Aluminum alloy matrix composite component, preparation method thereof and head-mounted display equipment

By using the preparation method of aluminum alloy-based composite components in the head-mounted display device, the sintering treatment of high-strength metal inserts and aluminum alloys is used to form metal bonds, which solves the lightweight, high strength and high wear resistance of the components Problem, efficient performance improvement has been achieved.

CN119062658APending Publication Date: 2024-12-03GOERTEK INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310647200.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

It is difficult for components in head-mounted display devices to meet the requirements of lightweight, high strength and high wear resistance at the same time.

Method used

Using the preparation method of aluminum alloy-based composite material components, the high-strength metal insert is positioned and embedded in the target mold, and the aluminum alloy substrate is injected and molded to obtain the composite blank, and the aluminum alloy and high-strength metal insert are realized through sintering treatment. The heterogeneous metal diffuses, forming metal bonds, and forming a dense overall structure.

Benefits of technology

The high strength, lightweight and high wear resistance of aluminum alloy-based composite components are achieved, and the difficulty of components in the prior art to meet the requirements of lightweight, high strength and high wear resistance at the same time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119062658A_ABST
    Figure CN119062658A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy-based composite material component, a preparation method thereof and head-mounted display equipment, and relates to the technical field of metal composite materials, the aluminum alloy-based composite material component is applied to the head-mounted display equipment, and the preparation method of the aluminum alloy-based composite material component comprises the following steps that an aluminum alloy feed is prepared; the aluminum alloy feed is injected into a target mold with a high-strength metal insert for injection molding, and a composite blank is obtained; and the composite blank is sintered, and the aluminum alloy matrix composite component is obtained. The technical problem that components in head-mounted display equipment in the prior art are difficult to meet the requirements of light weight, high strength and high wear resistance at the same time is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal composite materials, and in particular to an aluminum alloy-based composite material component and a preparation method thereof, and a head-mounted display device. Background Art

[0002] With the development of 5G (5th Generation Mobile Communication Technology), blockchain, cloud computing, and next-generation Internet technologies, electronic products such as mobile phones, tablets, laptops, AR (Augmented Reality) / VR (Virtual Reality) devices are moving towards lightweight and portable miniaturization. Metal precision components, as important components of consumer electronic products, have achieved great development, especially head-mounted display devices represented by AR / VR devices, which have higher requirements for lightweight and user experience. The human head is very sensitive to the weight of wearable products. Overweight products will make consumers feel uncomfortable and reduce comfort. Therefore, structural weight reduction is an important development direction to improve customer experience. Due to their complex structure and small size, the various components in head-mounted display devices have high requirements for strength and wear resistance in addition to lightweight requirements. For example, precision hardware such as AR glasses shafts will experience repeated folding when worn, and may be folded more than 50,000 times during their entire life cycle. Therefore, shaft-type components have high strength and high wear resistance requirements to prevent damage during wearing or folding.

[0003] However, it is currently difficult for components in head-mounted display devices to simultaneously meet the requirements of light weight, high strength, and high wear resistance. Summary of the invention

[0004] The main purpose of the present application is to provide an aluminum alloy-based composite material component and a preparation method thereof, and a head-mounted display device, aiming to solve the technical problem that the components in the head-mounted display device in the prior art are difficult to simultaneously meet the requirements of light weight, high strength and high wear resistance.

[0005] To achieve the above object, the present application provides a method for preparing an aluminum alloy-based composite material component, wherein the aluminum alloy-based composite material component is applied to a head-mounted display device, and the method for preparing the aluminum alloy-based composite material component comprises the following steps:

[0006] preparing aluminum alloy feedstock;

[0007] Injecting the aluminum alloy feed into a target mold with a high-strength metal insert for injection molding to obtain a composite blank;

[0008] The composite blank is sintered to obtain an aluminum alloy-based composite material component.

[0009] Optionally, the step of injecting the aluminum alloy feed into a target mold with a high-strength metal insert for injection molding to obtain a composite blank comprises:

[0010] The aluminum alloy feed is injected into a target mold with a high-strength metal insert, the injection temperature is controlled to be 160-220° C., the injection pressure is 1200-1600 bar, the mold temperature is 35° C.-45° C., the pressure is maintained at 800-1200 bar, and the composite blank is obtained by cooling for 4s-12s.

[0011] Optionally, the step of injecting the aluminum alloy feed into a target mold with a high-strength metal insert for injection molding to obtain a composite blank comprises:

[0012] Obtaining an aluminum alloy insert, and placing the aluminum alloy insert in the target mold;

[0013] The aluminum alloy feedstock is injected into a target mold where a high-strength metal insert and an aluminum alloy insert are placed for injection molding, so that the high-strength metal insert and the aluminum alloy insert are connected by the aluminum alloy feedstock to obtain a composite blank.

[0014] Optionally, the step of preparing the aluminum alloy feedstock comprises:

[0015] mixing aluminum alloy powder with a binder to obtain an aluminum alloy mixture;

[0016] The aluminum alloy mixture is heated, mixed and granulated to obtain an aluminum alloy feedstock.

[0017] Optionally, the volume proportion of the binder in the aluminum alloy mixture is 15-35%.

[0018] Optionally, the binder comprises polyethylene glycol, polymethyl methacrylate and stearic acid, wherein the volume proportion of the polyethylene glycol in the binder is 65-85%, the volume proportion of the polymethyl methacrylate in the binder is 14-30%, and the volume proportion of the stearic acid in the binder is 1-5%;

[0019] And / or, the aluminum alloy powder includes spherical aluminum alloy powder, D50 of the spherical aluminum alloy powder is less than 45 μm, and D90 of the spherical aluminum alloy powder is 35-40 μm.

[0020] Optionally, the temperature of the heating and kneading is 140-220° C., the rotation speed of the heating and kneading is 30-50 r / min, and the time of the heating and kneading is 1-4 h.

[0021] Optionally, the step of sintering the composite blank to obtain an aluminum alloy-based composite material component comprises:

[0022] The composite blank is heated to 400-600° C. at a rate of 3-6° C. / min in an inert atmosphere, and thermally degreased for 1-3 hours to obtain a thermally degreased blank;

[0023] The hot degreased blank is sintered in an inert atmosphere at a temperature of 300-650° C. for 3-5 hours, and then cooled to room temperature in the furnace to obtain an aluminum alloy-based composite material component.

[0024] Optionally, the strength of the high-strength metal insert is greater than 900 MPa, the Vickers hardness is greater than 350, and the strength of the raw aluminum alloy used to prepare the aluminum alloy feed is greater than 200 MPa.

[0025] Optionally, the high-strength metal insert is one of a steel insert and a titanium alloy insert.

[0026] Optionally, when the high-strength metal insert is a steel insert, the density of the aluminum alloy-based composite material component is 3.0 to 6.0 g / cm 3 ;

[0027] When the high-strength metal insert is a titanium alloy insert, the density of the aluminum alloy-based composite material component is 2.8 to 4.0 g / cm 3 .

[0028] The present application also provides an aluminum alloy-based composite material component, which is applied to a head-mounted display device. The aluminum alloy-based composite material component is prepared by the above-mentioned method for preparing an aluminum alloy-based composite material component, and the aluminum alloy-based composite material component comprises:

[0029] an aluminum alloy substrate; and

[0030] At least one load-bearing portion connected to the aluminum alloy substrate;

[0031] Wherein, the load-bearing part is one of a steel load-bearing part and a titanium alloy load-bearing part.

[0032] The present application also provides a head-mounted display device, which includes the aluminum alloy-based composite material component as described above.

[0033] Optionally, the head-mounted display device is a pair of glasses, and the aluminum alloy-based composite material component is arranged at the rotation axis position of the glasses; or, the head-mounted display device is a VR head-mounted display device, and the aluminum alloy-based composite material component is arranged at the flip structure between the main body and the headband of the VR head-mounted display device.

