Method for accurately measuring content of calcium oxide and magnesium oxide in fly ash and sludge
Through acid treatment of hydrochloric acid, nitric acid, hydrofluoric acid and EDTA titration methods, the content of calcium oxide and magnesium oxide in dust removal ash and sludge was accurately measured, and the problems of high cost and cumbersome operation in the existing technology were solved, and the rapid Accurate analysis results.
Patent Information
- Application Number
- CN202411138111.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-12-03
AI Technical Summary
The method for measuring calcium oxide and magnesium oxide in dust removal ash, sludge in the prior art is costly and cumbersome, making it difficult to meet the needs of small enterprises.
Hydrochloric acid, nitric acid and hydrofluoric acid were used to dissolve the samples, add sulfuric acid to smoke and cool it, adjust the pH by hydrochloric acid and deionized water, add EDTA standard solution to titrate, and use indicators to determine the content of calcium oxide and magnesium oxide.
Fast, efficient and low-cost measurements are achieved, and the results are accurate and stable, filling the gap in the analysis of calcium oxide and magnesium oxide components in dust removal ash and sludge.
Smart Images

Figure BDA0004999978900000061 
Figure BDA0004999978900000062 
Figure BDA0004999978900000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical analysis, and in particular relates to a method for accurately determining the contents of calcium oxide and magnesium oxide in dust and sludge. Background Art
[0002] Iron and steel enterprises are resource- and energy-intensive, generating a large amount of solid waste. In recent years, many countries at home and abroad have increased their efforts in research and development of solid waste in the metallurgical industry. The metallurgical process of my country's iron and steel enterprises is mainly concentrated in the long process of sintering-blast furnace-converter-rolling, accounting for more than 70% of the total steel production capacity. The output of sintering dust is 8-15kg / ton, blast furnace dust is 20-30kg / ton, converter dust is 8-20kg / ton, and electric furnace dust is 10-20kg / ton. The amount of dust in the steel industry is large and has good utilization value.
[0003] The uses are as follows:
[0004] 1. As ingredients for sintering and pelletizing: dust ash with an iron content of more than 60% and a low zinc content can be directly returned to sintering ingredients; it can also be used to make pellets. Advantages: simple method and low processing cost; Disadvantages: affects the quality of sintered ore, and harmful elements are still circulating inside the sintering.
[0005] 2. Dust ash briquetting: Hot briquetting uses the self-ignition characteristics of dust to heat the dust, and uses its plasticity at high temperature to press it into briquettes through a high-pressure briquetting machine. After cooling in a nitrogen-sealed state, it is transported to the converter to replace scrap steel or ore. The production of hot briquetting needs to be carried out under high temperature and air-tight conditions, which requires high equipment and process control, large one-time investment, harsh process conditions, and difficult long-term production. Cold briquetting adds some additives to dust ash and sludge, mixes with a binder, and uses a cold solidification process to make converter slag-making briquettes, which are used for converter slag making, improve dephosphorization effect, increase efficiency, have good slag-removing effect, and can prevent splashing.
[0006] 3. Dust ash briquetting process: Add appropriate amount of binder to iron ore powder, dust ash, sludge and other iron-containing wastes, mix them in a mixer, and send them to the briquetting machine to form pellets. The pellets are dried to increase their strength, enter the rotary hearth furnace, and rotate with the furnace bottom. The pellets are subjected to radiation heat transfer in the furnace, and are reduced at high temperature for 15-20 minutes to complete the metallization process, and the reduced zinc is gasified. When the iron content of iron ore powder is above 67%, the direct reduction process of the rotary hearth furnace is adopted, and the product is metallized pellets for use in electric furnaces; when the iron content of ore powder is lower than 62%, the molten iron reduction process of the rotary hearth furnace-melting furnace is adopted, and the product is molten iron for steelmaking. Usually the metallization rate can reach more than 80%, and the metallized pellets can be used as blast furnace raw materials.
