Mask mold spot inhibition method

Through vacuum microwave high-voltage electric field composite processing technology, the sodium ions of the mask plate are migrated to the inside, and combined with nitrogen packaging, the problem of mold points generated during transportation, storage and use of the mask plate is solved, and the length of the mask plate is achieved Effective anti-mold effect and efficient production.

CN119065197APending Publication Date: 2024-12-03CHENGDU ROADWAY OPTOELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411484152.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The mask plate is prone to mold spots during transportation, storage and use. The existing high-temperature drying process leads to low production efficiency and damage to the mask plate. Surfactants can only inhibit mold spots during transportation and cannot prevent storage. and mold spots during use.

Method used

The subsurface layer sodium ions of the mask plate are migrated to the interior by using a vacuum microwave high-voltage electric field environment, combined with nitrogen packaging to reduce moisture and CO2 concentration, and the sodium ion content and moisture content of the mask plate are reduced by the vacuum microwave high-voltage electric field composite treatment process.

Benefits of technology

Effectively prevent the mask plate from producing mildew points during transportation, storage and use, significantly extending the service life, improving production efficiency, ensuring cleanliness and avoiding stress damage caused by high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119065197A_ABST
    Figure CN119065197A_ABST
Patent Text Reader

Abstract

The invention discloses a mask mildew spot inhibition method, which relates to the field of mask cleaning methods, and comprises the step of migrating sodium ions on the subsurface layer of a mask to the inside of the mask by adopting a vacuum microwave high-voltage electric field environment. Sodium ions on the subsurface layer of the mask plate are migrated into the mask plate in a vacuum microwave high-voltage electric field environment, the content of the sodium ions on the surface of the mask plate is reduced to below 1 * 10 <-7 > g per square centimeter, and the content of the sodium ions on the subsurface layer of the mask plate is reduced to 2% of the original content. Compared with the prior art in which the sodium ion content per square centimeter of the surface of the mask which is not treated by the vacuum microwave high-voltage electric field composite treatment process is more than 5 * 10 <-6 > g, the method has obvious advantages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mask cleaning methods, and in particular to a mask mildew spot inhibition method. Background Art

[0002] During the transportation of the mask, whether by air or land, after arriving at the destination, some masks will have dense opaque point crystals with a diameter of 0.3-3um growing on the entire surface or in some areas on the patterned side. At the same time, a large number of opaque point crystals will also grow during storage and use. When observed under an optical microscope, they are similar to mold, which are called mold spots in this patent. Such mold spots will form a large number of defects after exposure by the user.

[0003] In order to solve the above problems, the existing technology uses the method of changing the cleaning process and high-temperature drying to inhibit the growth of mildew spots, using surfactants to clean the mask before shipment and using a drying box to bake the mask. The technical solution is: surfactant cleaning-AOI scanning-high-temperature drying-packaging. The disadvantage is that after the mask is processed: mildew spots will not be generated during the transportation process after processing, but mildew spots will still be generated during long-term storage and use due to contact with moisture in the air, affecting the service life; the high-temperature drying process takes too long, reaching 210 minutes, which is a huge challenge to production efficiency; after processing, it is found that some masks are contaminated by dust particles brought by hot air circulation and cannot meet the cleanliness standard, resulting in mask loss; the highest temperature of the high-temperature drying process reaches more than 200 degrees Celsius, so after high-temperature treatment, it is found that some masks are damaged due to stress changes, resulting in mask loss. Even if the surfactant is used to clean the mask before shipment and high-temperature baking, it can only solve the mildew spots generated during transportation but cannot prevent mildew spots from being generated during storage and use.

[0004] In view of this, this application is filed. Summary of the invention

[0005] The purpose of the present invention is to provide a method for inhibiting mildew spots on a mask plate, by adopting a vacuum microwave high-voltage electric field environment to migrate sodium ions in the sub-surface layer of the mask plate to the inside of the mask plate, so as to solve the problem in the prior art that mildew spots are easily generated on the mask plate during storage and use.

