Radiation-sensitive composition, cured film, method for producing cured film, semiconductor element, and display element

By introducing epoxy compounds into the radiation-sensitive linear composition and adopting specific manufacturing methods, the substrate adhesion and gas ejaculation problems are solved, and a high-quality hardened film is achieved, and the performance of semiconductor components and display components is improved.

CN119065201APending Publication Date: 2024-12-03JICC 02 LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410693391.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The conventional sensory radiation-linear compositions lead to poor substrate adhesion and gas ejaculation problems during development, making it difficult to form a high-quality hardened film.

Method used

By introducing an epoxy compound having a specific structure into the radiation-sensitive linear composition, a radiation-sensitive linear composition containing an epoxy group is formed, and a specific manufacturing method includes coating film formation, radiation irradiation, development and heating treatment, To improve substrate adhesion and low gas ejaculation.

Benefits of technology

An excellent hardened film with substrate adhesion and low gas elimination is achieved, the quality of semiconductor components and display components is improved, and efficient pattern formation and heat resistance are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119065201A_ABST
    Figure CN119065201A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a radiation-sensitive composition capable of forming a cured film that can exhibit sensitivity, substrate adhesion, and low gas escape properties at a sufficient level; a cured film formed from the radiation-sensitive composition; a method for producing the cured film; and a semiconductor element and a display element including the cured film. The present invention relates to a radiation-sensitive composition containing: a silicon-containing polymer (A) that is at least one type selected from the group consisting of a polymer containing a structural unit (I) having a group represented by formula (1) and a siloxane polymer; an epoxy group-containing compound (B) having one or more ring structures and two or more epoxy groups (excluding the silicon-containing polymer (A)); and a photoacid generator (C). # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a radiation-sensitive composition, a cured film and a method for producing the same, a semiconductor element and a display element. Background Art

[0002] The cured film (e.g., interlayer insulating film, spacer, protective film, etc.) of a semiconductor element or a display element is generally formed using a radiation-sensitive composition containing a polymer component and a radiation-sensitive compound (e.g., a photoacid generator or a photopolymerization initiator, etc.). For example, after a coating film formed of the radiation-sensitive composition is subjected to radiation irradiation and development treatment to form a pattern, it is subjected to heat treatment to thermally cure it, thereby obtaining a cured film having a pattern shape.

[0003] As a material for forming a cured film of a semiconductor element or a display element, a radiation-sensitive composition is proposed, which includes a polymer having a silicon-containing functional group such as an alkoxysilyl group or a silicon-containing polymer such as a siloxane polymer, and a quinonediazide compound (for example, see Patent Documents 1 and 2).

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 2021-009361

[0007] [Patent Document 2] Japanese Patent Application Publication No. 2011-253035 Summary of the invention

[0008] [Problems to be solved by the invention]

[0009] By using a photosensitive siloxane composition, a cured film having high heat resistance, high transparency, low dielectric constant, high chemical resistance, and high resolution can be formed. However, on the other hand, during the development process, the developer intrudes from the interface between the film and the substrate, sometimes resulting in poor adhesion between the film and the substrate (also called substrate adhesion, development adhesion). In addition, water absorption of the film sometimes causes outgassing.

[0010] An object of the present invention is to provide a radiation-sensitive composition capable of forming a cured film that can exhibit sufficient substrate adhesion and low outgassing properties, a cured film formed from the radiation-sensitive composition, a method for producing the same, and a semiconductor element and a display element including the cured film.

[0011] [Technical means to solve the problem]

[0012] The present inventors have made intensive studies to solve the problems and have found that the above-mentioned object can be achieved by blending an epoxy-group-containing compound having a specific structure into a radiation-sensitive composition, thereby completing the present invention.

[0013] In one embodiment, the present invention relates to a radiation-sensitive composition comprising:

[0014] a silicon-containing polymer (A) which is at least one selected from the group consisting of a polymer containing a structural unit (I) having a group represented by the following formula (1) and a siloxane polymer;

[0015] An epoxy-containing compound (B) having one or more ring structures and two or more epoxy groups (except the silicon-containing polymer (A)); and

[0016] Photoacid generator (C).

[0017] [Chemistry 1]

[0018]

[0019] (In formula (1), R 1 , R 2 and R 3 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. 1 , R 2 and R 3 At least one of them is an alkoxy group having 1 to 6 carbon atoms. "*" indicates a bond)

[0020] In another embodiment, the present invention relates to a method for manufacturing a hardened film, comprising:

[0021] A step of forming a coating film using the radiation-sensitive composition;

[0022] a step of irradiating at least a portion of the coating film with radiation;

[0023] a step of developing the coating film irradiated with radiation; and

[0024] A step of heating the developed coating film.

[0025] In another embodiment, the present invention relates to

[0026] A cured film formed using the radiation-sensitive composition, and a semiconductor element and a display element including the cured film.

[0027] [Effects of the Invention]

[0028] According to the radiation-sensitive composition of the present invention, a cured film that satisfies substrate adhesion and low outgassing can be constructed. The reasons can be inferred as follows. It is believed that the reduction in substrate adhesion during development is caused by the infiltration of the developer from the end of the unexposed portion, but in the present invention, it is believed that the epoxy-containing compound (B) contained in the radiation-sensitive composition has a highly hydrophobic structure, so the substrate interface becomes a hydrophobic environment, which can inhibit the infiltration of the developer during development to the interface between the film and the substrate, and as a result, the reduction in substrate adhesion can be inhibited. In addition, it is believed that the amount of outgassing can also be suppressed by the cross-linking effect of the epoxy-containing compound (B).