[0034] The present application provides an aluminum alloy-based composite material component and a preparation method thereof, and a head-mounted display device. The aluminum alloy-based composite material component is applied to the head-mounted display device. The preparation method of the aluminum alloy-based composite material component comprises the steps of: preparing an aluminum alloy feed; injecting the aluminum alloy feed into a target mold with a high-strength metal insert placed therein for injection molding to obtain a composite blank; and sintering the composite blank to obtain an aluminum alloy-based composite material component. The present application positions a high-strength metal insert with relatively large strength and embeds it in a target mold, performs injection molding of an aluminum alloy matrix portion, and obtains a composite blank formed by the aluminum alloy and the high-strength metal insert. Then, by degreasing and sintering the composite blank, diffusion of the aluminum alloy into the dissimilar metal of the high-strength metal insert is achieved, and aluminum atoms form metal bonds with metal atoms in the high-strength metal insert. Then, by sintering, the aluminum alloy portion in the composite blank and the high-strength metal insert form a dense whole, namely, an aluminum alloy-based composite material component. The portion of the high-strength metal insert in the obtained aluminum alloy-based composite material component can be used for bearing force or contact friction, while the aluminum alloy portion has a lower density, which can effectively reduce the mass of the aluminum alloy-based composite material component and meet the demand for lightweight. Thus, the finally prepared aluminum alloy-based composite material component has the advantages of high strength, lightweight and high wear resistance at the same time, overcoming the technical problem that the components in the head-mounted display device in the prior art are difficult to meet the requirements of lightweight, high strength and high wear resistance at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0037] Figure 1 A schematic diagram of a process of an embodiment of a method for preparing an aluminum alloy-based composite material component of the present application;

[0038] Figure 2 A stress diagram of an example of an aluminum alloy-based composite material component sample in this application;

[0039] Figure 3 A side cross-sectional view of the aluminum alloy-based composite material component prepared in Example 1 of the present application;

[0040] Figure 4A top view of the aluminum alloy-based composite material component prepared in Example 1 of the present application;

[0041] Figure 5 A side cross-sectional view of the aluminum alloy-based composite material component prepared in Example 2 of the present application;

[0042] Figure 6 This is a side cross-sectional view of the aluminum alloy-based composite material component prepared in Example 3 of the present application.

[0043] Description of Figure Numbers:

[0044] Label name Label name 10 Aluminum alloy substrate 20 High strength metal inserts 30 Aluminum alloy inserts 40 Load-bearing department

[0045] The purpose, features and advantages of this application will be further described in conjunction with the embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0046] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0047] With the development of 5G (5th Generation Mobile Communication Technology), blockchain, cloud computing, and next-generation Internet technologies, electronic products such as mobile phones, tablets, laptops, AR (Augmented Reality) / VR (Virtual Reality) devices are moving towards lightweight and portable miniaturization. Metal precision components, as important components of consumer electronic products, have achieved great development, especially head-mounted display devices represented by AR / VR devices, which have higher requirements for lightweight and user experience. The human head is very sensitive to the weight of wearable products. Overweight products will make consumers feel uncomfortable and reduce comfort. Therefore, structural weight reduction is an important development direction to improve customer experience. Due to their complex structure and small size, the various components in head-mounted display devices have high requirements for strength and wear resistance in addition to lightweight requirements. For example, precision hardware such as AR glasses shafts will experience repeated folding when worn, and may be folded more than 50,000 times during their entire life cycle. Therefore, shaft-type components have high strength and high wear resistance requirements to prevent damage during wearing or folding.

[0048] Steel has high strength, which can reach more than 1500MPa, good wear resistance, low cost and abundant output. It is very suitable for making small precision hardware such as mobile phone card trays, ejectors, gear precision shafts, etc. However, the density of steel is about 7.8g / cm 3 , it is not suitable for smart wearable products that have a strong demand for lightweight; titanium alloy has certain lightweight advantages over steel, but titanium alloy is more expensive and more difficult to process.

[0049] For lightweight, aluminum alloy is currently used, and the density of aluminum alloy is 2.7g / cm 3 , which is particularly beneficial for lightweighting and can also meet the requirements of general loads. However, due to the low strength and poor wear resistance of aluminum alloys, it can generally only be used as a shell material and cannot meet the wear resistance requirements of small precision hardware on smart wearable products. It is not suitable for making small precision hardware such as precision shafts. In order to improve the wear resistance of aluminum, a wear-resistant coating can be formed on the surface of the aluminum alloy, such as anodized coating, micro-arc oxidation coating, electroplating layer, magnetron sputtering layer, etc., to enhance the wear resistance of the aluminum alloy. However, the matrix of the aluminum alloy is relatively soft, and the coating is easy to fall off, and it is still difficult to meet the wear resistance requirements. That is, it is difficult for the components in the current head-mounted display device to simultaneously meet the requirements of lightweight, high strength and high wear resistance.

[0050] In this regard, the present application provides an aluminum alloy-based composite material component and a preparation method thereof, and a head-mounted display device, comprising the steps of: preparing an aluminum alloy feed; injecting the aluminum alloy feed into a target mold with a high-strength metal insert placed therein for injection molding to obtain a composite blank; and sintering the composite blank to obtain an aluminum alloy-based composite material component. The present application positions a high-strength metal insert with relatively large strength and embeds it in a target mold, performs injection molding of an aluminum alloy matrix portion, and obtains a composite blank formed by the aluminum alloy and the high-strength metal insert, and then sintering the composite blank to achieve diffusion of the aluminum alloy into the dissimilar metal of the high-strength metal insert, so that aluminum atoms form metal bonds with metal atoms in the high-strength metal insert, and then sintering is performed to form a dense whole with the high-strength metal insert in the composite blank, namely, an aluminum alloy-based composite material component, and the portion of the high-strength metal insert in the obtained aluminum alloy-based composite material component can be used for bearing force or contact friction, while the portion of the aluminum alloy has a lower density, which can effectively reduce the mass of the aluminum alloy-based composite material component and meet the requirements of lightweight, thereby making the finally prepared aluminum alloy-based composite material component have the advantages of high strength, lightweight and high wear resistance at the same time, overcoming the technical problem that the components in the head-mounted display device in the prior art are difficult to meet the requirements of lightweight, high strength and high wear resistance at the same time.

[0051] The present application provides a method for preparing an aluminum alloy-based composite material component. In one embodiment of the method for preparing an aluminum alloy-based composite material component of the present application, referring to Figure 1 , the preparation method of the aluminum alloy-based composite material component comprises:

[0052] Step S10, preparing aluminum alloy feed;

[0053] In this embodiment, it should be noted that the aluminum alloy-based composite material component prepared in this embodiment can be applied to head-mounted display devices that have requirements for lightweight and high strength and high wear resistance. The aluminum alloy-based composite material components include hinges, bearings, rotating shafts, balls, gears and other components that bear both bending moments and torques. These components move frequently during use and have greater requirements for strength and wear resistance. The head-mounted display devices include AR glasses, VR helmets, etc.

[0054] In an operative manner, the head mounted display device is an AR glasses, the aluminum alloy-based composite material component is disposed at the rotation axis position of the AR glasses, and at least part of the aluminum alloy-based composite material component is disposed in the accommodation space formed by the frame and temples of the AR glasses. Figure 2 The aluminum alloy-based composite material component includes two load-bearing parts whose projections overlap in a preset first direction, wherein the preset first direction may be perpendicular to the extension direction of the temple of the AR glasses.

