g of 4-pyridinecarboxaldehyde was added dropwise, and the reaction temperature was controlled to 70°C, and the reaction was kept warm for 6 hours. After the reaction was completed, part of the solvent was removed by distillation under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 4:3), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0050] S4. Add 2 g of chitosan to a mixed solution of 200 mL of acetic acid and toluene (the mass fraction of acetic acid is 28%), stir until completely dissolved, then add 17 g of intermediate 3 and 30 mL of piperidine, stir and react at room temperature for 30 min, add sodium hydroxide solution dropwise to adjust the pH to 5.5, continue the reaction for 2 h, and after the reaction is completed, let it stand and precipitate, filter, wash with ethanol and water in turn, and dry in an oven to obtain modified chitosan.
[0051] Embodiment 3
[0052] Preparation of antimicrobial coating:
[0053] 30g of butyl acrylate, 25g of methyl methacrylate and 3g of emulsifier (prepared by compounding 1g of alkylphenol polyoxyethylene ether and 2g of sodium dodecyl sulfate) were added to 60g of water and emulsified to obtain an emulsion. Then, 1g of azobisisopropylimidazoline was added to initiate a polymerization reaction. After the reaction was completed, 5g of the antibacterial agent prepared in Example 1 was added, and the mixture was vigorously stirred and ultrasonically dispersed for 40 minutes to obtain an antibacterial coating.
[0054] Embodiment 4
[0055] Preparation of antimicrobial coating:
[0056] 35g of butyl acrylate, 30g of methyl methacrylate and 6g of emulsifier (prepared by compounding 2g of alkylphenol polyoxyethylene ether and 4g of sodium dodecyl sulfate) were added to 70g of water and emulsified to obtain an emulsion. Then, 2g of azobisisopropylimidazoline was added to initiate polymerization. After the reaction was completed, 10g of the antibacterial agent prepared in Example 2 was added, the mixture was vigorously stirred and ultrasonically dispersed for 40 minutes to obtain an antibacterial coating.
[0057] Embodiment 5
[0058] Preparation of antimicrobial coating:
[0059] 40g of butyl acrylate, 35g of methyl methacrylate and 6g of emulsifier (prepared by compounding 2g of alkylphenol polyoxyethylene ether and 4g of sodium dodecyl sulfate) were added to 80g of water and emulsified to obtain an emulsion. Then, 3g of azobisisopropylimidazoline was added to initiate polymerization. After the reaction was completed, 15g of the antibacterial agent prepared in Example 2 was added, the mixture was vigorously stirred and ultrasonically dispersed for 40 minutes to obtain an antibacterial coating.
[0060] Embodiment 6
[0061] A1. Add 60g of bamboo into a grinder for grinding, then add 240g of water, stir and mix thoroughly, add 2g of lemon fat and 6g of sisal fiber, stir and mix well, then put into a beater, adjust the speed to 1000r / min, mix for 2h, and finally make paper to obtain paper;
[0062] A2. Use a coating machine to apply the antibacterial coating prepared in Example 5 on the upper and lower surfaces of the paper prepared in step A1. After drying and cooling, a packaging paper with the antibacterial coating on the surface is obtained.
[0063] Embodiment 7
[0064] A1. Add 80g of bamboo into a pulverizer for pulverization, then add 320g of water, stir and mix thoroughly, add 4g of lemon fat and 12g of sisal fiber, stir and mix well, then put into a beater, adjust the speed to 1000r / min, mix for 2h, and finally make paper to obtain paper;
[0065] A2. Use a coating machine to apply the antibacterial coating prepared in Example 5 on the upper and lower surfaces of the paper prepared in step A1. After drying and cooling, a packaging paper with the antibacterial coating on the surface is obtained.
[0066] Comparative Example 1
[0067] The antibacterial agent in Example 5 was replaced by a commercially available antibacterial agent of equal quality, and the remaining steps were the same as those in Example 5 to prepare an antibacterial coating.
[0068] Comparative Example 2
[0069] The antibacterial agent in Example 5 was replaced by ordinary chitosan of the same mass, and the remaining steps were the same as those in Example 5 to prepare the antibacterial coating.