[0007] The accurate determination of calcium oxide and magnesium oxide in dust and sludge is of great significance. At present, there are two methods for determining calcium oxide and magnesium oxide in dust and sludge: instrumental analysis and chemical analysis. Large enterprises mostly use large instrument analysis, but the cost is high. For small enterprises, chemical analysis methods better reflect its advantages, that is, convenience and speed. The determination of calcium oxide in dust and sludge by chemical analysis generally uses platinum sheet semi-dissolution, which requires demanganese and silicon removal. The operation is cumbersome, time-consuming and costly. Summary of the invention
[0008] In view of one or more problems existing in the prior art, the present invention provides a method for accurately measuring the content of calcium oxide and magnesium oxide in dust and sludge, which comprises the following steps:
[0009] 1) Weigh the sample;
[0010] 2) Use hydrochloric acid, nitric acid, or hydrofluoric acid to dissolve the sample, add sulfuric acid to generate smoke, and then cool;
[0011] 3) adding hydrochloric acid to the product obtained in step 2) and heating to dissolve the salts, then adding deionized water and adjusting the solution pH to about 7 with aqueous ammonia, heating and boiling, filtering the solution into a volumetric flask and fixing the volume;
[0012] 4) Take two equal parts of the solution from the volumetric flask in step 3), add equal amounts of triethanolamine, water and a small amount of hydroxylamine hydrochloride to each of them, add potassium hydroxide solution and an appropriate amount of calcium indicator to one of them, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point, and add ammonia-ammonium chloride buffer solution (pH=10) and a proper amount of chromium black T indicator to the other part, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point;
[0013] 5) Calculate the contents of calcium oxide and magnesium oxide in the sample based on the titration results obtained in step 4).
[0014] In some embodiments, the method comprises the following steps:
[0015] 1) Weigh the sample;
[0016] 2) Use hydrochloric acid (65%), nitric acid (67%), and hydrofluoric acid (40%) to dissolve the sample, add sulfuric acid to make it smoke, and then cool it;
[0017] 3) Add hydrochloric acid (65%) to the product obtained in step 2), heat to dissolve the salts, then add deionized water, and adjust the solution pH to about 7 with aqueous ammonia (50%), heat to boil, filter the solution into a volumetric flask and make up to volume;
[0018] 4) Take two equal parts of the solution from the volumetric flask in step 3), add equal amounts of triethanolamine (25%), water and a small amount of hydroxylamine hydrochloride to each of them, add potassium hydroxide solution and an appropriate amount of calcium indicator to one of them, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point, and add ammonia-ammonium chloride buffer solution (pH=10) and a proper amount of chromium black T indicator to the other part, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point;
[0019] 5) Calculate the contents of calcium oxide and magnesium oxide in the sample based on the titration results obtained in step 4).
[0020] In some embodiments, the method comprises the following steps:
[0021] Weigh 0.2500g of sample m into a polytetrafluoroethylene beaker, add 10mL hydrochloric acid (65%) and 10mL hydrofluoric acid (40%), dissolve the sample on a low-temperature electric hot plate (100°C), and after most of the sample is dissolved, add 5mL nitric acid (67%) and 20mL sulfuric acid (5%), continue heating until the sulfuric acid smokes and the test solution becomes wet salt. Remove it, cool it, and carefully add 5mL hydrochloric acid (65%) along the wall of the cup, and heat to dissolve the salts. Add 50mL of deionized water, adjust the solution pH to about 7 with ammonia water (50%), heat the solution to boil on a hot plate, remove it, filter the test solution into a 250mL volumetric flask with quantitative rapid filter paper, wash the precipitate with ammonium chloride washing solution (1%) 7-8 times, and then dilute it with deionized water to the scale, take two 50mL portions of the solution, add 5mL of triethanolamine (25%), 50mL of water, and a little hydroxylamine hydrochloride in 250mL beakers respectively, add 20mL of potassium hydroxide solution (20%) to one portion, and an appropriate amount of calcium indicator, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point, and measure the volume V Ca , do a blank test with the sample and calculate the volume V 01 ; Add 10mL of ammonia-ammonium chloride buffer solution (pH=10) to the other portion, add an appropriate amount of EDTA indicator, and titrate with EDTA standard solution until the purple-red color changes to blue as the end point, and measure the volume V (Mg+Ca) , do a blank test with the sample and calculate the volume V 02 .