[0055] In an operative manner, the head mounted display device is a VR head mounted display device, and the aluminum alloy-based composite material component is disposed on a flip structure between a main body of the VR head mounted display device and a headband. Exemplarily, the flip structure may include a first aluminum alloy-based composite material component disposed on the main body of the head mounted display device and a second aluminum alloy-based composite material component disposed on the headband, wherein the projection of the load-bearing portion of the first aluminum alloy-based composite material component and the load-bearing portion of the second aluminum alloy-based composite material component in a preset second direction overlap, wherein the preset second direction may be parallel to the main body of the head mounted display device, and the perpendicular midline of the aluminum alloy matrix portion on the first aluminum alloy-based composite material component and the perpendicular midline of the aluminum alloy matrix portion on the second aluminum alloy-based composite material may point to the wearer of the VR head mounted display device.

[0056] Specifically, aluminum alloy material is used as raw material, and auxiliary agents such as binders are added. After mixing and granulation, aluminum alloy feed is made, wherein the binder includes one or more of polyethylene glycol, polymethyl methacrylate, stearic acid, polyoxymethylene, polypropylene, etc. The specific process parameters of the mixing and granulation can be determined according to actual conditions and test results, etc., and this embodiment does not limit this. The binder can be purchased from the market or prepared by itself according to actual conditions, and the specific ingredients and proportions are not limited in this embodiment.

[0057] Optionally, the step of preparing the aluminum alloy feedstock comprises:

[0058] Step S11, mixing aluminum alloy powder with a binder to obtain an aluminum alloy mixture;

[0059] In this embodiment, specifically, a certain amount of aluminum alloy powder and a binder are measured and mixed to obtain an aluminum alloy mixture, wherein the mixing ratio of the aluminum alloy powder and the binder can be determined according to actual needs or actual test results, and this embodiment does not limit this.

[0060] Optionally, the volume proportion of the binder in the aluminum alloy mixture is 15-35%.

[0061] In this embodiment, the volume proportion of the binder in the aluminum alloy mixture is 15-35%, for example, 15%, 20%, 25%, 30%, 35%, etc., so that the aluminum alloy feed can be tightly bonded by the binder to improve the molding efficiency and molding effect of injection molding.

[0062] Optionally, the binder includes polyethylene glycol, polymethyl methacrylate and stearic acid, wherein the volume proportion of the polyethylene glycol in the binder is 65-85%, the volume proportion of the polymethyl methacrylate in the binder is 14-30%, and the volume proportion of the stearic acid in the binder is 1-5%.

[0063] In this embodiment, the binder includes polyethylene glycol, polymethyl methacrylate and stearic acid, wherein the volume proportion of the polyethylene glycol in the binder is 65-84%, for example, 65%, 75%, 84%, etc., the volume proportion of the polymethyl methacrylate in the binder is 14-30%, for example, 14%, 23%, 30%, etc., and the volume proportion of the stearic acid in the binder is 1-5%, for example, 1%, 2%, 5%, etc.

[0064] Optionally, the aluminum alloy powder includes spherical aluminum alloy powder, D50 of the spherical aluminum alloy powder is less than 45 μm, and D90 of the spherical aluminum alloy powder is 35-40 μm.

[0065] In this embodiment, the aluminum alloy powder includes spherical aluminum alloy powder, the D50 (the particle size corresponding to the cumulative particle size distribution percentage of a sample reaches 50%) of the spherical aluminum alloy powder is less than 45μm, and the D90 (the particle size corresponding to the cumulative particle size distribution percentage of a sample reaches 90%) of the spherical aluminum alloy powder is 35-40μm, for example, 35μm, 38μm, 40μm, etc.

[0066] Step S12, heating, mixing and granulating the aluminum alloy mixture to obtain aluminum alloy feed.

[0067] In this embodiment, the aluminum alloy powder mixture is mixed in a vacuum environment or an inert atmosphere, and then cooled and granulated to obtain an aluminum alloy feed. The specific process parameters of mixing, cooling and granulation can be determined based on actual conditions and test results, etc., and this embodiment does not impose any restrictions on this.

[0068] Optionally, the temperature of the heating and kneading is 140-220° C., the rotation speed of the heating and kneading is 30-50 r / min, and the time of the heating and kneading is 1-4 h.

[0069] In this embodiment, the heating and kneading temperature is 140-220°C, for example, 140°C, 170°C, 200°C, 220°C, etc., the heating and kneading speed is 30-50r / min, for example, 30r / min, 40r / min, 50r / min, etc., and the heating and kneading time is 1-4h, for example, 1h, 2h, 3h, 4h, etc.

[0070] In one practicable manner, the step of preparing the aluminum alloy feedstock comprises:

[0071] The aluminum alloy powder and the binder are added into an internal mixer and filled with argon gas. The mixture is kneaded for 1-4 hours at a temperature of 140-220° C. and a rotation speed of 30-50 r / min. After cooling, the mixture is crushed and granulated to obtain an aluminum alloy feed.

[0072] Step S20, injecting the aluminum alloy feed into a target mold with a high-strength metal insert placed therein to perform injection molding to obtain a composite blank;

[0073] In this embodiment, specifically, the aluminum alloy feed is injected into a target mold with a high-strength metal insert through a powder injection molding device, and injection molding is performed to prepare a composite blank, wherein the high-strength metal insert refers to a metal insert with a strength higher than that of the aluminum alloy material, and can be prepared in advance according to the actual requirements of the strength, structure, shape, etc. of the actual load-bearing or wear-resistant parts of the aluminum alloy-based composite material component to be prepared, through powder injection molding, stamping molding, forging, 3D printing and other processes, and this embodiment does not limit this. The material of the high-strength metal insert can be steel, titanium alloy, etc., and the specific process conditions of injection molding can be tested, designed and adjusted according to the actual situation, and this embodiment does not limit this. The powder injection molding process has a mature process, a complete industrial chain, can be mass-produced, and has low cost, which is conducive to the mass production and cost reduction and efficiency improvement of aluminum alloy-based composite material components.

[0074] In an practicable manner, before the step of injecting the aluminum alloy feed into a target mold having a high-strength metal insert placed therein for injection molding to obtain a composite blank, the following steps may also be included:

[0075] Obtain at least one high-strength metal insert, and place each of the high-strength metal inserts in a corresponding target to-be-embedded area in a target mold.

[0076] In this embodiment, specifically, according to the actual needs of the aluminum alloy-based composite material component to be prepared, at least one pre-prepared high-strength metal insert and a target mold can be selected, and according to the function of each high-strength metal insert in the aluminum alloy-based composite material component to be prepared, the target area to be embedded in the target mold corresponding to each high-strength metal insert is determined, and then each high-strength metal insert is positioned and embedded in the corresponding target area to be embedded in the target mold.

[0077] In an operative manner, an aluminum alloy-based composite material component sample can be prepared, and a stress diagram of the aluminum alloy-based composite material component sample during use can be detected. For example, a stress diagram of an aluminum alloy-based composite material component sample is as follows: Figure 2 As shown, the stress map can be used to determine the magnitude of stress borne by various regions on the aluminum alloy-based composite material component, and then the region in the stress map where the stress is greater than a preset stress threshold can be determined as the target region to be embedded, and a high-strength metal insert that matches the shape and specification of the target region to be embedded is prepared, and the shape and specification of the high-strength metal insert are the same as those of the target region to be embedded or the difference is less than a preset error threshold.

[0078] Optionally, the high-strength metal insert is one of a steel insert and a titanium alloy insert.

[0079] Optionally, when the high-strength metal insert is a steel insert, the density of the aluminum alloy-based composite material component is 3.0 to 6.0 g / cm 3 ;

[0080] When the high-strength metal insert is a titanium alloy insert, the density of the aluminum alloy-based composite material component is 2.8 to 4.0 g / cm 3 .