[0029] In the method for producing a cured film of the present invention, the radiation-sensitive composition capable of forming a cured film having excellent substrate adhesion and low outgassing is used, so a high-quality cured film can be efficiently formed. The cured film of the present invention uses the radiation-sensitive composition, so it has excellent sensitivity, substrate adhesion, and low outgassing.

[0030] The semiconductor element and the display element of the present invention include a cured film having excellent substrate adhesion and low outgassing properties, and therefore have high quality. DETAILED DESCRIPTION

[0031] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these embodiments. In addition, in this specification, the numerical range described using "to" means that the numerical values ​​described before and after "to" are included as the lower limit and the upper limit. The so-called "structural unit" refers to a unit that mainly constitutes the main chain structure, and refers to a unit that contains at least two or more in the main chain structure.

[0032] In this specification, "hydrocarbon group" means a chain hydrocarbon group, an alicyclic hydrocarbon group and an aromatic hydrocarbon group. The so-called "chain hydrocarbon group" refers to a straight-chain hydrocarbon group and a branched hydrocarbon group that do not contain a cyclic structure on the main chain but only contain a chain structure. Among them, it can be saturated or unsaturated. The so-called "alicyclic hydrocarbon group" refers to a hydrocarbon group that only contains the structure of alicyclic hydrocarbon as a ring structure and does not contain an aromatic ring structure. Among them, it is not necessary to only contain the structure of alicyclic hydrocarbons, and a group having a chain structure in a part thereof is also included. The so-called "aromatic hydrocarbon group" refers to a hydrocarbon group that contains an aromatic ring structure as a ring structure. Among them, it is not necessary to only contain the aromatic ring structure, and a chain structure or an alicyclic hydrocarbon structure may also be included in a part thereof. In addition, the ring structure possessed by the alicyclic hydrocarbon group and the aromatic hydrocarbon group may also have a substituent containing a hydrocarbon structure.

[0033] In this specification, "(meth)acryl" includes "acryl" and "methacryl", "(meth)acrylate" includes "acryl" and "methacrylate", and "(meth)acrylate" includes "acrylate" and "methacrylate".

[0034] 《Radiosensitive composite material》

[0035] The radiation-sensitive composition of the present embodiment (hereinafter, also simply referred to as "composition") contains: at least one silicon-containing polymer (A) selected from the group consisting of a polymer (A-1) containing a structural unit (I) having a group represented by the following formula (1) and a siloxane polymer (A-2);

[0036] An epoxy-containing compound (B) having one or more ring structures and two or more epoxy groups (except the silicon-containing polymer (A)); and

[0037] Photoacid generator (C).

[0038] [Chemistry 2]

[0039]

[0040] (In formula (1), R 1 , R 2 and R 3 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. 1 , R 2 and R 3 At least one of them is an alkoxy group having 1 to 6 carbon atoms. "*" indicates a bond)

[0041] <Silicon-containing polymer (A)>

[0042] The silicon-containing polymer (A) is at least one selected from the group consisting of a polymer (A-1) containing a structural unit (I) having a group represented by the formula (1) and a siloxane polymer (A-2).

[0043] (Polymer (A-1))

[0044] The polymer (A-1) is an aggregate of polymers containing a structural unit (I) having a group represented by the following formula (1) (hereinafter, the aggregate is also referred to as a "base polymer"). It is sufficient that at least one polymer contained in the polymer (A-1) contains the structural unit (I), and it is sufficient that the entire polymer constituting the polymer (A-1) contains the structural unit (I). The polymer (A-1) may also contain structural units other than the structural unit (I).

[0045] [Chemistry 3]

[0046]

[0047] (In formula (1), R 1 , R2 and R 3 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. 1 , R 2 and R 3 At least one of them is an alkoxy group having 1 to 6 carbon atoms. "*" indicates a bond)

[0048] Hereinafter, each structural unit contained in the polymer (A-1) will be described.

[0049] [Structural unit (I)]

[0050] The structural unit (I) has a group represented by the following formula (1).

[0051] [Chemistry 4]

[0052]

[0053] (In formula (1), R 1 , R 2 and R 3 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. 1 , R 2 and R 3 At least one of them is an alkoxy group having 1 to 6 carbon atoms. "*" indicates a bond)

[0054] In formula (1), as R 1 ~R 3 Examples of the alkoxy group having 1 to 6 carbon atoms represented by include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, and tert-butoxy. 1 ~R 3 The alkoxy group represented preferably has 1 to 3 carbon atoms, and is more preferably a methoxy group or an ethoxy group.

[0055] R 1 ~R 3 The alkyl group having 1 to 10 carbon atoms represented by R may be linear or branched. 1 ~R 3 Examples of the alkyl group represented by include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, and the like. 1 ~R 3 The alkyl group represented is preferably a methyl group, an ethyl group or a propyl group.

