Aluminum alloy matrix composite component and preparation method thereof
By using the preparation method of aluminum alloy-based composite material components in the head-mounted display device, the sintering treatment of high-strength metal inserts and aluminum alloy substrates is used to form a dense structure, which solves the lightweight, high strength and high level of the equipment components Wear resistance issues.
Patent Information
- Application Number
- CN202310647222.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
It is difficult for components in head-mounted display devices to meet the requirements of lightweight, high strength and high wear resistance at the same time.
Using the preparation method of aluminum alloy-based composite material components, aluminium alloy bases are obtained, and a matching insertion part is processed on the aluminum alloy bases, and the high-strength metal inserts are installed and sintered to achieve aluminum. The heterogeneous metal diffusion and metal bonds are formed between the alloy substrate and the high-strength metal insert to form a dense overall structure.
The aluminum alloy-based composite components have high strength, lightweight and high wear resistance, and overcome the difficulty of components in the prior art to meet the requirements of lightweight, high strength and high wear resistance at the same time.
Smart Images

Figure CN119062659A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal composite materials, and in particular to an aluminum alloy-based composite material component and a preparation method thereof. Background Art
[0002] With the development of 5G (5th Generation Mobile Communication Technology), blockchain, cloud computing, and next-generation Internet technologies, electronic products such as mobile phones, tablets, laptops, AR (Augmented Reality) / VR (Virtual Reality) devices are moving towards lightweight and portable miniaturization. Metal precision components, as important components of consumer electronic products, have achieved great development, especially head-mounted display devices represented by AR / VR devices, which have higher requirements for lightweight and user experience. The human head is very sensitive to the weight of wearable products. Overweight products will make consumers feel uncomfortable and reduce comfort. Therefore, structural weight reduction is an important development direction to improve customer experience. Due to their complex structure and small size, the various components in head-mounted display devices have high requirements for strength and wear resistance in addition to lightweight requirements. For example, precision hardware such as AR glasses shafts will experience repeated folding when worn, and may be folded more than 50,000 times during their entire life cycle. Therefore, shaft-type components have high strength and high wear resistance requirements to prevent damage during wearing or folding.
[0003] However, it is currently difficult for components in head-mounted display devices to simultaneously meet the requirements of light weight, high strength, and high wear resistance. Summary of the invention
[0004] The main purpose of the present application is to provide an aluminum alloy-based composite material component and a preparation method thereof, aiming to solve the technical problem that components in the prior art head-mounted display device are difficult to simultaneously meet the requirements of light weight, high strength and high wear resistance.
[0005] To achieve the above object, the present application provides a method for preparing an aluminum alloy-based composite material component, wherein the aluminum alloy-based composite material component is applied to a head-mounted display device, and the method for preparing the aluminum alloy-based composite material component comprises the following steps:
[0006] Obtaining a high-strength metal insert and an aluminum alloy base member, wherein an embedding portion matching the high-strength metal insert is processed on the aluminum alloy base member;
[0007] installing the high-strength metal insert in the embedding portion to obtain a composite component;
[0008] The composite component is sintered to obtain an aluminum alloy-based composite material component.
[0009] Optionally, the step of installing the high-strength metal insert in the embedding portion to obtain a composite component includes:
[0010] The high-strength metal insert is interference-fitted into the embedded portion to obtain a composite component.
[0011] Optionally, the interference fit has an interference amount of 1-200 μm.
[0012] Optionally, before the step of installing the high-strength metal insert in the embedding portion to obtain the composite component, the step further includes:
[0013] The high-strength metal insert and the contact surface on the aluminum alloy base are subjected to surface cleaning and surface roughening treatments.
[0014] Optionally, the surface roughness Ra of the contact surface on the high-strength metal insert and the aluminum alloy base is 10-1000.
[0015] Optionally, before the step of obtaining the aluminum alloy base member, the method further includes:
[0016] Obtaining a target mold and an aluminum alloy feed, wherein the target mold is provided with a protrusion structure, and the protrusion structure is used to form an embedding portion matching the high-strength metal insert on the aluminum alloy base member during the forming process of the aluminum alloy base member;
[0017] The aluminum alloy feedstock is injected into the target mold to obtain an aluminum alloy base part.
[0018] Optionally, the step of injecting the aluminum alloy feedstock into the target mold to obtain the aluminum alloy base member comprises:
[0019] The aluminum alloy feed is injected into the target mold, the injection temperature is controlled to be 160-220° C., the injection pressure is 1200-1600 bar, the mold temperature is 35° C.-45° C., the pressure is maintained at 800-1200 bar, and the mold is cooled for 4s-12s to obtain an aluminum alloy base part.
[0020] Optionally, the step of sintering the composite assembly to obtain an aluminum alloy-based composite material component comprises:
[0021] The composite component is heated to 400-600° C. at a rate of 3-6° C. / min in an inert atmosphere, and thermally degreased for 1-3 hours to obtain a thermally degreased blank;
[0022] The hot degreased blank is sintered in an inert atmosphere at a temperature of 300-650° C. for 3-5 hours, and then cooled to room temperature in the furnace to obtain an aluminum alloy-based composite material component.
[0023] Optionally, the high-strength metal insert has a strength greater than 900 MPa and a Vickers hardness greater than 350, and the strength of the aluminum alloy base component is greater than 200 MPa.
[0024] Optionally, the high-strength metal insert is one of a steel insert and a titanium alloy insert.
[0025] Optionally, when the high-strength metal insert is a steel insert, the density of the aluminum alloy-based composite material component is 3.0 to 6.0 g / cm3;
[0026] When the high-strength metal insert is a titanium alloy insert, the density of the aluminum alloy-based composite material component is 2.8 to 4.0 g / cm3.
[0027] The present application also provides an aluminum alloy-based composite material component, which is applied to a head-mounted display device. The aluminum alloy-based composite material component is prepared by the above-mentioned method for preparing an aluminum alloy-based composite material component, and the aluminum alloy-based composite material component comprises:
[0028] an aluminum alloy substrate; and
[0029] At least one load-bearing portion connected to the aluminum alloy substrate;
[0030] Wherein, the load-bearing part is one of a steel load-bearing part and a titanium alloy load-bearing part.
[0031] The present application also provides a head-mounted display device, which includes the aluminum alloy-based composite material component as described above.
[0032] Optionally, the head mounted display device is a pair of glasses, and the aluminum alloy based composite material component is arranged at a rotation axis position of the glasses, or,
[0033] The head-mounted display device is a VR helmet, and the aluminum alloy-based composite material component is arranged at a flip structure between a main body and a headband of the VR helmet.