[0081] In this embodiment, the steel has a high strength of more than 1500 MPa, good wear resistance, low cost, and abundant output. It is very suitable for making small precision hardware such as mobile phone card trays, ejectors, gear precision shafts, etc., but the density of steel is about 7.8 g / cm 3 By combining high-strength, high-wear-resistant and low-cost steel inserts with aluminum alloys, the steel part of the aluminum alloy-based composite component can be used for load bearing or contact friction, while the aluminum alloy part has a lower density, which can effectively reduce the mass of the aluminum alloy-based composite component. The density of the prepared aluminum alloy-based composite component is 3.0-6.0g / cm 3 , meeting the demand for lightweight, so that the final prepared aluminum alloy-based composite material components have the advantages of high strength, light weight, high wear resistance and low cost.

[0082] The steel insert is made of steel material through stamping, forging, powder injection molding and other processes. The steel material is an iron-carbon alloy material formed by adding an appropriate amount of one or more alloy elements to ordinary carbon steel, such as Mn13 high manganese steel, 17-4PH alloy stainless steel, GCr15 steel (high carbon chromium bearing steel), etc.

[0083] The density of titanium alloy is about 4.5g / cm 3 , with a strength of about 1000MPa. Compared with steel, titanium alloy has certain lightweight advantages. However, compared with steel, titanium alloy has higher cost and is more difficult to process. By compounding high-strength, high-wear-resistant and low-cost titanium alloy inserts with aluminum alloy, the titanium alloy part of the obtained aluminum alloy-based composite material component can be used for load bearing or contact friction, while the aluminum alloy part has a lower density, which can effectively reduce the quality of the aluminum alloy-based composite material component. The density of the prepared aluminum alloy-based composite material component is 2.8-4.0g / cm 3 , meeting the demand for lightweight, so that the final prepared aluminum alloy-based composite material components have the advantages of high strength, lightweight and high wear resistance.

[0084] The titanium alloy insert is made of titanium alloy material through stamping, forging, powder injection molding and other processes. The titanium alloy material is an alloy metal material made of titanium and other metals, such as TC4 titanium alloy (titanium alloy with elemental composition of Ti-6Al-4V), TC10 titanium alloy (titanium alloy with elemental composition of Ti-6Al-6V-2Sn-0.5Cu-0.5Fe), TC3 titanium alloy (titanium alloy with elemental composition of Ti-5Al-4V), TA7 titanium alloy (titanium alloy with elemental composition of Ti-5Al-2.5Sn), etc.

[0085] Optionally, the strength of the high-strength metal insert is greater than 900 MPa, the Vickers hardness is greater than 350, and the strength of the raw aluminum alloy used to prepare the aluminum alloy feed is greater than 200 MPa.

[0086] In this embodiment, the high-strength metal insert is mainly used for bearing force or friction, and has certain requirements for strength and hardness. Therefore, a high-strength metal insert with a strength greater than 900MPa and a Vickers hardness greater than 350 is selected. The density of the aluminum alloy is about 2.7g / cm 3 , which is particularly beneficial for lightweighting, and can effectively reduce the mass of the prepared aluminum alloy-based composite material components, thereby reducing the mass of smart wearable products processed with the aluminum alloy-based composite material components and improving the comfort of human body when wearing smart wearable products. That is, the main contribution of aluminum alloy is lightweighting, and the strength can meet the general load requirements. Therefore, a raw aluminum alloy with a strength greater than 200MPa is selected to prepare the aluminum alloy feed, which can reduce the overall mass of the finally prepared aluminum alloy-based composite material components, so that the aluminum alloy-based composite material components meet the lightweight requirements, and at the same time ensure that the parts of the finally prepared aluminum alloy-based composite material components that need to bear force or friction have sufficient strength and wear resistance.

[0087] Optionally, the step of injecting the aluminum alloy feed into a target mold with a high-strength metal insert for injection molding to obtain a composite blank comprises:

[0088] The aluminum alloy feed is injected into a target mold with a high-strength metal insert, the injection temperature is controlled to be 160-220° C., the injection pressure is 1200-1600 bar, the mold temperature is 35° C.-45° C., the pressure is maintained at 800-1200 bar, and the composite blank is obtained by cooling for 4s-12s.

[0089] In this embodiment, specifically, by using powder injection molding equipment, the injection temperature is controlled to be 160-220°C, for example, 160°C, 180°C, 200°C, 220°C, etc., the injection pressure is 1200-1600bar, for example, 1200bar, 1400bar, 1600bar, etc., the mold temperature is 35°C-45°C, for example, 35°C, 40°C, 45°C, etc., the aluminum alloy feed is injected into a target mold with a high-strength metal insert, injection molding is carried out, the pressure is maintained at 800-1200bar, for example, 800bar, 1000bar, 1200bar, etc., and the cooling is carried out for 4s-12s, for example, 4s, 8s, 12s, etc., to obtain a composite billet.

[0090] Optionally, the step of injecting the aluminum alloy feed into a target mold with a high-strength metal insert for injection molding to obtain a composite blank comprises:

[0091] Step S21, obtaining an aluminum alloy insert, and placing the aluminum alloy insert in the target mold;

[0092] In this embodiment, it should be noted that for the processing of materials with more complex structures, the powder injection molding process is relatively simple and has lower costs, but for the processing of materials with simpler shapes and structures such as plates, processes such as hot pressing forming and forging are simpler and have lower costs. Therefore, for the aluminum alloy matrix part that can be obtained by hot pressing forming, forging and other processes that are simpler or have lower costs than powder injection molding, aluminum alloy inserts can be obtained by hot pressing forming, forging and other processes that are simpler or have lower costs than injection molding, and then the aluminum alloy inserts and high-strength metal inserts can be tightly connected as a whole through injection molding.

[0093] Specifically, an aluminum alloy insert is obtained by hot pressing, forging, or other processes that are simpler or less costly than injection molding, and the aluminum alloy insert is placed in a corresponding area to be embedded in a target mold, wherein the raw aluminum alloy for preparing the aluminum alloy insert and the raw aluminum alloy for preparing the aluminum alloy feedstock may be the same or different.

[0094] It should be noted that the high-strength metal insert and the aluminum alloy insert are used as inserts and can be placed in the target mold before injecting the aluminum alloy feed. The numbering of the steps and the order of description in this embodiment do not limit the order of placing the aluminum alloy insert and placing the high-strength metal insert. That is, the aluminum alloy insert can be obtained first, and the aluminum alloy insert can be placed in the target mold, and then at least one high-strength metal insert can be obtained and each of the high-strength metal inserts can be placed in the corresponding target area to be embedded in the target mold. Alternatively, at least one high-strength metal insert can be obtained first, and each of the high-strength metal inserts can be placed in the corresponding target area to be embedded in the target mold, and then an aluminum alloy insert can be obtained and placed in the target mold.

[0095] Step S22, injecting the aluminum alloy feed material into a target mold having a high-strength metal insert and an aluminum alloy insert therein for injection molding, so as to connect the high-strength metal insert and the aluminum alloy insert through the aluminum alloy feed material to obtain a composite blank.

[0096] In this embodiment, specifically, the aluminum alloy feed is injected into a target mold in which a high-strength metal insert and an aluminum alloy insert are placed by a powder injection molding device, and injection molding is performed to connect the high-strength metal insert and the aluminum alloy insert by the aluminum alloy feed, so as to prepare an integrated composite billet formed by connecting the high-strength metal insert, the aluminum alloy insert and the aluminum alloy feed, wherein the specific process conditions of the injection molding can be tested, designed and adjusted according to actual conditions, and this embodiment does not limit this.

[0097] Step S30, sintering the composite blank to obtain an aluminum alloy-based composite material component.

[0098] In this embodiment, specifically, the injection molded composite blank is placed in an inert atmosphere for a period of time for high-temperature sintering treatment, and cooled to obtain an aluminum alloy-based composite material component, thereby obtaining a lightweight, high-strength and high-wear-resistant aluminum alloy-based composite material component, wherein the inert atmosphere can be an argon atmosphere, etc., and the temperature of the high-temperature sintering treatment can be determined according to actual needs or test results, etc., and this embodiment does not limit this.