[0056] R 1 ~R 3At least one of the groups represented by is an alkoxy group having 1 to 6 carbon atoms. From the viewpoint of obtaining a cured film having excellent heat resistance by forming a crosslinked structure, R 1 ~R 3 Two or more of them are alkoxy groups having 1 to 6 carbon atoms, and it is particularly preferred that all of them are alkoxy groups having 1 to 6 carbon atoms. 1 ~R 3 When one or two of the groups are alkoxy groups having 1 to 6 carbon atoms, it is preferred that the remaining group is hydroxyl group or alkyl group having 1 to 10 carbon atoms.

[0057] In the structural unit (I), it is preferred that the group represented by the formula (1) is bonded to an aromatic ring group or a chain hydrocarbon group. In addition, the so-called "aromatic ring group" in this specification refers to a group obtained by removing n (n is an integer) hydrogen atoms from the ring portion of the aromatic ring. Examples of the aromatic ring include: a benzene ring, a naphthalene ring, and an anthracene ring. These rings may also have substituents such as alkyl groups. In the case where the group represented by the formula (1) is bonded to a chain hydrocarbon group, examples of the chain hydrocarbon group include alkanediyl, alkenediyl, etc.

[0058] The group represented by formula (1) is preferably bonded to the benzene ring, naphthalene ring or alkyl chain in the above-mentioned. Specifically, the structural unit (I) preferably has at least one selected from the group consisting of the group represented by the following formula (1-1), the group represented by the following formula (1-2) and the group represented by the following formula (1-3).

[0059] [Chemistry 5]

[0060]

[0061] (In formula (1-1), formula (1-2) and formula (1-3), A 1 and A 2 Each of A is independently a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. n1 is an integer of 0 to 4. n2 is an integer of 0 to 6. When n1 is 2 or more, the plurality of A 1 When n2 is 2 or more, multiple A 2 The same as or different from each other. 6 is an alkanediyl group. 1 , R 2 and R 3 It has the same meaning as the above formula (1). "*" represents a bond)

[0062] In the above formula (1-1) and formula (1-2), regarding A 1 and A 2 Examples of the alkoxy group having 1 to 6 carbon atoms and the alkyl group having 1 to 6 carbon atoms represented by the formula (1) include the following: 1 ~R3 The groups exemplified are the same groups. n1 is preferably 0 or 1, and more preferably 0. n2 is preferably 0 to 2, and more preferably 0.

[0063] In the above formula (1-1) and formula (1-2), except for A 1 and A 2 The bonding position of the other groups other than the above (i.e., the position of the bond indicated by "*"), the group "-SiR 1 R 2 R 3 " can be any position. For example, in the case of the formula (1-1), relative to the position of the bond represented by "*", the group "-SiR 1 R 2 R 3 The position of " can be any one of the ortho, meta and para positions, preferably the para position.

[0064] In the formula (1-3), R 6 From the viewpoint of improving the heat resistance of the obtained cured film, R 6 The carbon number is preferably 1 to 6, and the carbon number is more preferably 1 to 4.

[0065] The structural unit (I) is preferably a structural unit derived from a monomer having a polymerizable carbon-carbon unsaturated bond as a bond participating in polymerization (hereinafter also referred to as an "unsaturated monomer"), and specifically, it is preferably at least one selected from the group consisting of a structural unit represented by the following formula (2-1) and a structural unit represented by the following formula (2-2).

[0066] [Chemistry 6]

[0067]

[0068] (In formula (2-1) and formula (2-2), R A is a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group or a trifluoromethyl group. 7 and R 8 R are each independently a divalent aromatic ring group or a chain hydrocarbon group. 1 , R 2 and R 3 has the same meaning as the above formula (1)

[0069] In the above formula (2-1) and formula (2-2), R 7 , R 8The divalent aromatic ring group represented is preferably a substituted or unsubstituted phenylene group or a substituted or unsubstituted naphthalenediyl group. As the substituent, one or more selected from the group consisting of a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms can be cited. The divalent chain hydrocarbon group is preferably an alkanediyl group having 1 to 6 carbon atoms, and more preferably an alkanediyl group having 1 to 4 carbon atoms.

[0070] As specific examples of the structural unit represented by the formula (2-1), the structural units represented by the following formulas (2-1-1) and (2-1-2) can be listed. In addition, as specific examples of the structural unit represented by the formula (2-2), the structural units represented by the following formulas (2-2-1) and (2-2-2) can be listed.

[0071] [Chemistry 7]

[0072]

[0073] (In formula (2-1-1), formula (2-1-2), formula (2-2-1) and formula (2-2-2), R 1a and R 2a Each R is independently an alkyl group having 1 to 4 carbon atoms. 3a A is an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a hydroxyl group. n3 is an integer of 1 to 4. 1 , A 2 , n1 and n2 have the same meanings as in the above formula (1-1) and formula (1-2). A has the same meaning as the above formula (2-1) and formula (2-2)

[0074] As a specific example of a monomer constituting the structural unit (I),

[0075] Examples of the compound having a group represented by the formula (1-1) include styryltrimethoxysilane, styryltriethoxysilane, styrylmethyldimethoxysilane, styrylethyldiethoxysilane, styryldimethoxyhydroxysilane, styryldiethoxyhydroxysilane, 4-vinylphenyltrimethoxysilane, (meth)acryloxyphenyltrimethoxysilane, (meth)acryloxyphenyltriethoxysilane, (meth)acryloxyphenylmethoxydimethoxysilane, and (meth)acryloxyphenylethyldiethoxysilane.