[0006] The present invention is achieved through the following technical solutions: An embodiment of the present invention provides a method for inhibiting mildew spots on a mask, comprising using a vacuum microwave high-voltage electric field environment to migrate sodium ions in the sub-surface layer of the mask toward the interior of the mask.

[0007] Preferably, the inhibition method comprises the following steps:

[0008] S1: Clean the mask to remove pollutants on the surface of the mask;

[0009] S2: Treat the mask in a vacuum microwave high-voltage electric field composite environment to migrate the sodium ions in the sub-surface layer of the mask to the inside of the mask and volatilize the water in the mask;

[0010] S3: Pack the mask after filling the packaging box with nitrogen.

[0011] Preferably, the conditions of the vacuum microwave high-voltage electric field composite environment in S2 include a vacuum degree of 18 to 22 Pa; a microwave frequency of 2 to 3 GHz, a power of 0.8 to 1.2 KW; an electrode voltage of 13 to 17 KV, an ambient temperature below 60° C., and a composite environment treatment time of 4 to 6 min.

[0012] Preferably, the instrument used in S2 is a microwave vacuum drying oven equipped with a high-voltage electrode, and the microwave vacuum drying oven equipped with a high-voltage electrode is used to process the mask after placing a sheet mask inside it. When the mask is processed in a vacuum microwave high-voltage electric field composite environment, the side of the mask with the pattern faces the positive pole of the electrode.

[0013] Preferably, the microwave vacuum drying box equipped with high-voltage electrodes comprises a box body, a microwave magnetron, electrodes, and a plurality of quartz baskets;

[0014] The microwave magnetron is located at the top of the box, the electrodes are located on the left and right sides of the box, and the quartz basket is arranged inside the box; a single quartz basket is used to place a plurality of mask plates, and a single mask plate is arranged vertically, and its edge is perpendicular to the box door of the box.

[0015] Preferably, at least two quartz baskets are provided, and at least two masks are placed in a single quartz basket to process multiple masks in batches, and each mask is placed facing the same direction.

[0016] Preferably, the operation process of the microwave vacuum drying oven equipped with high-voltage electrodes includes:

[0017] Place the quartz basket containing multiple masks into the box and lock the door;

[0018] Vacuuming;

[0019] Start the microwave magnetron;

[0020] Applying electricity to the electrodes generates voltage;

[0021] Treat the mask in a vacuum microwave high voltage electric field composite environment;

[0022] Fill the box with nitrogen to cool it down and break the vacuum. When the temperature of the mask drops to room temperature and the vacuum degree of the box returns to atmospheric pressure, unlock the box door and take out the quartz basket.

[0023] Preferably, the vacuuming time is 50 to 70 seconds, and the vacuum degree reached is 18 to 22 Pa;

[0024] After the microwave magnetron is started, the electrodes are energized for 110 to 130 seconds;

[0025] The time for filling nitrogen into the box to cool down and break the vacuum is 110 to 130 seconds.

[0026] Preferably, after S1 and before S2, the step further includes performing an appearance inspection on the cleaned mask to detect whether the mask has scratches, damages or other surface defects.

[0027] Preferably, after S2 and before S3, the process further includes scanning the mask using an AOI device to ensure the pattern transfer quality of the mask.

[0028] Compared with the prior art, the embodiments of the present invention have the following advantages and beneficial effects:

[0029] 1. The embodiment of the present invention uses a vacuum microwave high-voltage electric field environment to migrate the sodium ions in the sub-surface layer of the mask to the inside of the mask, and the sodium ion content on the mask surface is reduced to 1×10 -7 g, the sodium ion content of the mask subsurface layer is reduced to 2% of the original, compared with the existing technology that the sodium ion content of the mask surface without vacuum microwave high-voltage electric field composite treatment process is 5×10 -6 g and above have significant advantages.

[0030] 2. The vacuum microwave high-voltage electric field composite treatment process provided in the embodiment of the present invention can effectively reduce the sodium ion content in the sub-surface layer of the mask. This is the core element of this process method that prevents the mask from producing mold spots even if it comes into contact with water molecules during transportation, long-term storage, and long-term use, thereby greatly improving the service life of the mask.