[0099] In one feasible manner, before sintering the composite blank, the composite blank may be degreased, and the degreasing methods include thermal degreasing, solvent degreasing, catalytic degreasing, etc. It should be noted that if the degreasing effect can be achieved during the sintering process, degreasing may not be performed.

[0100] Optionally, the step of sintering the composite blank to obtain an aluminum alloy-based composite material component comprises:

[0101] Step S31, heating the composite blank to 400-600°C at a rate of 3-6°C / min in an inert atmosphere, and thermally debinding for 1-3 hours to obtain a thermally debinded blank;

[0102] In this embodiment, specifically, the composite blank is placed in a thermal degreasing device, an inert gas is introduced into the thermal degreasing device, and under the protection of the inert gas, the composite blank is heated to 400-600°C, for example, 400°C, 500°C, 600°C, etc., at a rate of 3-6°C / min, for example, 3°C / min, 5°C / min, 6°C / min, etc., so that the composite blank is thermally degreased for 1-3 hours, for example, 1 hour, 2 hours, 3 hours, etc., under the protection of the inert gas and at a high temperature of 400-600°C, so that the binder in the composite blank is removed from the blank by volatilization or decomposition to obtain a thermally degreased blank.

[0103] Step S32, sintering the hot debinded blank in an inert atmosphere at a temperature of 300-650° C. for 3-5 hours, and cooling it to room temperature in the furnace to obtain an aluminum alloy-based composite material component.

[0104] In this embodiment, specifically, the hot debinded blank is placed in a sintering treatment device, an inert gas is introduced into the sintering treatment device, and under the protection of the inert gas, the hot debinded blank is heated to 300-650°C, for example, 300°C, 400°C, 500°C, 650°C, etc., so that the hot debinded blank is sintered for 3-5 hours, for example, 3 hours, 4 hours, 5 hours, etc., under the protection of the inert gas and at a high temperature of 300-650°C, so that the aluminum alloy material adjacent to the high-strength metal insert in the hot debinded blank diffuses into the high-strength metal insert and forms a metal bond with the metal in the high-strength metal insert, thereby making the aluminum alloy matrix part in the hot debinded blank tightly combined with the high-strength metal insert. According to the test, the bonding strength between the aluminum alloy and the high-strength metal insert is greater than 80% of the lower strength of the aluminum alloy or the strength of the high-strength metal insert, that is, the aluminum alloy and the high-strength metal insert can form a metal bond through diffusion to achieve tight bonding. The hot degreased blank is cooled to room temperature in the furnace after sintering to obtain an aluminum alloy-based composite material component, wherein the density of the aluminum alloy-based composite material component is 3.0-6.0 g / cm 3 It is determined by the proportion of the high-strength metal insert and the aluminum alloy matrix in the aluminum alloy-based composite material component. The greater the proportion of the high-strength metal insert, the greater the density, and the smaller the proportion of the high-strength metal insert, the smaller the density.

[0105] It should be noted that the sintering processing equipment and the debinding equipment can be two independent equipment or the same equipment. If the sintering processing equipment and the debinding equipment are the same equipment, after debinding, there is no need to take out the hot debinded blank, and the temperature in the equipment can be adjusted to the sintering processing temperature to continue the sintering process.

[0106] In one feasible method, the aluminum alloy-based composite material component can be further subjected to post-treatment such as shaping, polishing and / or applying lubricating oil, and the obtained aluminum alloy-based composite material component can be subjected to surface processing to reduce surface roughness and / or friction, so as to reduce friction damage to the aluminum alloy-based composite material component during use, thereby improving the wear resistance of the aluminum alloy-based composite material component, and also improving the surface smoothness and aesthetics of the material.

[0107] In this embodiment, an aluminum alloy-based composite material component and a preparation method thereof, and a head-mounted display device are provided. The aluminum alloy-based composite material component is applied to the head-mounted display device. The preparation method of the aluminum alloy-based composite material structure comprises the steps of: preparing an aluminum alloy feed; injecting the aluminum alloy feed into a target mold with a high-strength metal insert placed therein to perform injection molding to obtain a composite blank; and sintering the composite blank to obtain an aluminum alloy-based composite material component. The present application positions a high-strength metal insert with relatively large strength and embeds it in a target mold, performs injection molding of an aluminum alloy matrix portion, and obtains a composite blank formed by the aluminum alloy and the high-strength metal insert. Then, by degreasing and sintering the composite blank, diffusion of the aluminum alloy into the dissimilar metal of the high-strength metal insert is achieved, and aluminum atoms form metal bonds with metal atoms in the high-strength metal insert. Then, by sintering, the aluminum alloy portion in the composite blank and the high-strength metal insert form a dense whole, namely, an aluminum alloy-based composite material component. The portion of the high-strength metal insert in the obtained aluminum alloy-based composite material component can be used for bearing force or contact friction, while the aluminum alloy portion has a lower density, which can effectively reduce the mass of the aluminum alloy-based composite material component and meet the demand for lightweight. Thus, the finally prepared aluminum alloy-based composite material component has the advantages of high strength, lightweight and high wear resistance at the same time, overcoming the technical problem that the components in the head-mounted display device in the prior art are difficult to meet the requirements of lightweight, high strength and high wear resistance at the same time.

[0108] Furthermore, the present invention also provides an aluminum alloy-based composite material component, which is applied to a head-mounted display device. The aluminum alloy-based composite material component is prepared by the above-mentioned method for preparing an aluminum alloy-based composite material component. In one embodiment of the aluminum alloy-based composite material component of the present application, the aluminum alloy-based composite material component comprises:

[0109] an aluminum alloy substrate; and

[0110] At least one load-bearing portion connected to the aluminum alloy substrate;

[0111] Wherein, the load-bearing part is one of a steel load-bearing part and a titanium alloy load-bearing part.

[0112] In this embodiment, it should be noted that the aluminum alloy-based composite material components can be applied to head-mounted display devices that have requirements for lightweight and high strength and high wear resistance. The aluminum alloy-based composite material components include hinges, bearings, rotating shafts, balls, gears and other components that bear both bending moments and torques. These components move frequently during use and have greater requirements for strength and wear resistance. The head-mounted display devices include AR glasses, VR helmets, etc.

[0113] Specifically, the aluminum alloy-based composite material component includes an aluminum alloy matrix, and at least one load-bearing part connected to the aluminum alloy matrix, such as the part of the hinge blade that contacts the pin, the tooth tip part of the gear, the connection point of the rotating shaft, the contact surface of the friction pair, etc. The load-bearing part is one of a steel load-bearing part and a titanium alloy load-bearing part. The load-bearing part used for bearing force in the aluminum alloy-based composite material component is made of steel or titanium alloy. Compared with aluminum alloy, steel or titanium alloy has higher strength and better wear resistance, while the partial density of aluminum alloy is lower, which can effectively reduce the mass of the aluminum alloy-based composite material component and meet the demand for lightweight, so that the finally prepared aluminum alloy-based composite material component has the advantages of high strength, lightweight and high wear resistance at the same time, overcoming the technical problem that the components in the head-mounted display device in the prior art are difficult to meet the requirements of lightweight, high strength and high wear resistance at the same time.

[0114] The aluminum alloy-based composite material component provided by the present application solves the technical problem that the components in the head-mounted display device of the prior art are difficult to simultaneously meet the requirements of light weight, high strength and high wear resistance. Compared with the prior art, the beneficial effects of the aluminum alloy-based composite material component provided by the embodiment of the present invention are the same as the beneficial effects of the preparation method of the aluminum alloy-based composite material component of the above embodiment, which will not be described in detail here.