[0070] The following performance tests were performed on Examples 3, 4, 5, and Comparative Examples 1 and 2 according to different test standards:
[0071] The flexibility is measured using the national standard GB / T 1731-1993 "Determination of paint film flexibility";
[0072] The national standard GB / T 21866-2008 "Determination of antibacterial properties and antibacterial effects of antibacterial coatings (paint films)" was used to determine the antibacterial performance and antibacterial durability;
[0073] The measured results are shown in the following table:
[0074]
[0075] It can be seen from the above table that the antibacterial coating prepared in the embodiment of the present invention has excellent antibacterial property, high antibacterial durability and is not easy to fall off. Coating it on the surface of packaging paper can greatly enhance the antibacterial property of the packaging paper, and has important application value in the field of packaging paper technology.
[0076] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0077] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A packaging paper with an antibacterial coating on its surface, It is characterized in that Prepared by the following steps: A1. Add bamboo to a crusher for crushing, then add water, stir and mix thoroughly, add lemon fat and sisal fiber, stir and mix well, then put into a pulper, and finally make paper to obtain paper; A2. Use a coating machine to apply the antibacterial coating on the upper and lower surfaces of the paper obtained in step A1. After drying and cooling, a packaging paper with the antibacterial coating on the surface is obtained.
2. The packaging paper with antibacterial coating on the surface according to claim 1, It is characterized in that The antibacterial coating is prepared by the following steps: Butyl acrylate, methyl methacrylate and an emulsifier are added into water and emulsified to obtain an emulsion. Then an initiator is added to initiate a polymerization reaction. After the reaction is completed, an antibacterial agent is added, vigorously stirred, and ultrasonically dispersed to obtain an antibacterial coating.
3. The packaging paper with antibacterial coating on the surface according to claim 2, It is characterized in that The antibacterial agent is prepared by the following steps: S1. Dissolve 5,5-dimethylhydantoin in acetone, add anhydrous potassium carbonate, heat to 70°C, reflux for 0.5h, add 1,3-dichloropropane, continue to heat to 80°C, reflux for 4h, complete, filter with diatomaceous earth column chromatography to remove inorganic salts, wash, purify by column chromatography, and rotary evaporate to obtain intermediate 1; S2, dissolving the intermediate 1 in a mixed solvent of tert-butyl alcohol and water, stirring and mixing evenly, adding tert-butyl hypochlorite, reacting at room temperature for 8 hours under light-proof conditions, and after the reaction is completed, distilling under reduced pressure to obtain the intermediate 2; S3. After the intermediate 2 and N,N-dimethylformamide are stirred and mixed evenly, 4-pyridinecarboxaldehyde is added dropwise, and the reaction is carried out at 70°C for 6. After the reaction is completed, vacuum distillation is performed, column chromatography is performed for purification, and rotary evaporation is performed to obtain the intermediate 3. S4. Add chitosan to the mixed solution of acetic acid and toluene, stir until completely dissolved, then add intermediate 3 and piperidine, stir and react at room temperature for 30 minutes, adjust the pH to 5.5, continue the reaction for 2 hours, and after the reaction is completed, let it stand and precipitate, filter, wash, and dry to obtain modified chitosan.
4. The packaging paper with antibacterial coating on the surface according to claim 3, It is characterized in that In step S1, the ratio of 5,5-dimethylhydantoin, acetone, anhydrous potassium carbonate and 1,3-dichloropropane is 12.8 g:150 mL:13.8 g:12.4 g.
5. The packaging paper with antibacterial coating on the surface according to claim 3, It is characterized in that In step S2, the ratio of the intermediate 1, the mixed solvent of tert-butyl alcohol and water, and tert-butyl hypochlorite is 20.4 g: 150 mL: 15 mL.
6. The packaging paper with antibacterial coating on the surface according to claim 3, It is characterized in that In step S3, the ratio of the amount of intermediate 2, N,N-dimethylformamide, and 4-pyridinecarboxaldehyde is 23.8 g:150 mL:10.7 g.
7. The packaging paper with antibacterial coating on the surface according to claim 3, It is characterized in that In step S4, the ratio of the mixed solution of acetic acid and toluene, chitosan, intermediate 3, and piperidine is 100 mL: 1 g: 8.5 g: 15 mL.
8. The packaging paper with antibacterial coating on the surface according to claim 1, It is characterized in that The raw materials are calculated as follows according to weight: 60-80 parts of bamboo, 240-320 parts of water, 2-4 parts of lemon fat, and 6-12 parts of sisal fiber.
9. The packaging paper with antibacterial coating on the surface according to claim 2, It is characterized in that The raw materials are calculated in parts by weight as follows: 30-40 parts of butyl acrylate, 25-35 parts of methyl methacrylate, 3-6 parts of emulsifier, 60-80 parts of water, 1-3 parts of initiator, and 5-15 parts of antibacterial agent.