[0031] 3. The vacuum microwave high-voltage electric field composite treatment process provided by the embodiment of the present invention reduces the moisture content of the mask to below 0.05% in 10 minutes, while the treatment time using the high-temperature drying process is more than 210 minutes. The vacuum microwave high-voltage electric field composite treatment process takes less time, greatly improving the production efficiency. At the same time, because the process is carried out in a vacuum environment, the cleanliness of the mask can be guaranteed, and no new dust particles will be polluted. The maximum temperature of the mask in this treatment process is 60 degrees Celsius, while the maximum temperature of the high-temperature drying process reaches more than 200 degrees Celsius, so the mask will not be damaged due to stress changes caused by high temperature.

[0032] 4. Through the inhibition method of the embodiment of the present invention, the occurrence rate of mildew spots during transportation and long-term storage of the product is reduced to 0. The effect of not generating mildew spots during transportation and not generating mildew spots during long-term storage, and reducing product losses to 0 is achieved. At the same time, compared with the prior art, even if the mask is in contact with water molecules during transportation, long-term storage, and especially long-term use, mildew spots will not be generated, thereby extending the service life of the mask.

[0033] 5. The moisture content of the mask was measured using the Karl Fischer moisture titration method. The moisture content of the mask that was not treated by the vacuum microwave high-voltage electric field composite treatment process was above 0.2%. After the vacuum microwave high-voltage electric field treatment, the moisture content of the mask was reduced to below 0.05%. The measured value of the water volume ratio of the air in the mask packaging box was as high as 12120PPM. The measured value of the water volume ratio of the high-purity nitrogen used to fill the packaging box by this process method was reduced to 3PPM. The measured value of the CO2 volume ratio in the air in the mask packaging box was as high as 420PPM. The measured value of the CO2 volume ratio in the high-purity nitrogen used to fill the packaging box by this process method was reduced to 0PPM. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0035] Figure 1 A process flow chart provided for an embodiment of the present invention;

[0036] Figure 2 A relationship diagram of mold growth factors provided by an embodiment of the present invention;

[0037] Figure 3A process diagram for processing a mask in a vacuum microwave high-voltage electric field composite environment provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0039] Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Through a large number of experiments and tests, the inventors discovered the theory of five elements for the growth of mildew spots on the mask, namely: (1) sodium ions on the surface of the mask; (2) water molecules in the subsurface layer of the mask after wet cleaning; (3) high ambient humidity; (4) high ambient temperature; (5) CO2 molecules in the environment. Among these five elements, elements 1, 2 and 3 are essential elements, among which element 1 is the core essential element, because sodium ions are the raw material for the first step of the chemical reaction in the production of mildew spots. As long as element 1 still exists, mildew spots will continue to be produced once the mask is exposed to moisture in the air; in addition, as long as elements 1 and 2 or 1 and 3 exist at the same time, mildew spots will be produced; elements 4 and 5 are catalytic elements, which will not cause mildew spots to grow if they exist alone, but the existence of these two elements will shorten the time for mildew spots to be produced, such as Figure 2 shown.

[0041] Finally, through multiple sets of tests and experiments, while balancing operability and production efficiency, we finally adopted a vacuum microwave high-voltage electric field composite treatment process to reduce the sodium ion content in the sub-surface layer of the mask (element 1) and remove the water molecules in the sub-surface layer of the glass, that is, to reduce the water content of the mask (element 2). At the same time, the mask packaging box was filled with dry nitrogen to reduce the ambient humidity and the concentration of CO2 molecules to prevent the formation of mildew spots (element 4, element 5). The most important point is to reduce the sodium ion content in the sub-surface layer of the mask, because sodium ions are the most important raw material in the process of mildew spot formation and the raw material for the first step of the chemical reaction of mildew spot formation. As long as this factor is eliminated, the chemical reaction of the entire mildew spot formation cannot start, thereby ensuring that mildew spots will not be generated during the transportation, storage and use of the mask.