[0076] Examples of the compound having a group represented by the formula (1-2) include trimethoxy (4-vinyl naphthyl) silane, triethoxy (4-vinyl naphthyl) silane, methyl dimethoxy (4-vinyl naphthyl) silane, ethyl diethoxy (4-vinyl naphthyl) silane, (meth) acrylate oxynaphthyl trimethoxy silane, and the like;

[0077] Examples of the compound having a group represented by the formula (1-3) include (meth)acryloxymethyltrimethoxysilane, (meth)acryloxymethyltriethoxysilane, (meth)acryloxymethylmethyldimethoxysilane, (meth)acryloxymethylmethyldiethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and 4-(meth)acryloxybutyltrimethoxysilane.

[0078] Moreover, as another compound, vinyltrimethoxysilane, vinyltriethoxysilane, etc. are mentioned.

[0079] The polymer (A-1) may contain one type of the structural unit (I) or a combination of two or more types.

[0080] The content ratio of the structural unit (I) relative to all structural units constituting the base polymer (the total content ratio when multiple types are included) is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 15% by mass or more. In addition, the content ratio relative to all structural units constituting the base polymer is preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less. By setting the content ratio of the structural unit (I) to the above range, it is preferred from the viewpoints of sensitivity and low outgassing.

[0081] [Structural unit (II)]

[0082] The polymer (A-1) preferably contains a structural unit derived from unsubstituted maleimide or a structural unit having an acid group as the structural unit (II). By containing the structural unit (II), the solubility (alkali solubility) of the polymer (A-1) in an alkaline developer can be improved, or the hardening reactivity can be improved. In addition, the so-called "alkali soluble" in this specification means that, for example, the polymer (A-1) containing the structural unit (II) can be dissolved or swelled in an alkaline aqueous solution such as an aqueous solution of tetramethylammonium hydroxide at a concentration of 2.38% by mass.

[0083] The structural unit having an acid group in the structural unit (II) is not particularly limited as long as it has an acid group, and is preferably at least one selected from the group consisting of a structural unit having a carboxyl group, a structural unit derived from unsubstituted maleimide, a structural unit having a sulfonic acid group, and a structural unit having a phenolic hydroxyl group, and more preferably a structural unit having a carboxyl group and a structural unit derived from unsubstituted maleimide. In addition, the so-called "phenolic hydroxyl group" in this specification refers to a hydroxyl group directly bonded to an aromatic ring (for example, a benzene ring, a naphthalene ring, an anthracene ring, etc.).

[0084] As the structural unit having an acid group, a structural unit derived from an unsaturated monomer having an acid group is preferred. As a specific example of an unsaturated monomer having an acid group,

[0085] Examples of monomers constituting the structural unit having a carboxyl group include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, and 4-vinylbenzoic acid; and unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, and itaconic acid.

[0086] Examples of the monomer constituting the structural unit having a sulfonic acid group include vinylsulfonic acid, (meth)allylsulfonic acid, styrenesulfonic acid, (meth)acryloyloxyethylsulfonic acid, and the like.

[0087] Examples of the monomer constituting the structural unit having a phenolic hydroxyl group include 4-hydroxystyrene, o-isopropenylphenol, m-isopropenylphenol, p-isopropenylphenol, and hydroxyphenyl (meth)acrylate.

[0088] Examples of the monomer constituting the structural unit derived from unsubstituted maleimide in the structural unit (II) include maleimide.

[0089] Among these, unsaturated monocarboxylic acid and maleimide are preferred, and (meth)acrylic acid and maleimide are more preferred.

[0090] The polymer (A-1) may contain one type of structural unit (II) or a combination of two or more types.

[0091] When the polymer (A-1) contains the structural unit (II), from the viewpoint of imparting good solubility in an alkaline developer, the content ratio of the structural unit (II) relative to all the structural units constituting the base polymer (the total content ratio when a plurality of structural units are included) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, further preferably 1% by mass or more, further more preferably 5% by mass or more, and particularly preferably 10% by mass or more. On the other hand, from the viewpoint of obtaining a good pattern shape, the content ratio of the structural unit (II) relative to all the structural units constituting the base polymer is preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less.

[0092] [Structural unit (III)]

[0093] The polymer (A-1) preferably contains, as the structural unit (III), one or more structural units selected from the group consisting of an oxirane group and an oxetane group. In the present specification, an oxirane group and an oxetane group are also referred to as an "epoxy group".

[0094] By including the structural unit (III) in the polymer (A-1), the resolvability or adhesion of the film can be further improved, which is preferred in this respect. In addition, by the epoxy group acting as a crosslinking group, a hardened film with high chemical resistance and long-term inhibition of degradation can be formed, which is preferred in this respect. The structural unit (III) is preferably a structural unit derived from an unsaturated monomer having an epoxy group, and specifically, it is preferably at least one selected from the group consisting of a structural unit represented by the following formula (3-1) and a structural unit represented by the following formula (3-2).

[0095] [Chemistry 8]

[0096]

[0097] (In formula (3-1) and formula (3-2), R 20 is a monovalent group having an oxetane or an oxetanyl group. A is a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group or a trifluoromethyl group. 1 is a single bond or a divalent linking group)

[0098] In the above formula (3-1) and formula (3-2), R 20 , examples include oxacyclopropyl, oxetanyl, 3,4-epoxycyclohexyl, 3,4-epoxytricyclo[5.2.1.0 2,6 ]decyl, 3-ethyloxetanyl, and the like.