[0115] Furthermore, the present invention also provides a head-mounted display device, which includes the aluminum alloy-based composite material component as described above.

[0116] In this embodiment, the head-mounted display device includes AR glasses, VR helmets, etc.

[0117] In an operative manner, the head mounted display device is an AR glasses, the aluminum alloy-based composite material component is disposed at the rotation axis position of the AR glasses, and at least part of the aluminum alloy-based composite material component is disposed in the accommodation space formed by the frame and temples of the AR glasses. Figure 2 The aluminum alloy-based composite material component includes two load-bearing parts whose projections overlap in a preset first direction, wherein the preset first direction may be perpendicular to the extension direction of the temple of the AR glasses.

[0118] In an operative manner, the head mounted display device is a VR head mounted display device, and the aluminum alloy-based composite material component is disposed on a flip structure between a main body of the VR head mounted display device and a headband. Exemplarily, the flip structure may include a first aluminum alloy-based composite material component disposed on the main body of the head mounted display device and a second aluminum alloy-based composite material component disposed on the headband, wherein the projection of the load-bearing portion of the first aluminum alloy-based composite material component and the load-bearing portion of the second aluminum alloy-based composite material component in a preset second direction overlap, wherein the preset second direction may be parallel to the main body of the head mounted display device, and the perpendicular midline of the aluminum alloy matrix portion on the first aluminum alloy-based composite material component and the perpendicular midline of the aluminum alloy matrix portion on the second aluminum alloy-based composite material may point to the wearer of the VR head mounted display device.

[0119] The head-mounted display device provided by the present application solves the technical problem that the components in the head-mounted display device of the prior art are difficult to simultaneously meet the requirements of light weight, high strength and high wear resistance. Compared with the prior art, the beneficial effects of the head-mounted display device provided by the embodiment of the present invention are the same as the beneficial effects of the aluminum alloy-based composite material components of the above-mentioned embodiment, which will not be repeated here.

[0120] In order to further understand the present application, the aluminum alloy-based composite material component and its preparation method, head-mounted display device and application provided by the present application are specifically described below in combination with the embodiments. The embodiments of the present invention all use commercially available raw materials.

[0121] Example 1

[0122] Material and parts design: Cylindrical 17-4 stainless steel parts are selected as the main force-bearing and wear-resistant parts, and aluminum alloy matrix parts use aluminum silicon alloy as the raw material for preparing aluminum alloy feed.

[0123] Powder injection molding: 17-4 stainless steel parts are positioned and embedded in the target mold as high-strength metal inserts. Polyethylene glycol, polymethyl methacrylate and stearic acid are measured according to the volume of polyethylene glycol: the volume of polymethyl methacrylate: the volume of stearic acid = 75:23:2, and mixed to obtain a binder. Aluminum silicon alloy powder with a D90 of 35 μm and the binder are loaded into an internal mixer at a volume ratio of 70:30 and filled with argon gas. The mixture is mixed at a temperature of 170°C and a speed of 40 r / min for 2 hours and granulated to obtain an aluminum alloy feed. The aluminum alloy feed is injected into the target mold embedded with the 17-4 stainless steel parts through a powder injection molding device to obtain a composite blank, wherein the injection parameters are: mold temperature 40°C, nozzle temperature 190°C, injection pressure 1500 bar, holding pressure 1000 bar, and cooling time 6 s.

[0124] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 600℃ at 5℃ / min, and hot debinding was performed for 2 hours to obtain a hot debinding blank; the temperature was adjusted to 450℃, and pressure-maintained sintering treatment was performed for 5 hours, and then the aluminum alloy-based composite material component was obtained by cooling to room temperature with the furnace. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 3 As shown, the top view of the aluminum alloy matrix composite material component is as shown Figure 4 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.

[0125] Test: The aluminum alloy matrix composite component prepared in Example 1 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-steel composite interface was 255 MPa, the bulk strength of the aluminum alloy matrix was 336 MPa, and the overall density of the aluminum alloy matrix composite component was 3.1 g / cm 3 , see Table 1 for details.

[0126] Example 2

[0127] Materials and parts design: 17-4 stainless steel parts are selected as the main force-bearing and wear-resistant parts, and 6063 aluminum alloy is selected as the raw material for preparing aluminum alloy feed.

[0128] Powder injection molding: 17-4 stainless steel parts are positioned and embedded in the target mold as high-strength metal inserts. Polyethylene glycol, polymethyl methacrylate and stearic acid are measured according to the volume of polyethylene glycol: the volume of polymethyl methacrylate: the volume of stearic acid = 65:30:5, and mixed to obtain a binder. 6063 aluminum alloy powder with a D90 of 38 μm and the binder are loaded into an internal mixer at a volume ratio of 85:15 and filled with argon gas. The mixture is mixed at a temperature of 140°C and a speed of 30 r / min for 4 hours and granulated to obtain an aluminum alloy feed. The aluminum alloy feed is injected into the target mold embedded with the 17-4 stainless steel parts through a powder injection molding device to obtain a composite blank, wherein the injection parameters are: mold temperature 35°C, nozzle temperature 220°C, injection pressure 1600 bar, holding pressure 1200 bar, and cooling time 12 s.

[0129] Debinding sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 400°C at 6°C / min, and thermal debinding was performed for 1 hour to obtain a thermally debinded blank; the temperature was adjusted to 300°C, and pressure-maintained sintering treatment was performed for 4 hours, and then the blank was cooled to room temperature with the furnace to obtain an aluminum alloy-based composite material component. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 5 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.

[0130] Test: The aluminum alloy matrix composite component prepared in Example 2 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-steel composite interface was 265 MPa, the bulk strength of the aluminum alloy matrix was 336 MPa, and the overall density of the aluminum alloy matrix composite component was 4.1 g / cm 3 , see Table 1 for details.

[0131] Example 3

[0132] Materials and parts design: Powder injection molded 17-4 stainless steel parts are selected as the main force-bearing and wear-resistant parts, stamping formed 7050 aluminum alloy plates are selected as aluminum alloy inserts, and the aluminum alloy matrix part uses 7050 aluminum alloy as the raw material for preparing aluminum alloy feed.

[0133] Powder injection molding: 17-4 stainless steel parts are used as high-strength metal inserts, and 7050 aluminum alloy plates are used as aluminum alloy inserts, which are positioned and embedded in the target mold respectively. According to the volume of polyethylene glycol: the volume of polymethyl methacrylate: the volume of stearic acid = 85:14:1, polyethylene glycol, polymethyl methacrylate and stearic acid are measured and mixed to obtain a binder. Aluminum silicon alloy powder with a D90 of 40 μm and the binder are loaded into an internal mixer at a volume ratio of 65:35 and filled with argon gas. The mixture is mixed at a temperature of 220° C. and a speed of 50 r / min for 1 hour and granulated to obtain an aluminum alloy feed. The aluminum alloy feed is injected into the target mold embedded with the 17-4 stainless steel parts through a powder injection molding device to obtain a composite blank, wherein the injection parameters are: mold temperature 45° C., nozzle temperature 160° C., injection pressure 1200 bar, holding pressure 800 bar, and cooling time 4 s.

[0134] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 500°C at 3°C / min, and thermal debinding was performed for 3 hours to obtain a thermally debinded blank; the temperature was adjusted to 650°C, and pressure-maintained sintering treatment was performed for 3 hours, and then the blank was cooled to room temperature with the furnace to obtain an aluminum alloy-based composite material component. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 6 As shown, the aluminum alloy matrix 10 and the high-strength metal insert 20 are tightly bonded via a metal bond, and the aluminum alloy matrix 10 and the aluminum alloy insert 30 are also tightly bonded via a metal bond, so that the high-strength metal insert 20 and the aluminum alloy insert 30 are connected as a whole through the aluminum alloy matrix 10.