[0022] In some embodiments, the calculation formula for the calcium oxide content in the sample is:
[0023] W(CaO)%=C(V Ca -V 01 )M(CaO)100 / m K×1000
[0024] Where:
[0025] M(CaO): molar mass of calcium oxide (g / mol);
[0026] m: sample mass (g);
[0027] K: sample liquid separation ratio (50 / 250=1 / 5);
[0028] C: EDTA standard solution concentration (mol / L);
[0029] V Ca : Volume of calcium-consumed EDTA standard solution in the sample (mL);
[0030] V 01 : The volume of EDTA standard solution consumed in the blank titration of calcium (mL).
[0031] In some embodiments, the calculation formula for the magnesium oxide content in the sample is:
[0032] W(MgO)%=C(V (Mg+Ca) -V Ca -(V 02 -V 01 )M(MgO)100 / m K×1000
[0033] Where:
[0034] M(MgO): molar mass of magnesium oxide (g / mol);
[0035] m: sample mass (g);
[0036] K: sample liquid separation ratio;
[0037] C: EDTA standard solution concentration (mol / L);
[0038] V (Mg+Ca) : The volume of EDTA standard solution consumed by the total amount of calcium and magnesium (mL);
[0039] V 02 : The volume of blank EDTA standard solution consumed when titrating the total amount of calcium and magnesium (mL).
[0040] The present invention has the following beneficial effects:
[0041] 1) Fast, efficient and low-cost: This method greatly shortens the operation process, saves drugs, reduces testing costs and improves production efficiency.
[0042] 2) Accurate and stable: The results measured by this method are the same as those after demanganese and desiliconization, which ensures the stability of the measurement results and the accuracy of the data.
[0043] 3) Filling method: The present invention provides accurate data for the content of calcium oxide and magnesium oxide in dust removal ash and sludge, filling the blank of the analysis of calcium oxide and magnesium oxide components in dust removal ash and sludge. DETAILED DESCRIPTION
[0044] The present invention aims to provide a method for determining calcium oxide and magnesium oxide in dust and sludge with a short operation process, low cost, rapidity, high efficiency, accuracy, good stability and easy mastery, so as to solve the problem of long process and high cost of existing analytical methods. The present invention is mainly achieved in the following ways.
[0045] In a polyethylene plastic beaker, hydrochloric acid (65%), nitric acid (67%), and hydrofluoric acid (40%) are used to dissolve the sample, and sulfuric acid is added to smoke (the sulfuric acid smokes for 1-2 minutes, that is, the sample is in a wet salt state. If the sulfuric acid smokes for too long, barium sulfate and calcium sulfate will generate barium persulfate and calcium persulfate, which cannot be dissolved by adding hydrochloric acid later, which will affect the measurement result. In addition, there is black residue in the sample in the beaker. After the residue is treated, the calcium and magnesium in the residue are zero. Therefore, it can be said that after a series of acid treatments in the early stage, the calcium and magnesium in the sample have been completely dissolved, so calcium and magnesium can be directly measured later without the need for residue treatment). Remove it, cool it, and carefully add 5mL of hydrochloric acid (65%) along the wall of the cup, and heat to dissolve the salts. Add 50mL of deionized water, adjust the solution pH to about 7 with ammonia (50%), heat the solution on a hot plate and boil it, remove it, filter the test solution into a 250mL volumetric flask with quantitative rapid filter paper, wash the precipitate 7-8 times with ammonium chloride washing solution (1%), and then dilute it with deionized water to the scale, take two 50mL solutions, add 5mL of triethanolamine (25%), 50mL of water, and a little hydroxylamine hydrochloride in a 250mL beaker, add 20mL of potassium hydroxide solution (20%), an appropriate amount of calcium indicator, and titrate with EDTA standard solution until the purple-red color changes to blue as the end point. Add 10mL of ammonia-ammonium chloride buffer solution (pH=10) to the other part, add an appropriate amount of chromium black T indicator, and titrate with EDTA standard solution until the purple-red color changes to blue as the end point.