[0099] As X 1 The divalent linking group in is preferably an alkanediyl group such as a methylene group, an ethylene group, or a 1,3-propylene group; or a divalent group in which any methylene group of the alkanediyl group is substituted with an oxygen atom.

[0100] Specific examples of monomers having an epoxy group include glycidyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 2-(3,4-epoxycyclohexyl)ethyl (meth)acrylate, 3,4-epoxytricyclo[5.2.1.0 2,6 ]decyl ester, methacrylate 2-hydroxyethyl [3,4-epoxytricyclo(5.2.1.0 2,6 )decane-9-yl] ester, methacrylate [3,4-epoxytricyclic (5.2.1.0 2,6)decane-9-yl] ester, (3-methyloxetane-3-yl)methyl (meth)acrylate, (3-ethyloxetane-3-yl)methyl (meth)acrylate, (3-ethyloxetane-3-yl)methyl (meth)acrylate, (oxetane-3-yl)methyl (meth)acrylate, 3-(meth)acryloyloxymethyl-3-ethyloxetane, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, and the like.

[0101] The base polymer may contain one type of structural unit (III) or a combination of two or more types.

[0102] When the polymer (A-1) contains a structural unit (III), the content ratio of the structural unit (III) relative to all the structural units constituting the polymer component (the total content ratio when multiple components are included) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and further preferably 1% by mass or more, further more preferably 5% by mass or more, and particularly preferably 10% by mass or more. In addition, the content ratio of the structural unit (III) relative to all the structural units constituting the polymer component is preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less. By setting the content ratio of the structural unit (III) to the range, the coating film shows better resolvability, and the heat resistance and chemical resistance of the obtained cured film can be fully improved, which is preferred in terms of the above aspect.

[0103] [Structural unit (IV)]

[0104] The polymer (A-1) may further include a structural unit (IV) derived from at least one monomer selected from the group consisting of (meth)acrylic acid alkyl esters, (meth)acrylic acid esters having an alicyclic structure, (meth)acrylic acid esters having an aromatic ring structure, aromatic vinyl compounds, N-substituted maleimide compounds, vinyl compounds having a heterocyclic structure, conjugated diene compounds, nitrogen-containing vinyl compounds, and unsaturated dicarboxylic acid dialkyl ester compounds. By introducing these structural units (IV) into the polymer, the glass transition temperature of the polymer (A-1) can be adjusted, and the pattern shape of the obtained cured film can be improved, which is preferred in this respect.

[0105] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-lauryl (meth)acrylate, and n-stearyl (meth)acrylate.

[0106] Examples of the (meth)acrylate having an alicyclic structure include cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, tricyclo[5.2.1.0 2,6 ] decane-8-yl ester, (meth) acrylic acid tricyclo[5.2.1.0 2,5 ]Decan-8-yloxyethyl ester, isobornyl (meth)acrylate, and the like.

[0107] Examples of the (meth)acrylate having an aromatic ring structure include phenyl (meth)acrylate and benzyl (meth)acrylate.

[0108] Examples of the aromatic vinyl compound include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 5-tert-butyl-2-methylstyrene, divinylbenzene, trivinylbenzene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, diphenylethylene, vinylnaphthalene, and vinylpyridine.

[0109] Examples of the N-substituted maleimide compound include N-cyclohexylmaleimide, N-cyclopentylmaleimide, N-(2-methylcyclohexyl)maleimide, N-(4-methylcyclohexyl)maleimide, N-(4-ethylcyclohexyl)maleimide, N-(2,6-dimethylcyclohexyl)maleimide, N-norbornylmaleimide, N-tricyclodecylmaleimide, N-adamantylmaleimide, N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(4-ethylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, N-benzylmaleimide, and N-naphthylmaleimide.

[0110] Examples of the vinyl compound having a heterocyclic structure include tetrahydrofurfuryl (meth)acrylate, tetrahydropyranyl (meth)acrylate, 5-ethyl-1,3-dioxane-5-ylmethyl (meth)acrylate, 5-methyl-1,3-dioxane-5-ylmethyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, 2-(meth)acryloyloxymethyl-1,4,6-trioxaspiro[4,6]undecane, (γ-butyrolactone-2-yl) (meth)acrylate, glycerol carbonate (meth)acrylate, (γ-lactam-2-yl) (meth)acrylate, and N-(meth)acryloyloxyethylhexahydrophthalimide.

[0111] Examples of the conjugated diene compound include 1,3-butadiene and isoprene, examples of the nitrogen-containing vinyl compound include (meth)acrylonitrile and (meth)acrylamide, and examples of the unsaturated dicarboxylic acid dialkyl ester compound include diethyl itaconate. In addition, examples of monomers constituting other structural units include monomers such as vinyl chloride, vinylidene chloride, and vinyl acetate in addition to the above monomers.

[0112] The monomer providing the structural unit (IV) preferably comprises at least one selected from the group consisting of alkyl (meth)acrylates, aromatic vinyl compounds, and N-substituted maleimide compounds, and more preferably comprises at least one selected from the group consisting of methyl (meth)acrylate, styrene, and N-cyclohexylmaleimide.