[0135] Test: The aluminum alloy matrix composite component prepared in Example 3 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-steel composite interface was 365 MPa, the bulk strength of the aluminum alloy matrix and the aluminum alloy insert was 460 MPa, and the overall density of the aluminum alloy matrix composite component was 4.8 g / cm 3 , see Table 1 for details.

[0136] Example 4

[0137] Material and parts design: Cylindrical TC4 titanium alloy parts are selected as the main force-bearing and wear-resistant parts, and aluminum alloy matrix parts use aluminum silicon alloy as the raw material for preparing aluminum alloy feed.

[0138] Powder injection molding: The TC4 titanium alloy part is positioned and embedded in the target mold as a high-strength metal insert. Polyethylene glycol, polymethyl methacrylate and stearic acid are measured according to the volume of polyethylene glycol: the volume of polymethyl methacrylate: the volume of stearic acid = 75:23:2, and a binder is obtained by mixing. The aluminum silicon alloy powder with a D90 of 35 μm and the binder are loaded into an internal mixer at a volume ratio of 70:30 and filled with argon gas. The mixture is mixed at a temperature of 170°C and a speed of 40 r / min for 2 hours and granulated to obtain an aluminum alloy feed. The aluminum alloy feed is injected into the target mold embedded with the TC4 titanium alloy part through a powder injection molding device to obtain a composite blank, wherein the injection parameters are: mold temperature 40°C, nozzle temperature 190°C, injection pressure 1500 bar, holding pressure 1000 bar, and cooling time 6s.

[0139] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 600℃ at 5℃ / min, and hot debinding was performed for 2 hours to obtain a hot debinding blank; the temperature was adjusted to 450℃, and pressure-maintained sintering treatment was performed for 5 hours, and then the aluminum alloy-based composite material component was obtained by cooling to room temperature with the furnace. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 3 As shown, the top view of the aluminum alloy matrix composite material component is as shown Figure 4 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.

[0140] Test: The aluminum alloy matrix composite component prepared in Example 1 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-titanium composite interface was 255 MPa, the bulk strength of the aluminum alloy matrix was 336 MPa, and the overall density of the aluminum alloy matrix composite component was 3.1 g / cm 3 , see Table 1 for details.

[0141] Example 5

[0142] Material and parts design: TC4 titanium alloy parts are selected as the main force-bearing and wear-resistant parts, and 6063 aluminum alloy is selected as the raw material for preparing aluminum alloy feed.

[0143] Powder injection molding: The TC4 titanium alloy part is positioned and embedded in the target mold as a high-strength metal insert. According to the volume of polyethylene glycol: the volume of polymethyl methacrylate: the volume of stearic acid = 65:30:5, polyethylene glycol, polymethyl methacrylate and stearic acid are measured and mixed to obtain a binder. The 6063 aluminum alloy powder with a D90 of 38 μm and the binder are loaded into an internal mixer at a volume ratio of 85:15 and filled with argon gas. The mixture is mixed at a temperature of 140°C and a speed of 30 r / min for 4 hours and granulated to obtain an aluminum alloy feed. The aluminum alloy feed is injected into the target mold embedded with the TC4 titanium alloy part through a powder injection molding device to obtain a composite blank, wherein the injection parameters are: mold temperature 35°C, nozzle temperature 220°C, injection pressure 1600 bar, holding pressure 1200 bar, and cooling time 12 s.

[0144] Debinding sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 400°C at 6°C / min, and thermal debinding was performed for 1 hour to obtain a thermally debinded blank; the temperature was adjusted to 300°C, and pressure-maintained sintering treatment was performed for 4 hours, and then the blank was cooled to room temperature with the furnace to obtain an aluminum alloy-based composite material component. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 5 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.

[0145] Test: The aluminum alloy matrix composite component prepared in Example 2 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-titanium composite interface was 255 MPa, the bulk strength of the aluminum alloy matrix was 306 MPa, and the overall density of the aluminum alloy matrix composite component was 3.2 g / cm 3 , see Table 1 for details.

[0146] Example 6

[0147] Materials and parts design: TC4 titanium alloy parts made by powder injection molding are selected as the main force-bearing and wear-resistant parts, 7050 aluminum alloy plates made by stamping are selected as aluminum alloy inserts, and 7050 aluminum alloy is selected as the raw material for preparing aluminum alloy feed for the aluminum alloy matrix.

[0148] Powder injection molding: TC4 titanium alloy parts are used as high-strength metal inserts, and 7050 aluminum alloy plates are used as aluminum alloy inserts, which are positioned and embedded in the target mold respectively. According to the volume of polyethylene glycol: the volume of polymethyl methacrylate: the volume of stearic acid = 85:14:1, polyethylene glycol, polymethyl methacrylate and stearic acid are measured and mixed to obtain a binder. Aluminum silicon alloy powder with a D90 of 40 μm and the binder are loaded into an internal mixer at a volume ratio of 65:35 and filled with argon gas. The mixture is mixed at a temperature of 220° C. and a speed of 50 r / min for 1 hour and granulated to obtain an aluminum alloy feed. The aluminum alloy feed is injected into the target mold embedded with the TC4 titanium alloy parts through a powder injection molding device to obtain a composite blank, wherein the injection parameters are: mold temperature 45° C., nozzle temperature 160° C., injection pressure 1200 bar, holding pressure 800 bar, and cooling time 4 s.

[0149] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 500°C at 3°C / min, and thermal debinding was performed for 3 hours to obtain a thermally debinded blank; the temperature was adjusted to 650°C, and pressure-maintained sintering treatment was performed for 3 hours, and then the blank was cooled to room temperature with the furnace to obtain an aluminum alloy-based composite material component. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 6 As shown, the aluminum alloy matrix 10 and the high-strength metal insert 20 are tightly bonded via a metal bond, and the aluminum alloy matrix 10 and the aluminum alloy insert 30 are also tightly bonded via a metal bond, so that the high-strength metal insert 20 and the aluminum alloy insert 30 are connected as a whole through the aluminum alloy matrix 10.

[0150] Test: The aluminum alloy matrix composite component prepared in Example 3 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-titanium composite interface was 365 MPa, the bulk strength of the aluminum alloy matrix and the aluminum alloy insert was 450 MPa, and the overall density of the aluminum alloy matrix composite component was 3.8 g / cm 3 , see Table 1 for details.

[0151] Comparative Example 1

[0152] Material and part design: 17-4 stainless steel powder was used to prepare the stainless steel test specimens.

[0153] Powder injection molding: polyethylene glycol, polymethyl methacrylate and stearic acid are measured and mixed to obtain a binder according to the ratio of polyethylene glycol volume: polymethyl methacrylate volume: stearic acid volume = 75:23:2, 17-4 stainless steel powder with a D90 of 40 μm and the binder are charged into an internal mixer at a volume ratio of 70:30 and filled with argon gas, mixed at a temperature of 170° C. and a speed of 40 r / min for 2 hours and granulated to obtain a stainless steel feed; the stainless steel feed is injected into a target mold through a powder injection molding device to obtain a stainless steel blank, wherein the injection parameters are: mold temperature 40° C., nozzle temperature 190° C., injection pressure 1500 bar, holding pressure 1000 bar, and cooling time 6 s.

[0154] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 600°C at a rate of 5°C / min, and hot debinding was performed for 2 hours to obtain a hot debinded blank; the temperature was adjusted to 1200°C, and after pressure-maintaining sintering treatment for 3 hours, the stainless steel test sample was obtained by cooling with the furnace to room temperature.

[0155] Test: The stainless steel test sample prepared in the comparative example of the present invention was subjected to a tensile test. The stainless steel test sample was subjected to a tensile test according to GB / T228.1-2010, and the tensile strength was measured to be 1033 MPa and the density was 7.7 g / cm 3 , see Table 1 for details.