[0046] The following reagents and equipment are used in the embodiments of the present invention:
[0047] (1) Nitric acid (67%)
[0048] (2) Hydrofluoric acid (40%)
[0049] (3) Sulfuric acid (5%)
[0050] (4) Hydrochloric acid (65%)
[0051] (5) Hydroxylamine hydrochloride (solid)
[0052] (6) Triethanolamine (25%)
[0053] (7) Potassium hydroxide solution (20%)
[0054] (8) Calcein indicator: 1 g calcein and 100 g dried sodium chloride are ground into powder and mixed evenly. The mixture is placed in a ground-mouth bottle for later use.
[0055] (9) EDTA standard solution C(EDTA) = 0.01783 mol / L
[0056] (10) Ammonia-ammonium chloride buffer solution (pH = 10): 67 g of ammonium chloride was dissolved in 200 mL of water, 570 mL of concentrated aqueous ammonia was added, and the solution was diluted to 1000 mL with water.
[0057] (11) Ammonium chloride washing solution (1%)
[0058] (12) Chromium Black T indicator: Grind 1 g of Chromium Black T and 100 g of dried sodium chloride into a fine powder and mix them evenly. Place the mixture in a ground-mouth bottle and set aside.
[0059] The content of the present invention is described in detail below with reference to specific embodiments.
[0060] Embodiment 1:
[0061] 1.1. Weigh 0.2500g of sample
[0062] 1.2. Blank test
[0063] Carry out a blank test along with the sample.
[0064] In a polytetrafluoroethylene beaker, add 10mL hydrochloric acid (65%), add 10mL hydrofluoric acid (40%), dissolve the sample on a low-temperature electric hot plate (100°C), add 5mL nitric acid (67%), add 20mL sulfuric acid (5%), continue heating until the sulfuric acid smokes and the test solution becomes wet salt, remove it, cool it, carefully add 5mL hydrochloric acid (65%) along the wall of the cup, and heat to dissolve the salts. Add 50mL of deionized water, adjust the solution pH to about 7 with ammonia (50%), heat the solution on a hot plate and boil it, remove it, filter the test solution into a 250mL volumetric flask with quantitative rapid filter paper, wash the precipitate 7-8 times with ammonium chloride washing solution (1%), and then dilute it with deionized water to the scale, take two 50mL portions of the solution, add 5mL of triethanolamine (25%), 50mL of water, and a little hydroxylamine hydrochloride in a 250mL beaker, add 20mL of potassium hydroxide solution (20%), an appropriate amount of calcium indicator, and titrate with EDTA standard solution until the color changes from purple to blue. Measure the volume V 01 . Add 10 mL of ammonia-ammonium chloride buffer solution (pH = 10) to the other portion, add an appropriate amount of EDTA indicator, and titrate with EDTA standard solution until the purple-red color changes to blue. Count the volume V 02 .
[0065] 1.3. Sample measurement
[0066] Place the sample m in a polytetrafluoroethylene beaker, add 10mL hydrochloric acid (65%), add 10mL hydrofluoric acid (40%), dissolve the sample on a low-temperature electric hot plate (100°C), and after most of the sample is dissolved, add 5mL nitric acid (67%) and 20mL sulfuric acid (5%), and continue to heat until the sulfuric acid smokes and the test solution becomes wet salt. (This step is critical. Remove the test solution when it becomes wet salt. Do not keep it for too long, otherwise, insoluble calcium pyrosulfate and barium pyrosulfate will be formed, which cannot be dissolved by hydrochloric acid in the next step, affecting the measurement results. In addition, there is black residue in the sample in the beaker. After the residue is treated, the calcium and magnesium in the residue are zero. Therefore, it can be said that after a series of acid treatments in the early stage, the calcium and magnesium in the sample have been completely dissolved, so calcium and magnesium can be directly measured in the later stage without the need for residue treatment.) Remove it, cool it, carefully add 5mL hydrochloric acid (65%) along the wall of the cup, and heat to dissolve the salts. Add 50mL of deionized water, adjust the solution pH to about 7 with ammonia (50%), heat the solution to boil on a hot plate, remove it, filter the test solution into a 250mL volumetric flask with quantitative rapid filter paper, wash the precipitate 7-8 times with ammonium chloride washing solution (1%), and then dilute it with deionized water to the scale. Take two 50mL portions of the solution, add 5mL of triethanolamine (25%), 50mL of water, and a little hydroxylamine hydrochloride in a 250mL beaker, add 20mL of potassium hydroxide solution (20%), and an appropriate amount of calcium indicator, and titrate with EDTA standard solution until the color changes from purple to blue. Measure the volume V Ca . Add 10 mL of ammonia-ammonium chloride buffer solution (pH = 10) to the other portion, add an appropriate amount of EDTA indicator, and titrate with EDTA standard solution until the purple-red color changes to blue. Count the volume V (Mg+Ca) .