[0113] The base polymer may contain one type of structural unit (IV) or a combination of two or more types.

[0114] When the polymer (A-1) contains the structural unit (IV), from the viewpoint of appropriately increasing the glass transition temperature of the polymer (A-1), the content ratio of the structural unit (IV) relative to all the structural units constituting the polymer component (the total content ratio when multiple structural units are included) is preferably 1% by mass or more, more preferably 5% by mass or more. In addition, the content ratio is preferably 50% by mass or less, more preferably 40% by mass or less.

[0115] [Other structural units]

[0116] The polymer (A-1) may also contain structural units other than the structural units (I) to (IV). Examples of the structural units other than these include structural units (V) having an acid-dissociable group, and structural units (VI) having a group represented by the following formula (1') (except structural units (I) and (V)).

[0117] [Chemistry 9]

[0118]

[0119] [Structural unit (V)]

[0120] The acid dissociable group is a group that replaces the hydrogen atom possessed by an acidic group such as a carboxyl group, a phenolic hydroxyl group, an alcoholic hydroxyl group, or a sulfonic acid group, and is a group that dissociates by the action of an acid. According to the composition of the present invention, the acid dissociable group is dissociated by the acid generated by irradiating the composition with radiation to generate an acidic group. This is preferred because the solubility of the polymer (A-1) in the developer can be changed, and a hardened film having a pattern can be obtained.

[0121] Among them, the structural unit (V) is preferably a structural unit in which an acid-dissociable group is separated by the action of an acid to generate a carboxyl group (hereinafter also referred to as "structural unit (V-1)"), or a structural unit in which an acid-dissociable group is separated by the action of an acid to generate a phenolic hydroxyl group (hereinafter also referred to as "structural unit (V-2)").

[0122] Examples of the structural unit (V-1) include structural units derived from protected unsaturated carboxylic acids. The unsaturated carboxylic acid used is not particularly limited, and examples thereof include unsaturated monocarboxylic acids, unsaturated dicarboxylic acids, unsaturated acid anhydrides, and unsaturated polycarboxylic acids.

[0123] As specific examples of these, as unsaturated monocarboxylic acids, there can be listed: (meth) acrylic acid, crotonic acid, α-chloroacrylic acid, cinnamic acid, 2-(meth)acryloyloxyethyl-succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl-phthalic acid, (meth)acrylic acid-2-carboxyethyl ester, 4-vinylbenzoic acid, etc. As unsaturated dicarboxylic acids, there can be listed: maleic acid, fumaric acid, itaconic acid, citraconic acid, etc. As unsaturated acid anhydrides, there can be listed: maleic anhydride, itaconic anhydride, citraconic anhydride, etc. As unsaturated polycarboxylic acids, there can be listed: ω-carboxy polycaprolactone mono(meth)acrylate, etc.

[0124] Examples of the acid-dissociable group contained in the structural unit (V-1) include acetal functional groups, tertiary alkyl groups, tertiary alkyl carbonate groups, trialkylsilyl groups, etc. Among these, acetal functional groups are preferred because they are easily dissociated by acid.

[0125] When the acid-dissociable group is an acetal functional group, the structural unit (V-1) preferably has an acetal ester structure of a carboxylic acid as a protected carboxyl group, and specifically, preferably has a group represented by the following formula (X-1).

[0126] [Chemistry 10]

[0127]

[0128] (In formula (X-1), R 31 , R 32 and R 33 It is (1) or (2) below.

[0129] (1)R 31 R is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 32 and R 33 Each independently represents an alkyl group having 1 to 12 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms.

[0130] (2)R 31 R is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 32 and R 33 Indicates the combination with R 32 OR 33 The bonded carbon atoms together form a cyclic ether structure.

[0131] "*" indicates a bond)

[0132] R 31 , R 32 and R 33 The alkyl group having 1 to 12 carbon atoms represented by R may be linear or branched. 31 , R 32 and R 33 Specific examples of the alkyl group having 1 to 12 carbon atoms represented by include R 1 ~R 3 The groups are the same groups as those exemplified in .

[0133] As R 31 , R 32 and R 33 Examples of the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms represented by include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, norbornyl, isobornyl, and adamantyl. 32 and R 33 Examples of the aralkyl group having 7 to 20 carbon atoms include phenylmethyl, phenylethyl, methylphenylmethyl, and the like.

[0134] R 32 and R 33 The cyclic ether structure formed by bonding to each other preferably has a ring member number of 5 or more. Specific examples thereof include a tetrahydrofuran ring structure and a tetrahydropyran ring structure.

[0135] In terms of the ease of acid dissociation, R 31 It is preferably a hydrogen atom, a methyl group or an ethyl group, and more preferably a hydrogen atom.

[0136] Specific examples of the acetal ester structure of carboxylic acid represented by the structural unit (V-1) include 1-methoxyethoxycarbonyl, 1-ethoxyethoxycarbonyl, 1-propoxyethoxycarbonyl, 1-butoxyethoxycarbonyl, 1-cyclohexyloxyethoxycarbonyl, 2-tetrahydrofuranyloxycarbonyl, 2-tetrahydropyranyloxycarbonyl, and 1-phenylmethoxyethoxycarbonyl.

[0137] Among the above, the structural unit (V-1) is preferably a structural unit represented by the following formula (Y-1) and a structural unit represented by the following formula (Y-2).