[0034] The present application provides an aluminum alloy-based composite material component and a preparation method thereof, wherein the aluminum alloy-based composite material component is applied to a head-mounted display device, and the preparation method of the aluminum alloy-based composite material component comprises the steps of: obtaining a high-strength metal insert and an aluminum alloy base component, wherein an embedding portion matching the high-strength metal insert is processed on the aluminum alloy base component; installing the high-strength metal insert on the embedding portion to obtain a composite component; and sintering the composite component to obtain the aluminum alloy-based composite material component. The present application obtains a composite component formed by the aluminum alloy base and the high-strength metal insert by installing a high-strength metal insert with relatively large strength into an aluminum alloy base with relatively small density, and then the composite component is degreased and sintered to achieve diffusion of dissimilar metals between the aluminum alloy base and the high-strength metal insert, so that aluminum atoms form metal bonds with metal atoms in the high-strength metal insert, and then the aluminum alloy part in the composite component and the high-strength metal insert form a dense whole through sintering, namely, an aluminum alloy-based composite material component. The high-strength metal insert part in the obtained aluminum alloy-based composite material component can be used for load bearing or contact friction, while the aluminum alloy part has a relatively low density, which can effectively reduce the mass of the aluminum alloy-based composite material component and meet the demand for lightweight, so that the finally prepared aluminum alloy-based composite material component has the advantages of high strength, lightweight and high wear resistance at the same time, overcoming the technical problem that the components in the head-mounted display device in the prior art are difficult to meet the requirements of lightweight, high strength and high wear resistance at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0037] Figure 1 A schematic diagram of a process of an embodiment of a method for preparing an aluminum alloy-based composite material component of the present application;
[0038] Figure 2 A stress diagram of an example of an aluminum alloy-based composite material component sample in this application;
[0039] Figure 3 A side cross-sectional view of an aluminum alloy-based composite material component prepared in one embodiment of the present application;
[0040] Figure 4A top view of an aluminum alloy-based composite material component prepared in one embodiment of the present application;
[0041] Figure 5 A side cross-sectional view of an aluminum alloy-based composite component prepared according to another embodiment of the present application.
[0042] Description of Figure Numbers:
[0043] Label name Label name 10 Aluminum alloy substrate 20 High strength metal inserts 40 Load-bearing department
[0044] The purpose, features and advantages of this application will be further described in conjunction with the embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0045] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0046] With the development of 5G (5th Generation Mobile Communication Technology), blockchain, cloud computing, and next-generation Internet technologies, electronic products such as mobile phones, tablets, laptops, AR (Augmented Reality) / VR (Virtual Reality) devices are moving towards lightweight and portable miniaturization. Metal precision components, as important components of consumer electronic products, have achieved great development, especially head-mounted display devices represented by AR / VR devices, which have higher requirements for lightweight and user experience. The human head is very sensitive to the weight of wearable products. Overweight products will make consumers feel uncomfortable and reduce comfort. Therefore, structural weight reduction is an important development direction to improve customer experience. Due to their complex structure and small size, the various components in head-mounted display devices have high requirements for strength and wear resistance in addition to lightweight requirements. For example, precision hardware such as AR glasses shafts will experience repeated folding when worn, and may be folded more than 50,000 times during their entire life cycle. Therefore, shaft-type components have high strength and high wear resistance requirements to prevent damage during wearing or folding.
[0047] Steel has high strength, which can reach more than 1500MPa, good wear resistance, low cost and abundant output. It is very suitable for making small precision hardware such as mobile phone card trays, ejectors, gear precision shafts, etc. However, the density of steel is about 7.8g / cm3 , it is not suitable for smart wearable products that have a strong demand for lightweight; titanium alloy has certain lightweight advantages over steel, but titanium alloy is more expensive and more difficult to process.
[0048] For lightweight, aluminum alloy is currently used, and the density of aluminum alloy is 2.7g / cm 3 , which is particularly beneficial for lightweighting and can also meet the requirements of general loads. However, due to the low strength and poor wear resistance of aluminum alloys, it can generally only be used as a shell material and cannot meet the wear resistance requirements of small precision hardware on smart wearable products. It is not suitable for making small precision hardware such as precision shafts. In order to improve the wear resistance of aluminum, a wear-resistant coating can be formed on the surface of the aluminum alloy, such as anodized coating, micro-arc oxidation coating, electroplating layer, magnetron sputtering layer, etc., to enhance the wear resistance of the aluminum alloy. However, the matrix of the aluminum alloy is relatively soft, and the coating is easy to fall off, and it is still difficult to meet the wear resistance requirements. That is, it is difficult for the components in the current head-mounted display device to simultaneously meet the requirements of lightweight, high strength and high wear resistance.
[0049] In this regard, the present application provides an aluminum alloy-based composite material component and a method for preparing the same, comprising the steps of: obtaining a high-strength metal insert and an aluminum alloy base, wherein the aluminum alloy base is processed with an embedded portion that matches the high-strength metal insert; installing the high-strength metal insert in the embedded portion to obtain a composite component; and sintering the composite component to obtain an aluminum alloy-based composite material component. The present application obtains a composite component formed by the aluminum alloy base and the high-strength metal insert by installing a high-strength metal insert with relatively large strength into an aluminum alloy base with relatively small density, and then the composite component is degreased and sintered to achieve diffusion of dissimilar metals between the aluminum alloy base and the high-strength metal insert, so that aluminum atoms form metal bonds with metal atoms in the high-strength metal insert, and then the aluminum alloy part in the composite component and the high-strength metal insert form a dense whole through sintering, namely, an aluminum alloy-based composite material component. The high-strength metal insert part in the obtained aluminum alloy-based composite material component can be used for load bearing or contact friction, while the aluminum alloy part has a relatively low density, which can effectively reduce the mass of the aluminum alloy-based composite material component and meet the demand for lightweight, so that the finally prepared aluminum alloy-based composite material component has the advantages of high strength, lightweight and high wear resistance at the same time, overcoming the technical problem that the components in the head-mounted display device in the prior art are difficult to meet the requirements of lightweight, high strength and high wear resistance at the same time.
[0050] The present application provides a method for preparing an aluminum alloy-based composite material component. In one embodiment of the method for preparing an aluminum alloy-based composite material component of the present application, referring to Figure 1 , the preparation method of the aluminum alloy-based composite material component comprises:
[0051] Step S10, obtaining a high-strength metal insert and an aluminum alloy base member, wherein an embedding portion matching the high-strength metal insert is processed on the aluminum alloy base member;
[0052] In this embodiment, it should be noted that the aluminum alloy-based composite material component prepared in this embodiment can be applied to head-mounted display devices that have requirements for lightweight and high strength and high wear resistance. The aluminum alloy-based composite material components include hinges, bearings, rotating shafts, balls, gears and other components that bear both bending moments and torques. These components move frequently during use and have greater requirements for strength and wear resistance. The head-mounted display devices include AR glasses, VR helmets, etc.
[0053] In an operative manner, the head mounted display device is an AR glasses, the aluminum alloy-based composite material component is disposed at the rotation axis position of the AR glasses, and at least part of the aluminum alloy-based composite material component is disposed in the accommodation space formed by the frame and temples of the AR glasses. Figure 2 The aluminum alloy-based composite material component includes two load-bearing parts whose projections overlap in a preset first direction, wherein the preset first direction may be perpendicular to the extension direction of the temple of the AR glasses.