[0042] Therefore, in the combination of elements 1 and 2 or elements 1 and 3, elements 1, 2, and 3 all need to be eliminated, that is, the core essential elements are eliminated, and the combination of other essential elements is not established, and mold spots cannot be produced; among the catalytic elements, element 5 is eliminated, further reducing possible risks.

[0043] Principle of mildew spot generation A: When elements 1 and 2 exist at the same time, the following reaction occurs between the water molecules in the subsurface layer of mildew spot generation and the mask:

[0044]

[0045] The NaOH produced by the reaction continues to corrode the silica gel and mask skeleton on the mask surface:

[0046]

[0047] That is, mildew spots appear on the mask. First, the water molecules in the sub-surface layer of the mask corrode the mask. Then the sodium ions on the surface of the mask form sodium hydroxide to dissolve the mask. The reaction product is the opaque mildew spots.

[0048] Principle B of mildew spot generation: When factors 1 and 3 exist at the same time, the generation of mildew spots makes the surface of the mask plate loose, porous, and cracked in a microscopic structure, with a large surface area and a strong adsorption force on water molecules in the environment; there are unsaturated bonds on the surface of the mask plate, and the active water molecules in the environment will be adsorbed to the surface, which will reduce the surface energy. At the same time, the high humidity of the environment will lead to an increase in the molecular weight of water adsorbed on the surface.

[0049] When a large number of water molecules are adsorbed on the surface of the mask, the following chemical reactions begin to occur:

[0050]

[0051] That is, mildew spots appear on the mask. After the mask absorbs a large amount of water molecules in the environment, ion exchange and hydration reactions occur between the water molecules, sodium ions and glass, and the reaction product is opaque mildew spots.

[0052] Among them, elements 3 and 5 are catalytic elements, which will shorten the time it takes for mold spots to form.

[0053] For factor 4, the temperature of the mask will affect the ion diffusion and ion exchange rate, thereby affecting the erosion rate. The higher the temperature, the higher the ion diffusion and ion exchange rate, the higher the erosion rate, and the easier it is to produce mold spots. The reaction principle is:

[0054]

[0055] For factor 5, CO2 in the air dissolves into the surface film water, which will accelerate the Na + , Ca2+ Mg 2+ The dissolution rate of plasma, and then the erosion rate, provides more sodium ions for the ion exchange reaction, that is, the ion exchange rate will increase, and the mold spots will be generated faster. The reaction principle is:

[0056]

[0057] Therefore, the embodiment of the present invention provides a method for inhibiting mildew spots on a mask, such as Figure 1 As shown, it specifically includes: 1. Cleaning machine cleans the mask; 2. CCD camera performs appearance inspection on the mask; 3. Vacuum microwave high-voltage electric field composite treatment of the mask; 4. AOI equipment scans the mask; 5. The mask packaging box is filled with high-purity nitrogen; 6. Product packaging.

[0058] Among them, the vacuum microwave high-voltage electric field composite treatment of the mask is an innovative process method. The vacuum microwave high-voltage electric field composite treatment uses a microwave vacuum drying oven equipped with high-voltage electrodes. The microwave magnetron of the drying oven is located at the top of the box, and the electrodes are located on the left and right sides of the box. Multiple quartz baskets are used during processing. A single quartz basket can hold multiple masks, so batch processing can be performed. The mask is placed vertically in the drying oven with the edges perpendicular to the door of the drying oven. The most important thing in the operation steps is: all masks are placed in the same direction, that is, the side with the pattern on the mask faces the positive electrode of the electrode, because sodium ions will migrate away from the positive electrode. This operation step is to ensure the correct migration direction of sodium ions, that is, from the sub-surface layer to the inside. According to the production process of the mask raw materials: the sub-surface layer is located on the side of the mask with the pattern. At the same time, according to actual experiments and tests, the effect of this placement direction has been proved, so there is a regulation for this placement direction. The correct placement direction is crucial. Once the placement direction is wrong, it will not only fail to prevent the formation of mildew spots, but also cause mildew spots to form rapidly. The operation process includes:

[0059] 1. Place the quartz basket containing multiple masks into the drying oven in the specified direction (the specified direction is that the side with the pattern on the mask faces the positive electrode), and lock the oven door.