[0138] [Chemistry 11]

[0139]

[0140] (In formula (Y-1), R 30 X is a hydrogen atom or a methyl group. 30 is a single bond or an arylene group. 40 is a hydrogen atom or an alkyl group. 41 and R 42 are each independently an alkyl group having 1 to 12 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms)

[0141] [Chemistry 12]

[0142]

[0143] (In formula (Y-2), R 30 X is a hydrogen atom or a methyl group. 31 is a single bond or an arylene group. 43 ~R 49 are independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. k is 1 or 2)

[0144] Preferred specific examples of the structural unit (V-1) include structural units represented by the following formulas. In the formula, R 30 A hydrogen atom or a methyl group.

[0145] [Chemistry 13]

[0146]

[0147] The structural unit (V-2) only needs to have a protected phenolic hydroxyl group. Among them, the structural unit (V-2) is preferably at least one selected from the group consisting of structural units derived from hydroxystyrene or its derivatives and structural units derived from (meth)acrylic compounds having a hydroxybenzene structure.

[0148] The acid dissociable group possessed by the structural unit (V-2) is not particularly limited, but is preferably an acetal functional group. The acetal functional group that can be used for the structural unit (V-2) includes the same groups as the acid dissociable groups that can be used for the structural unit (V-1). Among them, the acid dissociable group via "-OC(R 31 )(R 32 )(OR 33 )”(where R 31 , R 32 and R 33 The phenolic hydroxyl group is a phenolic hydroxyl group protected by a group represented by the structural unit (X-1). In this case, the protected phenolic hydroxyl group contained in the structural unit (V-2) can be represented by the following formula (Z-1).

[0149] [Chemistry 14]

[0150]

[0151] (In formula (Z-1), Ar 1 R is an arylene group. 31 , R 32 and R 33 It has the same meaning as formula (X-1). "*" represents a bond)

[0152] As the "-C(R 31 )(R 32 )(OR 33 Preferred specific examples of the group represented by ")" include 1-alkoxyalkyl and 1-arylalkoxyalkyl. Specifically, for example, 1-ethoxyethyl, 1-methoxyethyl, 1-butoxyethyl, 1-isobutoxyethyl, 1-(2-ethylhexyloxy)ethyl, 1-propoxyethyl, 1-cyclohexyloxyethyl, 1-(2-cyclohexylethoxy)ethyl, 1-benzyloxyethyl, etc.

[0153] Preferred specific examples of the structural unit (V-2) include structural units represented by the following formulas. In the formula, R 30 A hydrogen atom or a methyl group.

[0154] [Chemistry 15]

[0155]

[0156] When the polymer (A-1) contains the structural unit (V), it can be added within a range that does not impair the effects of the present invention.

[0157] [Structural unit (VI)]

[0158] The polymer (A-1) may contain a structural unit (VI) having a group represented by the following formula (1').

[0159] [Chemistry 16]

[0160]

[0161] (In formula (1'), R 1 '、R 2 ' and R 3 ' are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a monovalent hydrocarbon group having 1 to 20 carbon atoms, or a group in which a part or all of the hydrogen atoms in the hydrocarbon group are substituted with a substituent. 4 is a divalent aromatic ring group. n3 is 0 or 1. "*" represents a bond. Where n3 is 0, the silicon atom in formula (1') is bonded to the nitrogen atom of the maleimide ring)

[0162] In the formula (1'), R 1 '~R 3 ', as the monovalent hydrocarbon group, there can be listed: a monovalent chain hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 4 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, etc. Specific examples of these, as the chain hydrocarbon group having 1 to 20 carbon atoms, there can be listed: alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and n-pentyl; alkenyl groups such as vinyl and allyl; etc.

[0163] Examples of the alicyclic hydrocarbon group having 4 to 20 carbon atoms include monocyclic alicyclic hydrocarbon groups such as cyclobutyl, cyclopentyl, cyclohexyl, methylcyclohexyl, and cyclooctyl; bicyclo[2.2.2]octyl, tricyclo[5.2.1.0 2,6 ] polycyclic alicyclic hydrocarbon groups such as decyl, adamantyl and norbornyl.

[0164] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include aryl groups such as phenyl, tolyl, xylyl, and naphthyl; and aralkyl groups such as benzyl and phenethyl.

[0165] In R 1 '~R 3 In the case where a part or all of the hydrogen atoms possessed by a hydrocarbon group having 1 to 20 carbon atoms are substituted with a substituent, examples of the substituent include a halogen atom (fluorine atom, chlorine atom, bromine atom, iodine atom, etc.), a hydroxyl group, and the like.

[0166] In the formula (1'), R4 The divalent aromatic ring group in R is a group obtained by removing two hydrogen atoms from the ring part of a substituted or unsubstituted aromatic ring. Examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, and the like. 4 When the aromatic ring has a substituent, examples of the substituent include a halogen atom, an alkyl group, and an alkoxy group.

[0167] The structural unit (VI) preferably has a group in which n3 in the formula (1') is 1, and specifically, preferably has at least one selected from the group consisting of a group represented by the following formula (1'-1) and a group represented by the following formula (1'-2).