[0054] In an operative manner, the head mounted display device is a VR head mounted display device, and the aluminum alloy-based composite material component is disposed on a flip structure between a main body of the VR head mounted display device and a headband. Exemplarily, the flip structure may include a first aluminum alloy-based composite material component disposed on the main body of the head mounted display device and a second aluminum alloy-based composite material component disposed on the headband, wherein the projection of the load-bearing portion of the first aluminum alloy-based composite material component and the load-bearing portion of the second aluminum alloy-based composite material component in a preset second direction overlap, wherein the preset second direction may be parallel to the main body of the head mounted display device, and the perpendicular midline of the aluminum alloy matrix portion on the first aluminum alloy-based composite material component and the perpendicular midline of the aluminum alloy matrix portion on the second aluminum alloy-based composite material may point to the wearer of the VR head mounted display device.
[0055] The high-strength metal insert refers to a metal insert with a strength higher than that of an aluminum alloy material, and can be prepared in advance by powder injection molding, stamping molding, forging, 3D printing and other processes according to the actual requirements of the strength, structure, shape and other actual requirements of the load-bearing or wear-resistant parts of the aluminum alloy-based composite material component to be prepared. This is not limited in this embodiment. The material of the high-strength metal insert can be steel, titanium alloy, etc. The specific process conditions of injection molding can be tested, designed and adjusted according to actual conditions, and this is not limited in this embodiment.
[0056] The aluminum alloy base part refers to a basic structural part made of aluminum alloy. Its specific material, structure, shape, etc. can be determined in advance according to the actual needs of the aluminum alloy-based composite material component to be prepared, and can be prepared by powder injection molding, stamping molding, forging, 3D printing and other processes. In an practicable manner, the aluminum alloy base part can be made by powder injection molding. The powder injection molding process has a mature process, a complete industrial chain, can be mass-produced, and has low cost, which is conducive to the mass production and cost reduction and efficiency improvement of aluminum alloy-based composite material components.
[0057] Specifically, the high-strength metal inserts and aluminum alloy base parts can be designed and processed in advance according to the actual needs of the aluminum alloy-based composite material components to be prepared, wherein the aluminum alloy base part should be processed with an embedding portion that matches the specifications and shape of the high-strength metal insert, so that the high-strength metal insert can be installed in the embedding portion and can fit with a partial area of the surface of the aluminum alloy base part. Furthermore, when the aluminum alloy-based composite material components are actually processed, the prepared high-strength metal inserts and aluminum alloy base parts can be directly obtained.
[0058] Optionally, before the step of obtaining the aluminum alloy base member, the method further includes:
[0059] Step A10, obtaining a target mold and an aluminum alloy feed, wherein the target mold is provided with a protruding structure, and the protruding structure is used to form an embedded portion matching the high-strength metal insert on the aluminum alloy base member during the forming process of the aluminum alloy base member;
[0060] In the present embodiment, it should be noted that the target mold refers to an injection molding mold for preparing an aluminum alloy base member. The target mold can be designed and processed according to the aluminum alloy-based composite material to be prepared. A protruding structure can be set at the installation position corresponding to the high-strength metal insert in the target mold. The protruding structure is used to form an embedded part matching the high-strength metal insert on the aluminum alloy base member during the molding process of the aluminum alloy base member. The embedded part can be a through hole structure, a non-through recessed structure, a vacant structure located at the edge, etc.; the aluminum alloy feed is a feed made of aluminum alloy material as a raw material, adding additives such as a binder, and mixing and granulating. The binder includes one or more of polyethylene glycol, polymethyl methacrylate, stearic acid, polyoxymethylene, polypropylene, etc. The specific process parameters of the mixing and granulation can be determined according to actual conditions and test results, etc., and this embodiment does not limit this. The binder can be purchased from the market or configured by itself according to actual conditions, and the specific composition and ratio are not limited in this embodiment.
[0061] In one practicable manner, the preparation method of the aluminum alloy feedstock may include:
[0062] Step B10, mixing aluminum alloy powder with a binder to obtain an aluminum alloy mixture;
[0063] Step B20, heating, mixing and granulating the aluminum alloy mixture to obtain aluminum alloy feed.
[0064] In the present embodiment, specifically, a certain amount of aluminum alloy powder and a binder are measured and mixed to obtain an aluminum alloy mixture, and then, the aluminum alloy powder mixture is kneaded in a vacuum environment or an inert atmosphere, and then cooled and granulated to obtain an aluminum alloy feed, wherein the mixing ratio of the aluminum alloy powder and the binder can be determined according to actual needs or actual test results, which is not limited in the present embodiment; the specific process parameters of mixing, cooling, and granulation can be determined according to actual conditions and test results, etc., which is not limited in the present embodiment.
[0065] In one practicable manner, the volume proportion of the binder in the aluminum alloy mixture is 15-35%.
[0066] In this embodiment, the volume proportion of the binder in the aluminum alloy mixture is 15-35%, for example, 15%, 20%, 25%, 30%, 35%, etc., so that the aluminum alloy feed can be tightly bonded by the binder to improve the molding efficiency and molding effect of injection molding.
[0067] In one practicable manner, the binder includes polyethylene glycol, polymethyl methacrylate and stearic acid, wherein the volume proportion of the polyethylene glycol in the binder is 65-85%, the volume proportion of the polymethyl methacrylate in the binder is 14-30%, and the volume proportion of the stearic acid in the binder is 1-5%.
[0068] In this embodiment, the binder includes polyethylene glycol, polymethyl methacrylate and stearic acid, wherein the volume proportion of the polyethylene glycol in the binder is 65-84%, for example, 65%, 75%, 84%, etc., the volume proportion of the polymethyl methacrylate in the binder is 14-30%, for example, 14%, 23%, 30%, etc., and the volume proportion of the stearic acid in the binder is 1-5%, for example, 1%, 2%, 5%, etc.
[0069] In an operative manner, the aluminum alloy powder includes a spherical aluminum alloy powder, the D50 of the spherical aluminum alloy powder is less than 45 μm, and the D90 of the spherical aluminum alloy powder is 35-40 μm.
[0070] In this embodiment, the aluminum alloy powder includes spherical aluminum alloy powder, the D50 (the particle size corresponding to the cumulative particle size distribution percentage of a sample reaches 50%) of the spherical aluminum alloy powder is less than 45μm, and the D90 (the particle size corresponding to the cumulative particle size distribution percentage of a sample reaches 90%) of the spherical aluminum alloy powder is 35-40μm, for example, 35μm, 38μm, 40μm, etc.
[0071] In an practicable manner, the temperature of the heating and kneading is 140-220° C., the rotation speed of the heating and kneading is 30-50 r / min, and the time of the heating and kneading is 1-4 h.