[0060] 2. Press the start button and the drying oven will start running according to the parameters set in the program.

[0061] 3. The first step of the procedure is to evacuate the air, which lasts for 60 seconds until the vacuum degree reaches 20Pa.

[0062] 4. The microwave magnetron starts to start, lasting for 120 seconds, with a microwave frequency of 2.45 GHz and a power of 1 kW.

[0063] 5. After 120 seconds, the high voltage electrode is energized, and the voltage of the high voltage electrode during processing is 15KV.

[0064] 6. At this time, the mask is in a vacuum environment, and microwaves and high-voltage electric fields act simultaneously. The processing time for this step is 5 minutes.

[0065] 7. After the 5-minute treatment process is completed, the drying box is automatically filled with high-purity nitrogen to cool down and break the vacuum. After the built-in infrared thermometer detects that the temperature of the mask has dropped to room temperature and the vacuum degree of the box has returned to atmospheric pressure, the drying box will issue a warning sound to prompt the operator to unlock the door and take out the quartz basket. This process lasts for 120 seconds.

[0066] In general, during the above operation, the high vacuum microwave high voltage electric field composite treatment process is as follows Figure 3 As described above, it is mainly divided into three parts: 1. Vacuum environment, 2. Microwave field, 3. High voltage electric field.

[0067] In the vacuum environment, a large number of gaps are generated by accelerating the evaporation of water molecules on the mask surface and the continuous movement of water molecules inside the mask toward the surface, providing space for sodium ions to migrate into the mask and accelerating the evaporation of water molecules on the surface of the mask. In the microwave field, water molecules on the mask surface enter an excited state and transfer energy to sodium ions to help sodium ions migrate into the mask. Under the action of the microwave field, water molecules inside the mask will continue to migrate toward the surface and evaporate at the same time. In the high-voltage electric field, sodium ions on the mask surface migrate to the mask. Under the action of the high-voltage electric field, the sodium ions migrate at a rate of 1.3×10 -9 cm 2 / (V·s), calculated based on a processing time of 5 minutes, the migration depth of sodium ions on the mask surface to the inside of the mask is 0.000585cm, while the thickness of the mask sub-surface layer is 0.0001cm. According to the calculation results, the sodium ions on the mask surface can completely cross the mask sub-surface layer and migrate into the inside of the mask, eliminating the key raw material of the chemical reaction of sodium ions on the mask surface, thereby avoiding the formation of mildew spots. In addition, according to the actual use, transportation and storage of the mask, no mildew spots are generated on the mask. At the same time, because the mask is in a high-voltage electric field, the water molecules in the sub-surface layer and the internal water molecules migrate to the surface layer under the action of the high-voltage electric field, thereby accelerating evaporation.

[0068] In the embodiment of the present invention, the vacuum microwave high-voltage electric field composite treatment process has the following effects: the surface of the mask is ground, and the sodium ion content in the grinding liquid on the surface of the mask is measured by ion chromatography. The sodium ion content per square centimeter of the mask surface that has not been treated by the vacuum microwave high-voltage electric field composite treatment process is within 5×10 -6 g, after vacuum microwave high-voltage electric field composite treatment, the sodium ion content on the mask surface was reduced to 1×10 per square centimeter. -7g, the sodium ion content of the mask sub-surface layer is reduced to 2% of the original. This data verifies the good effect of vacuum microwave high-voltage electric field composite treatment on sodium ion migration. At the same time, the sodium ion content of the mask sub-surface layer is the core indicator of the vacuum microwave high-voltage electric field composite treatment process. In addition, the water content of the mask that has not been treated by the vacuum microwave high-voltage electric field composite treatment process is above 0.2%. After the vacuum microwave high-voltage electric field treatment, the water content of the mask is reduced to below 0.05%.