[0067] 1.4. Calculation of analysis results
[0068] W(CaO)%=C(V Ca -V 01 )M(CaO)100 / m K×1000
[0069] Where:
[0070] M(CaO): molar mass of calcium oxide (g / mol);
[0071] m: sample mass (g);
[0072] K: sample liquid separation ratio (50 / 250=1 / 5);
[0073] C: EDTA standard solution concentration (mol / L);
[0074] V Ca : Volume of calcium-consumed EDTA standard solution in the sample (mL);
[0075] V 01 : The volume of EDTA standard solution consumed in the blank titration of calcium (mL).
[0076] In some embodiments, the calculation formula for the magnesium oxide content in the sample is:
[0077] W(MgO)%=C(V (Mg+Ca) -V Ca -(V 02 -V 01 )M(MgO)100 / m K×1000
[0078] Where:
[0079] M(MgO): molar mass of magnesium oxide (g / mol);
[0080] m: sample mass (g);
[0081] K: sample liquid separation ratio;
[0082] C: EDTA standard solution concentration (mol / L);
[0083] V (Mg+Ca) : The volume of EDTA standard solution consumed by the total amount of calcium and magnesium (mL);
[0084] V 02 : The volume of blank EDTA standard solution consumed when titrating the total amount of calcium and magnesium (mL).
[0085] Example 2: Accuracy Test
[0086] Accuracy: Since there is no standard sample for dust removal ash and sludge, the sample is dissolved in a platinum crucible, manganese is removed, and interfering elements are separated by ammonia water. The measurement results (W1%) are compared with the results of this method (W2%) as shown in Table 1 below:
[0087] Table 1: Method accuracy experiment
[0088]
[0089] The above data show that the measured data is accurate, and the operation process is short, fast and efficient.
[0090] Example 3: Precision Experiment
[0091] Weigh 11 samples of dust and sludge, and perform precision tests according to the experimental method. The test results are shown in Table 2 below:
[0092] Table 2: Method precision experiment
[0093]
[0094]
[0095] The above data show that the precision of this analytical method is good.
[0096] From the results of the above examples 1-3, it can be seen that the method can accurately determine the content of calcium oxide and magnesium oxide in dust and sludge, greatly shorten the operation time, reduce energy consumption, make the measurement data accurate and reliable, and achieve good results in production.
[0097] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for accurately determining the content of calcium oxide and magnesium oxide in dust and sludge, comprising the following steps: 1) Weigh the sample; 2) Use hydrochloric acid, nitric acid, or hydrofluoric acid to dissolve the sample, add sulfuric acid to generate smoke, and then cool; 3) adding hydrochloric acid to the product obtained in step 2) and heating to dissolve the salts, then adding deionized water and adjusting the solution pH to about 7 with aqueous ammonia, heating and boiling, filtering the solution into a volumetric flask and fixing the volume; 4) Take two equal parts of the solution from the volumetric flask in step 3), add equal amounts of triethanolamine, water and a small amount of hydroxylamine hydrochloride to each of them, add potassium hydroxide solution and an appropriate amount of calcium indicator to one of them, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point, and add ammonia-ammonium chloride buffer solution (pH=10) and a proper amount of chromium black T indicator to the other part, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point; 5) Calculate the contents of calcium oxide and magnesium oxide in the sample based on the titration results obtained in step 4).