[0072] In this embodiment, the heating and kneading temperature is 140-220°C, for example, 140°C, 170°C, 200°C, 220°C, etc., the heating and kneading speed is 30-50r / min, for example, 30r / min, 40r / min, 50r / min, etc., and the heating and kneading time is 1-4h, for example, 1h, 2h, 3h, 4h, etc.
[0073] In one practicable manner, the method for preparing the aluminum alloy feedstock may include:
[0074] The aluminum alloy powder and the binder are added into an internal mixer and filled with argon gas. The mixture is kneaded for 1-4 hours at a temperature of 140-220° C. and a rotation speed of 30-50 r / min. After cooling, the mixture is crushed and granulated to obtain an aluminum alloy feed.
[0075] Step A20, injecting the aluminum alloy feed into the target mold to obtain an aluminum alloy base part.
[0076] In this embodiment, specifically, the aluminum alloy feed is injected into the target mold by powder injection molding equipment, and injection molding is performed to prepare the aluminum alloy base member.
[0077] Optionally, the step of injecting the aluminum alloy feedstock into the target mold to obtain the aluminum alloy base member comprises:
[0078] The aluminum alloy feed is injected into the target mold, the injection temperature is controlled to be 160-220° C., the injection pressure is 1200-1600 bar, the mold temperature is 35° C.-45° C., the pressure is maintained at 800-1200 bar, and the mold is cooled for 4s-12s to obtain an aluminum alloy base part.
[0079] In this embodiment, specifically, by using powder injection molding equipment, the injection temperature is controlled to be 160-220°C, for example, 160°C, 180°C, 200°C, 220°C, etc., the injection pressure is 1200-1600bar, for example, 1200bar, 1400bar, 1600bar, etc., the mold temperature is 35°C-45°C, for example, 35°C, 40°C, 45°C, etc., the aluminum alloy feed is injected into a target mold with a high-strength metal insert, injection molding is performed, the pressure is maintained at 800-1200bar, for example, 800bar, 1000bar, 1200bar, etc., and the cooling is performed for 4s-12s, for example, 4s, 8s, 12s, etc., to obtain a composite component.
[0080] Optionally, the high-strength metal insert is one of a steel insert and a titanium alloy insert.
[0081] Optionally, when the high-strength metal insert is a steel insert, the density of the aluminum alloy-based composite material component is 3.0 to 6.0 g / cm 3 ;
[0082] When the high-strength metal insert is a titanium alloy insert, the density of the aluminum alloy-based composite material component is 2.8 to 4.0 g / cm 3 .
[0083] In this embodiment, the steel has a high strength of more than 1500 MPa, good wear resistance, low cost, and abundant output. It is very suitable for making small precision hardware such as mobile phone card trays, ejectors, gear precision shafts, etc., but the density of steel is about 7.8 g / cm 3 By combining high-strength, high-wear-resistant and low-cost steel inserts with aluminum alloys, the steel part of the aluminum alloy-based composite component can be used for load bearing or contact friction, while the aluminum alloy part has a lower density, which can effectively reduce the mass of the aluminum alloy-based composite component. The density of the prepared aluminum alloy-based composite component is 3.0-6.0g / cm 3 , meeting the demand for lightweight, so that the final prepared aluminum alloy-based composite material components have the advantages of high strength, light weight, high wear resistance and low cost.
[0084] The steel insert is made of steel material through stamping, forging, powder injection molding and other processes. The steel material is an iron-carbon alloy material formed by adding an appropriate amount of one or more alloy elements to ordinary carbon steel, such as Mn13 high manganese steel, 17-4PH alloy stainless steel, GCr15 steel (high carbon chromium bearing steel), etc.
[0085] The density of titanium alloy is about 4.5g / cm 3, with a strength of about 1000MPa. Compared with steel, titanium alloy has certain lightweight advantages. However, compared with steel, titanium alloy has higher cost and is more difficult to process. By compounding high-strength, high-wear-resistant and low-cost titanium alloy inserts with aluminum alloy, the titanium alloy part of the obtained aluminum alloy-based composite material component can be used for load bearing or contact friction, while the aluminum alloy part has a lower density, which can effectively reduce the quality of the aluminum alloy-based composite material component. The density of the prepared aluminum alloy-based composite material component is 2.8-4.0g / cm 3 , meeting the demand for lightweight, so that the final prepared aluminum alloy-based composite material components have the advantages of high strength, lightweight and high wear resistance.
[0086] The titanium alloy insert is made of titanium alloy material through stamping, forging, powder injection molding and other processes. The titanium alloy material is an alloy metal material made of titanium and other metals, such as TC4 titanium alloy (titanium alloy with elemental composition of Ti-6Al-4V), TC10 titanium alloy (titanium alloy with elemental composition of Ti-6Al-6V-2Sn-0.5Cu-0.5Fe), TC3 titanium alloy (titanium alloy with elemental composition of Ti-5Al-4V), TA7 titanium alloy (titanium alloy with elemental composition of Ti-5Al-2.5Sn), etc.
[0087] Optionally, the high-strength metal insert has a strength greater than 900 MPa and a Vickers hardness greater than 350, and the strength of the aluminum alloy base component is greater than 200 MPa.
[0088] In this embodiment, the high-strength metal insert is mainly used for bearing force or friction, and has certain requirements for strength and hardness. Therefore, a high-strength metal insert with a strength greater than 900MPa and a Vickers hardness greater than 350 is selected. The density of the aluminum alloy is about 2.7g / cm 3 , which is particularly beneficial for lightweighting, and can effectively reduce the mass of the prepared aluminum alloy-based composite material components, thereby reducing the mass of smart wearable products processed with the aluminum alloy-based composite material components and improving the comfort of human body when wearing smart wearable products. That is, the main contribution of aluminum alloy is lightweighting, and the strength can meet the general load requirements. Therefore, a raw aluminum alloy with a strength greater than 200MPa is selected to prepare the aluminum alloy feed, which can reduce the overall mass of the finally prepared aluminum alloy-based composite material components, so that the aluminum alloy-based composite material components meet the lightweight requirements, and at the same time ensure that the parts of the finally prepared aluminum alloy-based composite material components that need to bear force or friction have sufficient strength and wear resistance.
[0089] Step S20, installing the high-strength metal insert in the embedding portion to obtain a composite component;
[0090] In this embodiment, specifically, the high-strength metal insert is pushed into the embedding portion so that a partial area on the high-strength metal insert fits with a partial area on the embedding portion to obtain a composite component.
[0091] In one feasible manner, the high-strength metal insert can be just accommodated in the embedded portion, and then the high-strength metal insert can be pushed by a worm to be embedded in the embedded portion. In this case, the relative position between the high-strength metal insert and the aluminum alloy base can be fixed by friction; the specification of the high-strength metal insert can also be slightly smaller than the specification of the embedded portion. In this case, the high-strength metal insert can be installed by interference fitting. In addition to the friction, the high-strength metal insert and the aluminum alloy base will also generate contact pressure due to the interference, so the two are fixed more firmly, and after subsequent sintering, the deformation is smaller, and the dimensional accuracy of the aluminum alloy-based composite material components is higher.