[0069] Compared with the high-temperature drying process in the prior art, the vacuum microwave high-voltage electric field composite treatment process in the embodiment of the present invention can effectively reduce the sodium ion content in the sub-surface layer of the mask. This is the core element of the process method in the embodiment of the present invention that ensures that the mask will not produce mold spots even if it comes into contact with water molecules during transportation, long-term storage, and long-term use, thereby greatly improving the service life of the mask.

[0070] The vacuum microwave high-voltage electric field composite treatment process of the embodiment of the present invention reduces the moisture content of the mask to below 0.05% in a processing time of 10 minutes, while the processing time using the high-temperature drying process is more than 210 minutes. The vacuum microwave high-voltage electric field composite treatment process takes less time, greatly improving production efficiency.

[0071] Because the mask plate processed by the vacuum microwave high-voltage electric field composite processing process of the embodiment of the present invention is processed in a vacuum environment, the cleanliness of the mask plate can be guaranteed without additional dust particle pollution.

[0072] During the vacuum microwave high-voltage electric field composite treatment process of the embodiment of the present invention, the maximum temperature of the mask is 60 degrees Celsius, and the maximum temperature of the high-temperature drying process reaches more than 200 degrees Celsius, so the mask will not be damaged due to stress changes caused by high temperature.

[0073] The subsurface layer Na of the mask of the embodiment of the present invention + Quality (10 -6 g / cm 2 ) are shown in Table 1:

[0074] Table 1

[0075]

[0076] As shown in Table 1, the sodium ion content of the mask after vacuum microwave high-voltage electric field composite treatment is lower than 1×10 -7 g, make Na + The migration ability is better than that of high-voltage electric field treatment, high-voltage electric field microwave field treatment, and high-voltage electric field vacuum treatment, because the sub-surface layer of the mask Na +The lower the content, the stronger the ability to prevent mildew growth. The data in Table 1 proves the superiority of the vacuum microwave high-voltage electric field composite process.

[0077] Through a large number of transportation experiments and actual product shipments, the method of the embodiment of the present invention has reduced the incidence of mildew spots on the mask during transportation and long-term storage to 0. The effect of not generating mildew spots during transportation and not generating mildew spots during long-term storage, and reducing product losses to 0, is achieved. At the same time, compared with the prior art, even if the mask contacts water molecules during transportation, long-term storage, and especially long-term use, mildew spots will not be generated, thereby extending the service life of the mask.

[0078] The surface of the mask was ground, and the sodium ion content in the grinding liquid on the mask surface was measured using ion chromatography. The sodium ion content per square centimeter of the mask surface that was not treated by the vacuum microwave high-voltage electric field composite treatment process was 5×10 -6 g, after vacuum microwave high-voltage electric field composite treatment, the sodium ion content on the mask surface was reduced to 1×10 per square centimeter. -7 Below g, the sodium ion content in the mask sub-surface layer is reduced to 2% of the original. This indicator is the core indicator of the vacuum microwave high-voltage electric field composite processing process.

[0079] The moisture content of the mask was measured using the Karl Fischer moisture titration method. The moisture content of the mask that was not treated by the vacuum microwave high-voltage electric field composite treatment process was above 0.2%. After the vacuum microwave high-voltage electric field treatment, the moisture content of the mask was reduced to below 0.05%. The measured value of the water volume ratio of the air in the mask packaging box was as high as 12120PPM. The measured value of the water volume ratio of the high-purity nitrogen used to fill the packaging box by this process method was reduced to 3PPM. The measured value of the CO2 volume ratio in the air in the mask packaging box was as high as 420PPM. The measured value of the CO2 volume ratio in the high-purity nitrogen used to fill the packaging box by this process method was reduced to 0PPM.