[0156] Comparative Example 2

[0157] Material and part design: TC4 titanium alloy powder was used to prepare titanium alloy test samples.

[0158] Powder injection molding: polyethylene glycol, polymethyl methacrylate and stearic acid are measured according to the volume of polyethylene glycol: the volume of polymethyl methacrylate: the volume of stearic acid = 75:23:2, and mixed to obtain a binder. TC4 titanium alloy powder with a D90 of 40 μm and the binder are loaded into an internal mixer at a volume ratio of 70:30 and filled with argon gas. The mixture is mixed at a temperature of 170°C and a speed of 40 r / min for 2 hours and granulated to obtain a titanium alloy feed. The titanium alloy feed is injected into a target mold through a powder injection molding device to obtain a titanium alloy billet, wherein the injection parameters are: mold temperature 40°C, nozzle temperature 190°C, injection pressure 1500 bar, holding pressure 1000 bar, and cooling time 6 s.

[0159] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 600°C at 5°C / min, and hot debinding was performed for 2 hours to obtain a hot debinded blank; the temperature was adjusted to 1200°C, and after pressure-maintaining sintering treatment for 3 hours, the titanium alloy test sample was obtained by cooling with the furnace to room temperature.

[0160] Test: The titanium alloy test sample prepared in the comparative example of the present invention was subjected to a tensile test. The titanium alloy test sample was subjected to a tensile test according to GB / T228.1-2010, and the tensile strength was measured to be 853 MPa and the density was 4.4 g / cm 3 , see Table 1 for details.

[0161] Table 1 Performance indexes of composite materials prepared in the embodiments of the present invention

[0162]

[0163] As can be seen from Table 1, compared with the strength of the aluminum alloy matrix, the strength of the high-strength metal insert is higher, so the bearing capacity of the high-strength metal insert is higher, and the wear resistance when rubbing on the surface of the high-strength metal insert is higher than the wear resistance when rubbing on the surface of the aluminum alloy matrix, and compared with the stainless steel sample or the titanium alloy sample, the density of the aluminum alloy-based composite material component is smaller, and the prepared aluminum alloy-based composite material component has the advantages of high strength, light weight and high wear resistance. It should be noted that although the density of the aluminum alloy-based composite material component prepared in Example 3 is higher than the density of the titanium alloy test sample, the cost of titanium alloy is relatively high. In low-cost products, aluminum alloy-based composite material components of aluminum-steel composites with a density similar to that of titanium alloy can be prepared to meet the requirements of low cost, high strength, light weight and high wear resistance at the same time.

[0164] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent processing scope of the present application.

Claims

1. A method for preparing an aluminum alloy-based composite material component, It is characterized in that The aluminum alloy-based composite material component is applied to a head mounted display device, and the preparation method of the aluminum alloy-based composite material component comprises the following steps: preparing aluminum alloy feedstock; Injecting the aluminum alloy feed into a target mold with a high-strength metal insert for injection molding to obtain a composite blank; The composite blank is sintered to obtain an aluminum alloy-based composite material component.

2. The method for preparing the aluminum alloy-based composite material component according to claim 1, It is characterized in that The step of injecting the aluminum alloy feed into a target mold with a high-strength metal insert for injection molding to obtain a composite blank comprises: The aluminum alloy feed is injected into a target mold with a high-strength metal insert, the injection temperature is controlled to be 160-220° C., the injection pressure is 1200-1600 bar, the mold temperature is 35° C.-45° C., the pressure is maintained at 800-1200 bar, and the composite blank is obtained by cooling for 4s-12s.

3. The method for preparing the aluminum alloy-based composite material component according to claim 1, It is characterized in that The step of injecting the aluminum alloy feed into a target mold with a high-strength metal insert for injection molding to obtain a composite blank comprises: Obtaining an aluminum alloy insert, and placing the aluminum alloy insert in the target mold; The aluminum alloy feedstock is injected into a target mold where a high-strength metal insert and an aluminum alloy insert are placed for injection molding, so that the high-strength metal insert and the aluminum alloy insert are connected by the aluminum alloy feedstock to obtain a composite blank.

4. The method for preparing the aluminum alloy-based composite material component according to claim 1, It is characterized in that The step of preparing the aluminum alloy feed comprises: mixing aluminum alloy powder with a binder to obtain an aluminum alloy mixture; The aluminum alloy mixture is heated, mixed and granulated to obtain an aluminum alloy feedstock.

5. The method for preparing the aluminum alloy-based composite material component according to claim 4, It is characterized in that The volume proportion of the binder in the aluminum alloy mixture is 15-35%.

6. The method for preparing the aluminum alloy-based composite material component according to claim 4, It is characterized in that The binder comprises polyethylene glycol, polymethyl methacrylate and stearic acid, wherein the volume proportion of the polyethylene glycol in the binder is 65-85%, the volume proportion of the polymethyl methacrylate in the binder is 14-30%, and the volume proportion of the stearic acid in the binder is 1-5%; And / or, the aluminum alloy powder includes spherical aluminum alloy powder, D50 of the spherical aluminum alloy powder is less than 45 μm, and D90 of the spherical aluminum alloy powder is 35-40 μm.

7. The method for preparing the aluminum alloy-based composite material component according to claim 4, It is characterized in that The temperature of the heating and mixing is 140-220° C., the rotation speed of the heating and mixing is 30-50 r / min, and the time of the heating and mixing is 1-4 h.

8. The method for preparing the aluminum alloy-based composite material component according to claim 1, It is characterized in that The step of sintering the composite blank to obtain an aluminum alloy-based composite material component comprises: The composite blank is heated to 400-600° C. at a rate of 3-6° C. / min in an inert atmosphere, and thermally degreased for 1-3 hours to obtain a thermally degreased blank; The hot degreased blank is sintered in an inert atmosphere at a temperature of 300-650° C. for 3-5 hours, and then cooled to room temperature in the furnace to obtain an aluminum alloy-based composite material component.

9. A method for preparing an aluminum alloy-based composite material component according to any one of claims 1 to 8, It is characterized in that The strength of the high-strength metal insert is greater than 900 MPa, and the Vickers hardness is greater than 350. The strength of the raw aluminum alloy used to prepare the aluminum alloy feed is greater than 200 MPa.

10. A method for preparing an aluminum alloy-based composite material component according to any one of claims 1 to 8, It is characterized in that The high-strength metal insert is one of a steel insert and a titanium alloy insert.

11. The method for preparing the aluminum alloy-based composite material component according to claim 10, It is characterized in that When the high-strength metal insert is a steel insert, the density of the aluminum alloy-based composite material component is 3.0 to 6.0 g / cm 3 ; When the high-strength metal insert is a titanium alloy insert, the density of the aluminum alloy-based composite material component is 2.8 to 4.0 g / cm 3 .

12. An aluminum alloy-based composite material component, It is characterized in that The aluminum alloy-based composite material component is applied to a head mounted display device, and the aluminum alloy-based composite material component is prepared by the method for preparing an aluminum alloy-based composite material component according to any one of claims 1 to 11, and the aluminum alloy-based composite material component comprises: an aluminum alloy substrate; and At least one load-bearing portion connected to the aluminum alloy substrate; Wherein, the load-bearing part is one of a steel load-bearing part and a titanium alloy load-bearing part.

13. A head mounted display device, It is characterized in that The head-mounted display device comprises the aluminum alloy-based composite material component as claimed in claim 12.

14. The head mounted display device according to claim 13, It is characterized in that The head mounted display device is glasses, and the aluminum alloy based composite material component is arranged at the rotation axis position of the glasses, or, The head mounted display device is a VR head mounted display device, and the aluminum alloy based composite material component is arranged at a flip structure between a main body and a headband of the VR head mounted display device.