[0092] Optionally, the step of installing the high-strength metal insert in the embedding portion to obtain a composite component includes:
[0093] The high-strength metal insert is interference-fitted into the embedded portion to obtain a composite component.
[0094] In this embodiment, specifically, the high-strength metal insert is pushed into the embedded part on the aluminum alloy base by interference fitting, so that a partial area on the high-strength metal insert fits with a partial area on the embedded part to obtain a composite component, wherein the interference fitting method can be a static pressing method, a dynamic pressing method, a temperature difference assembly method, etc., which can be specifically determined according to actual conditions, and this embodiment does not limit this.
[0095] Optionally, the interference fit has an interference amount of 1-200 μm.
[0096] In this embodiment, the interference amount of the interference fit is 1-200 μm, for example, 1 μm, 10 μm, 25 μm, 50 μm, 100 μm, 200 μm, etc.
[0097] Optionally, before the step of installing the high-strength metal insert in the embedding portion to obtain the composite component, the step further includes:
[0098] The high-strength metal insert and the contact surface on the aluminum alloy base are subjected to surface cleaning and surface roughening treatments.
[0099] In this embodiment, it should be noted that the pre-prepared high-strength metal insert and the aluminum alloy base may be processed intermediate parts that have not been further sintered, or may be commercially available finished products that have been sintered. In the case where the high-strength metal insert and / or the aluminum alloy base are finished products, the grease, oxide layer, etc. on their surfaces may reduce the bonding strength between the high-strength metal insert and the aluminum alloy base. Therefore, in this embodiment, the bonding strength between the high-strength metal insert and the aluminum alloy base after the subsequent sintering process can be effectively improved by performing a surface cleaning process on the contact surface to remove the surface grease, and performing a surface roughening process on the contact surface to increase the contact area of the contact surface.
[0100] Specifically, before combining the high-strength metal insert and the aluminum alloy base, the contact surfaces of the high-strength metal insert and the aluminum alloy base after the high-strength metal insert and the aluminum alloy base are determined, and each contact surface is cleaned to remove grease on the contact surface, and the surface is roughened to increase the roughness of the contact surface, wherein the surface cleaning method may be to use an organic solvent, emulsion, alkaline cleaning solution, water-based cleaning agent, acid cleaning solution or other cleaning agent to clean the contact surface; the surface roughening method may be sandblasting, corrosion, etc.
[0101] Optionally, the surface roughness Ra of the contact surface on the high-strength metal insert and the aluminum alloy base is 10-1000.
[0102] In this embodiment, increasing the surface roughness of the contact surface can increase the contact area between the high-strength metal insert and the aluminum alloy substrate, and the bonding between the aluminum atoms and the metal atoms in the high-strength metal insert is tighter. Therefore, the surface roughness Ra of the contact surface on the high-strength metal insert and the aluminum alloy substrate can be 10-1000.
[0103] Step S30, sintering the composite component to obtain an aluminum alloy-based composite material component.
[0104] In this embodiment, specifically, the injection molded composite component is placed in an inert atmosphere for a period of time for high-temperature sintering treatment, and cooled to obtain an aluminum alloy-based composite material component, thereby obtaining a lightweight, high-strength and high-wear-resistant aluminum alloy-based composite material component, wherein the inert atmosphere can be an argon atmosphere, etc., and the temperature of the high-temperature sintering treatment can be determined according to actual needs or test results, etc., and this embodiment does not limit this.
[0105] In one feasible manner, before sintering the composite component, the composite component may be degreased, and the degreasing methods include thermal degreasing, solvent degreasing, catalytic degreasing, etc. It should be noted that if the degreasing effect can be achieved during the sintering process, degreasing may not be performed.
[0106] Optionally, the step of sintering the composite assembly to obtain an aluminum alloy-based composite material component comprises:
[0107] Step S31, heating the composite component to 400-600°C at a rate of 3-6°C / min in an inert atmosphere, and thermally debinding for 1-3 hours to obtain a thermally debinded blank;
[0108] In this embodiment, specifically, the composite component is placed in a thermal debinding device, an inert gas is introduced into the thermal debinding device, and under the protection of the inert gas, the composite component is heated to 400-600°C, for example, 400°C, 500°C, 600°C, etc., at a rate of 3-6°C / min, for example, 3°C / min, 5°C / min, 6°C / min, etc., so that the composite component is thermally debound for 1-3 hours, for example, 1 hour, 2 hours, 3 hours, etc., under the protection of the inert gas and at a high temperature of 400-600°C, so that the binder in the composite component is removed from the blank by volatilization or decomposition to obtain a thermally debound blank.
[0109] Step S32, sintering the hot debinded blank in an inert atmosphere at a temperature of 300-650° C. for 3-5 hours, and cooling it to room temperature in the furnace to obtain an aluminum alloy-based composite material component.
[0110] In this embodiment, specifically, the hot debinded blank is placed in a sintering treatment device, an inert gas is introduced into the sintering treatment device, and under the protection of the inert gas, the hot debinded blank is heated to 300-650°C, for example, 300°C, 400°C, 500°C, 650°C, etc., so that the hot debinded blank is sintered for 3-5 hours, for example, 3 hours, 4 hours, 5 hours, etc., under the protection of the inert gas and at a high temperature of 300-650°C, so that the aluminum alloy material adjacent to the high-strength metal insert in the hot debinded blank diffuses into the high-strength metal insert and forms a metal bond with the metal in the high-strength metal insert, thereby making the aluminum alloy base member in the hot debinded blank tightly combined with the high-strength metal insert. According to tests, the bonding strength between the aluminum alloy and the high-strength metal insert is greater than 80% of the lower strength of the aluminum alloy or the strength of the high-strength metal insert, that is, the aluminum alloy and the high-strength metal insert can form a metal bond through diffusion to achieve tight bonding. The hot degreased blank is cooled to room temperature in the furnace after sintering to obtain an aluminum alloy-based composite material component, wherein the density of the aluminum alloy-based composite material component is 3.0-6.0 g / cm 3 It is determined by the proportion of high-strength metal inserts and aluminum alloy base components in the aluminum alloy-based composite material component. The greater the proportion of high-strength metal inserts, the greater the density, and the smaller the proportion of high-strength metal inserts, the smaller the density.
[0111] It should be noted that the sintering processing equipment and the debinding equipment can be two independent equipment or the same equipment. If the sintering processing equipment and the debinding equipment are the same equipment, after debinding, there is no need to take out the hot debinded blank, and the temperature in the equipment can be adjusted to the sintering processing temperature to continue the sintering process.