2. The method according to claim 1, comprising the steps of: 1) Weigh the sample; 2) Use hydrochloric acid (65%), nitric acid (67%), and hydrofluoric acid (40%) to dissolve the sample, add sulfuric acid to make it smoke, and then cool it; 3) Add hydrochloric acid (65%) to the product obtained in step 2), heat to dissolve the salts, then add deionized water, and adjust the solution pH to about 7 with aqueous ammonia (50%), heat to boil, filter the solution into a volumetric flask and make up to volume; 4) Take two equal parts of the solution from the volumetric flask in step 3), add equal amounts of triethanolamine (25%), water and a small amount of hydroxylamine hydrochloride to each of them, add potassium hydroxide solution and an appropriate amount of calcium indicator to one of them, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point, and add ammonia-ammonium chloride buffer solution (pH=10) and a proper amount of chromium black T indicator to the other part, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point; 5) Calculate the contents of calcium oxide and magnesium oxide in the sample based on the titration results obtained in step 4).
3. The method according to claim 2, comprising the steps of: Weigh 0.2500g of sample m into a polytetrafluoroethylene beaker, add 10mL hydrochloric acid (65%) and 10mL hydrofluoric acid (40%), dissolve the sample on a low-temperature electric hot plate (100°C), and after most of the sample is dissolved, add 5mL nitric acid (67%) and 20mL sulfuric acid (5%), continue heating until the sulfuric acid smokes and the test solution becomes wet salt. Remove it, cool it, and carefully add 5mL hydrochloric acid (65%) along the wall of the cup, and heat to dissolve the salts. Add 50mL of deionized water, adjust the solution pH to about 7 with ammonia water (50%), heat the solution to boil on a hot plate, remove it, filter the test solution into a 250mL volumetric flask with quantitative rapid filter paper, wash the precipitate with ammonium chloride washing solution (1%) 7-8 times, and then dilute it with deionized water to the scale, take two 50mL portions of the solution, add 5mL of triethanolamine (25%), 50mL of water, and a little hydroxylamine hydrochloride in 250mL beakers respectively, add 20mL of potassium hydroxide solution (20%) to one portion, and an appropriate amount of calcium indicator, and titrate with EDTA standard solution until the color changes from purple-red to blue as the end point, and measure the volume V Ca , do a blank test with the sample and calculate the volume V 01 ; Add 10mL of ammonia-ammonium chloride buffer solution (pH=10) to the other portion, add an appropriate amount of EDTA indicator, and titrate with EDTA standard solution until the purple-red color changes to blue as the end point, and measure the volume V (Mg+Ca) , do a blank test with the sample and calculate the volume V 02 .
4. The method according to claim 3, wherein the calculation formula for the calcium oxide content in the sample is: W(CaO)%=C(V Ca -V 01 )M(CaO)100 / m K×1000 Where: M(CaO): molar mass of calcium oxide (g / mol); m: sample mass (g); K: sample liquid separation ratio (50 / 250=1 / 5); C: EDTA standard solution concentration (mol / L); V Ca : Volume of calcium-consumed EDTA standard solution in the sample (mL); V 01 : The volume of EDTA standard solution consumed in the blank titration of calcium (mL).
5. The method according to claim 3 or 4, wherein the calculation formula of the magnesium oxide content in the sample is: W(MgO)%=C(V (Mg+Ca) -V Ca -(V 02 -V 01 )M(MgO)100 / m K×1000 Where: M(MgO): molar mass of magnesium oxide (g / mol); m: sample mass (g); K: sample liquid separation ratio; C: EDTA standard solution concentration (mol / L); V (Mg+Ca) : The volume of EDTA standard solution consumed by the total amount of calcium and magnesium (mL); V 02 : The volume of blank EDTA standard solution consumed when titrating the total amount of calcium and magnesium (mL).
Citation Information
Patent Citations
Determination method of calcium oxide content in open-hearth slag, converter slag and electro-furnace slag
CN104833769A
Method for continuous determination of calcium oxide and magnesium oxide content of limestone and dolomite
CN104977385A
Method for continuously determining content of calcium oxide and magnesium oxide in bentonite
CN105158405A
Measuring method for content of calcium oxide and magnesium oxide in open-hearth furnace slag, converter slag and electric furnace slag
CN105606762A
Method for measuring content of calcium oxide and magnesium oxide in refined slag
CN105651931A