[0080] In general, the embodiments of the present invention use the mildew spot inhibition scheme generated by the five-element theory of mildew spots on the mask and the innovative vacuum microwave high-voltage electric field composite treatment process and treatment process adopted thereby, the corresponding process parameters and the control limit standards for the corresponding characteristics of the mask, to achieve precise control of the sodium ion content in the sub-surface layer of the mask, the water content of the mask, the water volume ratio of the gas in the packaging box, and the CO2 volume ratio of the gas in the packaging box while avoiding contamination and damage to the mask that affects the quality of the mask, wherein the core is the control of the sodium ion content in the sub-surface layer of the mask, thereby achieving the avoidance of mildew spots growing on the surface of the mask during transportation, storage, and use; this process method can be used in the field of mask manufacturing; other forms of processing equipment and transformation of the processing process, and other process parameters can be used to replace the treatment method for reducing the surface sodium ion content and water content of the mask, thereby achieving a certain mildew spot prevention effect.

[0081] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for inhibiting mildew spots on a mask, characterized in that: The method includes using a vacuum microwave high-voltage electric field environment to migrate sodium ions in the sub-surface layer of the mask toward the interior of the mask.

2. A method for inhibiting mildew spots on a mask according to claim 1, characterized in that: The following steps are involved: S1: Clean the mask to remove pollutants on the surface of the mask; S2: Treat the mask in a vacuum microwave high-voltage electric field composite environment to migrate the sodium ions in the sub-surface layer of the mask to the inside of the mask and volatilize the water in the mask; S3: Pack the mask after filling the packaging box with nitrogen.

3. A method for inhibiting mildew spots on a mask according to claim 2, characterized in that: The conditions of the vacuum microwave high-voltage electric field composite environment in S2 include a vacuum degree of 18 to 22 Pa; a microwave frequency of 2 to 3 GHz, a power of 0.8 to 1.2 KW; an electrode voltage of 13 to 17 KV, an ambient temperature below 60°C, and a composite environment treatment time of 4 to 6 minutes.

4. A method for inhibiting mildew spots on a mask according to claim 3, characterized in that: The instrument used in S2 is a microwave vacuum drying oven equipped with a high-voltage electrode. The microwave vacuum drying oven equipped with a high-voltage electrode is used to process the mask after placing it inside. When the mask is processed in a vacuum microwave high-voltage electric field composite environment, the side of the mask with the pattern faces the positive pole of the electrode.

5. A method for inhibiting mildew spots on a mask according to claim 4, characterized in that: The microwave vacuum drying box equipped with high-voltage electrodes comprises a box body, a microwave magnetron, electrodes, and a plurality of quartz baskets; The microwave magnetron is located at the top of the box, the electrodes are located on the left and right sides of the box, and the quartz basket is arranged inside the box; a single quartz basket is used to place a plurality of mask plates, and a single mask plate is arranged vertically, and its edge is perpendicular to the box door of the box.

6. A method for inhibiting mildew spots on a mask according to claim 5, characterized in that: At least two quartz baskets are provided, and at least two masks are placed in a single quartz basket to process multiple masks in batches, and each mask is placed facing the same direction.

7. A method for inhibiting mildew spots on a mask according to claim 6, characterized in that: The operation process of the microwave vacuum drying oven equipped with high-voltage electrodes includes: Place the quartz basket containing multiple masks into the box and lock the door; Vacuuming; Start the microwave magnetron; Applying electricity to the electrodes generates voltage; Treat the mask in a vacuum microwave high voltage electric field composite environment; Fill the box with nitrogen to cool it down and break the vacuum. When the temperature of the mask drops to room temperature and the vacuum degree of the box returns to atmospheric pressure, unlock the box door and take out the quartz basket.

8. The method for inhibiting mildew spots on a mask according to claim 7, characterized in that: The vacuuming time is 50 to 70 seconds, and the vacuum degree reached is 18 to 22 Pa; After the microwave magnetron is started, the electrodes are energized for 110 to 130 seconds; The time for filling nitrogen into the box to cool down and break the vacuum is 110 to 130 seconds.

9. The method for inhibiting mildew spots on a mask according to claim 2, characterized in that: After S1 and before S2, the cleaned mask is visually inspected to detect whether there are scratches, damages or other surface defects on the mask.

10. The method for inhibiting mildew spots on a mask according to claim 2, characterized in that: After S2 and before S3, the mask is scanned using AOI equipment to ensure the quality of the mask pattern transfer.