[0112] In one feasible method, the aluminum alloy-based composite material component can be further subjected to post-treatment such as shaping, polishing and / or applying lubricating oil, and the obtained aluminum alloy-based composite material component can be subjected to surface processing to reduce surface roughness and / or friction, so as to reduce friction damage to the aluminum alloy-based composite material component during use, thereby improving the wear resistance of the aluminum alloy-based composite material component, and also improving the surface smoothness and aesthetics of the material.
[0113] In this embodiment, an aluminum alloy-based composite material component and a preparation method thereof are provided. The aluminum alloy-based composite material component is applied to a head-mounted display device. The preparation method of the aluminum alloy-based composite material component comprises the steps of: obtaining a high-strength metal insert and an aluminum alloy base component, wherein an embedding portion matching the high-strength metal insert is processed on the aluminum alloy base component; installing the high-strength metal insert on the embedding portion to obtain a composite component; and sintering the composite component to obtain the aluminum alloy-based composite material component. The present application obtains a composite component formed by the aluminum alloy base and the high-strength metal insert by installing a high-strength metal insert with relatively large strength into an aluminum alloy base with relatively small density, and then the composite component is degreased and sintered to achieve diffusion of dissimilar metals between the aluminum alloy base and the high-strength metal insert, so that aluminum atoms form metal bonds with metal atoms in the high-strength metal insert, and then the aluminum alloy part in the composite component and the high-strength metal insert form a dense whole through sintering, namely, an aluminum alloy-based composite material component. The high-strength metal insert part in the obtained aluminum alloy-based composite material component can be used for load bearing or contact friction, while the aluminum alloy part has a relatively low density, which can effectively reduce the mass of the aluminum alloy-based composite material component and meet the demand for lightweight, so that the finally prepared aluminum alloy-based composite material component has the advantages of high strength, lightweight and high wear resistance at the same time, overcoming the technical problem that the components in the head-mounted display device in the prior art are difficult to meet the requirements of lightweight, high strength and high wear resistance at the same time.
[0114] Furthermore, the present invention also provides an aluminum alloy-based composite material component, which is applied to a head-mounted display device. The aluminum alloy-based composite material component is prepared by the above-mentioned method for preparing an aluminum alloy-based composite material component. In one embodiment of the aluminum alloy-based composite material component of the present application, the aluminum alloy-based composite material component comprises:
[0115] an aluminum alloy substrate; and
[0116] At least one load-bearing portion connected to the aluminum alloy substrate;
[0117] Wherein, the load-bearing part is one of a steel load-bearing part and a titanium alloy load-bearing part.
[0118] In this embodiment, it should be noted that the aluminum alloy-based composite material components can be applied to head-mounted display devices that have requirements for lightweight and high strength and high wear resistance. The aluminum alloy-based composite material components include hinges, bearings, rotating shafts, balls, gears and other components that bear both bending moments and torques. These components move frequently during use and have greater requirements for strength and wear resistance. The head-mounted display devices include AR glasses, VR helmets, etc.
[0119] Specifically, the aluminum alloy-based composite material component includes an aluminum alloy matrix, and at least one load-bearing part connected to the aluminum alloy matrix, such as the part of the hinge blade that contacts the pin, the tooth tip part of the gear, the connection point of the rotating shaft, the contact surface of the friction pair, etc. The load-bearing part is one of a steel load-bearing part and a titanium alloy load-bearing part. The load-bearing part used for bearing force in the aluminum alloy-based composite material component is made of steel or titanium alloy. Compared with aluminum alloy, steel or titanium alloy has higher strength and better wear resistance, while the partial density of aluminum alloy is lower, which can effectively reduce the mass of the aluminum alloy-based composite material component and meet the demand for lightweight, so that the finally prepared aluminum alloy-based composite material component has the advantages of high strength, lightweight and high wear resistance at the same time, overcoming the technical problem that the components in the head-mounted display device in the prior art are difficult to meet the requirements of lightweight, high strength and high wear resistance at the same time.
[0120] The aluminum alloy-based composite material component provided by the present application solves the technical problem that the components in the head-mounted display device of the prior art are difficult to simultaneously meet the requirements of light weight, high strength and high wear resistance. Compared with the prior art, the beneficial effects of the aluminum alloy-based composite material component provided by the embodiment of the present invention are the same as the beneficial effects of the preparation method of the aluminum alloy-based composite material component of the above embodiment, which will not be described in detail here.
[0121] Furthermore, the present invention also provides a head-mounted display device, which includes the aluminum alloy-based composite material component as described above.
[0122] In this embodiment, the head-mounted display device includes AR glasses, VR helmets, etc.
[0123] In an operative manner, the head mounted display device is an AR glasses, the aluminum alloy-based composite material component is disposed at the rotation axis position of the AR glasses, and at least part of the aluminum alloy-based composite material component is disposed in the accommodation space formed by the frame and temples of the AR glasses. Figure 2 The aluminum alloy-based composite material component includes two load-bearing parts whose projections overlap in a preset first direction, wherein the preset first direction may be perpendicular to the extension direction of the temple of the AR glasses.
[0124] In an operative manner, the head mounted display device is a VR head mounted display device, and the aluminum alloy-based composite material component is disposed on a flip structure between a main body of the VR head mounted display device and a headband. Exemplarily, the flip structure may include a first aluminum alloy-based composite material component disposed on the main body of the head mounted display device and a second aluminum alloy-based composite material component disposed on the headband, wherein the projection of the load-bearing portion of the first aluminum alloy-based composite material component and the load-bearing portion of the second aluminum alloy-based composite material component in a preset second direction overlap, wherein the preset second direction may be parallel to the main body of the head mounted display device, and the perpendicular midline of the aluminum alloy matrix portion on the first aluminum alloy-based composite material component and the perpendicular midline of the aluminum alloy matrix portion on the second aluminum alloy-based composite material may point to the wearer of the VR head mounted display device.
[0125] The head-mounted display device provided by the present application solves the technical problem that the components in the head-mounted display device of the prior art are difficult to simultaneously meet the requirements of light weight, high strength and high wear resistance. Compared with the prior art, the beneficial effects of the head-mounted display device provided by the embodiment of the present invention are the same as the beneficial effects of the aluminum alloy-based composite material components of the above-mentioned embodiment, which will not be repeated here.
[0126] In order to further understand the present application, the aluminum alloy-based composite material component provided by the present application and its preparation method and application are specifically described below in combination with the embodiments. The embodiments of the present invention all use commercially available raw materials.
[0127] Example 1
[0128] Material and parts design: A cylindrical 17-4 stainless steel insert is selected as the main force-bearing and wear-resistant part, and an aluminum alloy base is made of aluminum silicon alloy for powder injection molding. The interference between the aluminum alloy base and the high-strength metal insert is 50 μm.
[0129] Assembly: The high-strength metal insert is interference-fitted into the embedded portion of the aluminum alloy base component to form a composite component.
[0130] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 600℃ at 5℃ / min, and hot debinding was performed for 2 hours to obtain a hot debinding blank; the temperature was adjusted to 450℃, and pressure-maintained sintering treatment was performed for 5 hours, and then the aluminum alloy-based composite material component was obtained by cooling to room temperature with the furnace. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 3 As shown, the top view of the aluminum alloy matrix composite material component is as shown Figure 4 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.
[0131] Test: The aluminum alloy matrix composite component prepared in Example 1 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-steel composite interface was 255 MPa, the bulk strength of the aluminum alloy matrix was 336 MPa, and the overall density of the aluminum alloy matrix composite component was 3.1 g / cm 3 , see Table 1 for details.
[0132] Example 2
[0133] Material and parts design: 17-4 stainless steel inserts are selected as the main force-bearing and wear-resistant parts, and the aluminum alloy base is made of 6063 aluminum alloy for powder injection molding. The shape specifications of the high-strength metal inserts are the same as those of the embedded part.
[0134] Assembly: The high-strength metal insert is fixed in the embedded portion of the aluminum alloy base component to form a composite component.
[0135] Debinding sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 400°C at 6°C / min, and thermal debinding was performed for 1 hour to obtain a thermally debinded blank; the temperature was adjusted to 300°C, and pressure-maintained sintering treatment was performed for 4 hours, and then the blank was cooled to room temperature with the furnace to obtain an aluminum alloy-based composite material component. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 5 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.
[0136] Test: The aluminum alloy matrix composite component prepared in Example 2 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-steel composite interface was 265 MPa, the bulk strength of the aluminum alloy matrix was 336 MPa, and the overall density of the aluminum alloy matrix composite component was 4.1 g / cm 3 , see Table 1 for details.
[0137] Example 3
[0138] Materials and parts design: 17-4 stainless steel inserts made of powder injection molding are selected as the main force-bearing and wear-resistant parts, and the aluminum alloy base parts are made of finished aluminum alloy plates made of 7050 aluminum alloy. The interference between the aluminum alloy base parts and the high-strength metal inserts is 200μm.
[0139] Assembly: The high-strength metal insert is interference-fitted into the embedded portion of the aluminum alloy base component to form a composite component.
[0140] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 500°C at 3°C / min, and thermal debinding was performed for 3 hours to obtain a thermally debinded blank; the temperature was adjusted to 650°C, and pressure-maintained sintering treatment was performed for 3 hours, and then the blank was cooled to room temperature with the furnace to obtain an aluminum alloy-based composite material component. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 3 As shown, the top view of the aluminum alloy matrix composite material component is as shown Figure 4 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.
[0141] Test: The aluminum alloy matrix composite material component prepared in Example 3 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-steel composite interface was 365 MPa, the bulk strength of the aluminum alloy matrix was 460 MPa, and the overall density of the aluminum alloy matrix composite material component was 4.8 g / cm 3 , see Table 1 for details.
[0142] Example 4
[0143] Material and parts design: A cylindrical TC4 titanium alloy insert is selected as the main force-bearing and wear-resistant part, and an aluminum alloy base is made of aluminum silicon alloy for powder injection molding. The interference between the aluminum alloy base and the high-strength metal insert is 200 μm.
[0144] Assembly: The high-strength metal insert is interference-fitted into the embedded portion of the aluminum alloy base component to form a composite component.
[0145] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 600℃ at 5℃ / min, and hot debinding was performed for 2 hours to obtain a hot debinding blank; the temperature was adjusted to 450℃, and pressure-maintained sintering treatment was performed for 5 hours, and then the aluminum alloy-based composite material component was obtained by cooling to room temperature with the furnace. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 3 As shown, the top view of the aluminum alloy matrix composite material component is as shown Figure 4 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.
[0146] Test: The aluminum alloy matrix composite component prepared in Example 1 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-titanium composite interface was 255 MPa, the bulk strength of the aluminum alloy matrix was 336 MPa, and the overall density of the aluminum alloy matrix composite component was 3.1 g / cm 3 , see Table 1 for details.
[0147] Example 5
[0148] Material and parts design: TC4 titanium alloy inserts are selected as the main force-bearing and wear-resistant parts, and the aluminum alloy base parts are selected from finished aluminum alloy plates of 6063 aluminum alloy. The shape specifications of the high-strength metal inserts are the same as those of the embedded parts, and the contact surfaces of the high-strength metal inserts and the titanium alloy inserts are both surface cleaned and roughened.
[0149] Assembly: The high-strength metal insert is fixed in the embedded portion of the aluminum alloy base component to form a composite component.
[0150] Debinding sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 400°C at 6°C / min, and thermal debinding was performed for 1 hour to obtain a thermally debinded blank; the temperature was adjusted to 300°C, and pressure-maintained sintering treatment was performed for 4 hours, and then the blank was cooled to room temperature with the furnace to obtain an aluminum alloy-based composite material component. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 5 As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.
[0151] Test: The aluminum alloy matrix composite component prepared in Example 2 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-titanium composite interface was 255 MPa, the bulk strength of the aluminum alloy matrix was 306 MPa, and the overall density of the aluminum alloy matrix composite component was 3.2 g / cm 3 , see Table 1 for details.
[0152] Example 6
[0153] Material and part design: TC4 titanium alloy inserts made of powder injection molding are selected as the main force-bearing and wear-resistant parts, and the aluminum alloy base parts are made of finished aluminum alloy plates made of 7050 aluminum alloy. The interference between the aluminum alloy base parts and the high-strength metal inserts is 100μm, and the contact surfaces of the high-strength metal inserts and the titanium alloy inserts are surface cleaned and roughened.
[0154] Assembly: The high-strength metal insert is interference-fitted into the embedded portion of the aluminum alloy base component to form a composite component.
[0155] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 500°C at 3°C / min, and thermal debinding was performed for 3 hours to obtain a thermally debinded blank; the temperature was adjusted to 650°C, and pressure-maintained sintering treatment was performed for 3 hours, and then the blank was cooled to room temperature with the furnace to obtain an aluminum alloy-based composite material component. The side profile of the obtained aluminum alloy-based composite material component is shown in FIG. Figure 3 As shown, the top view of the aluminum alloy matrix composite material component is as shown Figure 4As shown, the high-strength metal insert 20 and the aluminum alloy substrate 10 are tightly combined via a metal bond.
[0156] Test: The aluminum alloy matrix composite component prepared in Example 3 of the present invention was sampled for tensile test. The sample was subjected to tensile test according to GB / T228.1-2010. The tensile strength of the aluminum-titanium composite interface was 365 MPa, the bulk strength of the aluminum alloy matrix was 450 MPa, and the overall density of the aluminum alloy matrix composite component was 3.8 g / cm 3 , see Table 1 for details.
[0157] Comparative Example 1
[0158] Material and part design: 17-4 stainless steel powder was used to prepare the stainless steel test specimens by powder injection molding.
[0159] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 600°C at a rate of 5°C / min, and hot debinding was performed for 2 hours to obtain a hot debinded blank; the temperature was adjusted to 1200°C, and after pressure-maintaining sintering treatment for 3 hours, the stainless steel test sample was obtained by cooling with the furnace to room temperature.
[0160] Test: The stainless steel test sample prepared in the comparative example of the present invention was subjected to a tensile test. The stainless steel test sample was subjected to a tensile test according to GB / T228.1-2010, and the tensile strength was measured to be 1033 MPa and the density was 7.7 g / cm 3 , see Table 1 for details.
[0161] Comparative Example 2
[0162] Material and part design: TC4 titanium alloy powder was used to prepare titanium alloy test specimens through powder injection molding.
[0163] Debinding and sintering treatment: In an argon flow environment of 40L / min, the temperature was raised to 600°C at 5°C / min, and hot debinding was performed for 2 hours to obtain a hot debinded blank; the temperature was adjusted to 1200°C, and after pressure-maintaining sintering treatment for 3 hours, the titanium alloy test sample was obtained by cooling with the furnace to room temperature.
[0164] Test: The titanium alloy test sample prepared in the comparative example of the present invention was subjected to a tensile test. The titanium alloy test sample was subjected to a tensile test according to GB / T228.1-2010, and the tensile strength was measured to be 853 MPa and the density was 4.4 g / cm 3 , see Table 1 for details.
[0165] Table 1 Performance indexes of composite materials prepared in the embodiments of the present invention
[0166]
[0167] As can be seen from Table 1, compared with the strength of the aluminum alloy matrix, the strength of the high-strength metal insert is higher, so the bearing capacity of the high-strength metal insert is higher, and the wear resistance when rubbing on the surface of the high-strength metal insert is higher than the wear resistance when rubbing on the surface of the aluminum alloy matrix, and compared with the stainless steel sample or the titanium alloy sample, the density of the aluminum alloy-based composite material component is smaller, and the prepared aluminum alloy-based composite material component has the advantages of high strength, light weight and high wear resistance. It should be noted that although the density of the aluminum alloy-based composite material component prepared in Example 3 is higher than the density of the titanium alloy test sample, the cost of titanium alloy is relatively high. In low-cost products, aluminum alloy-based composite material components of aluminum-steel composites with a density similar to that of titanium alloy can be prepared to meet the requirements of low cost, high strength, light weight and high wear resistance at the same time.
[0168] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent processing scope of the present application.
Claims
1. A method for preparing an aluminum alloy-based composite material component, characterized in that: The aluminum alloy-based composite material component is applied to a head mounted display device, and the preparation method of the aluminum alloy-based composite material component comprises the following steps: Obtaining a high-strength metal insert and an aluminum alloy base member, wherein an embedding portion matching the high-strength metal insert is processed on the aluminum alloy base member; installing the high-strength metal insert in the embedding portion to obtain a composite component; The composite component is sintered to obtain an aluminum alloy-based composite material component.
2. The method for preparing an aluminum alloy-based composite material component according to claim 1, characterized in that: The step of installing the high-strength metal insert in the embedding portion to obtain a composite component comprises: The high-strength metal insert is interference-fitted into the embedded portion to obtain a composite component.
3. The method for preparing an aluminum alloy-based composite material component according to claim 2, characterized in that: The interference fit has an interference amount of 1-200 μm.
4. The method for preparing an aluminum alloy-based composite material component according to claim 1, characterized in that: Before the step of installing the high-strength metal insert in the embedding portion to obtain a composite component, the step further includes: The high-strength metal insert and the contact surface on the aluminum alloy base are subjected to surface cleaning and surface roughening treatments.
5. The method for preparing an aluminum alloy-based composite material component according to claim 4, characterized in that: The surface roughness Ra of the contact surface on the high-strength metal insert and the aluminum alloy base is 10-1000.
6. The method for preparing an aluminum alloy-based composite material component according to claim 1, characterized in that: Before the step of obtaining the aluminum alloy base part, it also includes: Obtaining a target mold and an aluminum alloy feed, wherein the target mold is provided with a protrusion structure, and the protrusion structure is used to form an embedding portion matching the high-strength metal insert on the aluminum alloy base member during the forming process of the aluminum alloy base member; The aluminum alloy feedstock is injected into the target mold to obtain an aluminum alloy base part.
7. The method for preparing an aluminum alloy-based composite material component according to claim 6, characterized in that: The step of injecting the aluminum alloy feed material into the target mold to obtain the aluminum alloy base member comprises: The aluminum alloy feed is injected into the target mold, the injection temperature is controlled to be 160-220° C., the injection pressure is 1200-1600 bar, the mold temperature is 35° C.-45° C., the pressure is maintained at 800-1200 bar, and the mold is cooled for 4s-12s to obtain an aluminum alloy base part.
8. The method for preparing an aluminum alloy-based composite material component according to claim 1, characterized in that: The step of sintering the composite assembly to obtain an aluminum alloy-based composite material component comprises: The composite component is heated to 400-600° C. at a rate of 3-6° C. / min in an inert atmosphere, and thermally degreased for 1-3 hours to obtain a thermally degreased blank; The hot degreased blank is sintered in an inert atmosphere at a temperature of 300-650° C. for 3-5 hours, and then cooled to room temperature in the furnace to obtain an aluminum alloy-based composite material component.
9. The method for preparing an aluminum alloy-based composite material component according to any one of claims 1 to 8, characterized in that: The high-strength metal insert has a strength greater than 900 MPa and a Vickers hardness greater than 350, and the strength of the aluminum alloy base component is greater than 200 MPa.
10. The method for preparing an aluminum alloy-based composite material component according to any one of claims 1 to 8, characterized in that: The high-strength metal insert is one of a steel insert and a titanium alloy insert.
11. The method for preparing an aluminum alloy-based composite material component according to claim 10, characterized in that: When the high-strength metal insert is a steel insert, the density of the aluminum alloy-based composite material component is 3.0 to 6.0 g / cm 3 ; When the high-strength metal insert is a titanium alloy insert, the density of the aluminum alloy-based composite material component is 2.8 to 4.0 g / cm 3 .
12. An aluminum alloy-based composite material component, characterized in that: The aluminum alloy-based composite material component is applied to a head mounted display device, the aluminum alloy-based composite material component is prepared by the method for preparing an aluminum alloy-based composite material component according to any one of claims 1 to 11, and the aluminum alloy-based composite material component comprises: an aluminum alloy substrate; and At least one load-bearing portion connected to the aluminum alloy substrate; Wherein, the load-bearing part is one of a steel load-bearing part and a titanium alloy load-bearing part.
13. A head mounted display device, characterized in that: The head-mounted display device comprises the aluminum alloy-based composite material component as claimed in claim 12.
14. The head mounted display device according to claim 13, wherein: The head mounted display device is glasses, and the aluminum alloy based composite material component is arranged at the rotation axis position of the glasses, or, The head-mounted display device is a VR helmet, and the aluminum alloy-based composite material component is arranged at a flip structure between a main body and a headband of the VR helmet.