[0168] [Chemistry 17]

[0169]

[0170] (In formula (1'-1) and formula (1'-2), A 1 ' and A 2 ' are independently a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. n4 is an integer of 0 to 4. n5 is an integer of 0 to 6. When n4 is 2 or more, multiple A 1 ' are mutually identical groups or different groups. When n5 is 2 or more, multiple A 2 ' are mutually identical groups or different groups. 1 '、R 2 ' and R 3 ' has the same meaning as the above formula (1'). "*" represents a bond)

[0171] In the above formula (1'-1) and formula (1'-2), with respect to A 1 ' and A 2 Specific examples of the alkyl group having 1 to 6 carbon atoms and the alkoxy group having 1 to 6 carbon atoms in the formula (1') include: 1 '~R 3 ' are exemplified by the alkyl group or alkoxy group.

[0172] Compared with A 1 ' and A 2 'Other groups, groups bonded to the aromatic ring "-O-SiR 1 'R 2 'R 3 The position of "" can be any position. For example, in the case of the formula (1'-1), the group "-O-SiR 1 'R 2 'R 3 The position of '" can be any one of the ortho, meta, and para positions, and is preferably the para position.

[0173] The group "-SiR 1 'R 2 'R 3 '" is preferably an acid dissociable group. In structural unit (VI), the group "-SiR 1 'R 2 'R 3 '" functions as an acid-dissociable group, and thus, when n3 in the formula (1') is 1, a phenolic hydroxyl group is generated by the action of an acid generated from the photoacid generator (C) accompanying radiation irradiation, and -NH- is generated when n3 in the formula (1') is 0. As a result, the solubility (alkali solubility) and curing reactivity of the polymer (A-1) in an alkaline developer can be improved. In addition, in this specification, the so-called "acid-dissociable group" is a group that replaces a polar hydrogen atom of a carboxyl group, a hydroxyl group, an amino group, a sulfonic group, etc., and refers to a group that dissociates by the action of an acid. The so-called "alkali-soluble" means, as described above, that the polymer (A-1) can be dissolved or swelled in an alkaline aqueous solution such as an aqueous solution of tetramethylammonium hydroxide at a concentration of 2.38% by mass.

[0174] The structural unit (VI) is preferably a structural unit derived from a monomer having a polymerizable carbon-carbon unsaturated bond. Specifically, the structural unit (VI) is preferably at least one selected from the group consisting of a structural unit represented by the following formula (1'-1A) and a structural unit represented by the following formula (1'-2A).

[0175] [Chemistry 18]

[0176]

[0177] (In formula (1'-1A) and formula (1'-2A), R A is a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group or a trifluoromethyl group. 1 '、R 2 ' and R 3 ' has the same meaning as in the formula (1'). 1 '、A 2 ', n4 and n5 have the same meanings as those in the formula (1'-1) and formula (1'-2))

[0178] Specific examples of monomers providing structural unit (VI) include, as examples when n3 in the formula (1') is 1, 4-isopropenylphenyloxytrimethylsilane, 4-isopropenylphenyloxytriethylsilane, 4-isopropenylphenyloxymethyldiethylsilane, 4-isopropenylphenyloxydimethylethylsilane, 3-isopropenylphenyloxytrimethylsilane, 4-isopropenylnaphthyloxytrimethylsilane, 4-vinylphenyloxytrimethylsilane, 4-vinylphenyloxytriethylsilane, 4-vinylphenyloxymethyldiethylsilane, 4-vinylphenyloxydimethylethylsilane, 3-vinylphenyloxytrimethylsilane, 4-vinylnaphthyloxytrimethylsilane, 4-trimethylsilyloxy-N-phenylmaleimide, and 4-trimethylsilyloxyphenyl (meth)acrylate.

[0179] In addition, examples of the case where n3 in the formula (1′) is 0 include N-trimethylsilylmaleimide, N-triethylsilylmaleimide, and N-methyldiethylsilylmaleimide.

[0180] When the polymer (A-1) contains the structural unit (VI), it can be added within a range that does not impair the effects of the present invention.

[0181] (Method for synthesizing polymer (A-1))

[0182] The polymer (A-1) can be produced, for example, by using an unsaturated monomer capable of introducing the above-mentioned structural units, in a suitable solvent in the presence of a polymerization initiator or the like, according to a known method such as radical polymerization.

[0183] Examples of the polymerization initiator include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(isobutyric acid)dimethyl ester. The polymerization initiator is preferably used in an amount of 0.01 to 30 parts by mass based on 100 parts by mass of the total amount of monomers used in the reaction.

[0184] Examples of the polymerization solvent include alcohols, ethers, ketones, esters, hydrocarbons, etc. The polymerization solvent is preferably used in an amount such that the total amount of monomers used in the reaction is 0.1 to 60% by mass based on the total amount of the reaction solution.

[0185] In the polymerization, the reaction temperature is usually 30°C to 180°C. The reaction time varies depending on the type of polymerization initiator and monomer or the reaction temperature, and is usually 0.5 hours to 10 hours. The polymer obtained by the polymerization reaction can be directly used for the preparation of the radiation-sensitive composition in a state of being dissolved in the reaction solution, or can be used for the preparation of the radiation-sensitive composition after being separated from the reaction solution. The separation of the polymer can be carried out by a known separation method, for example, by a method in which the reaction solution is injected into a large amount of a poor solvent and the precipitate obtained thereby is dried under reduced pressure, or by a method in which the reaction solution is removed by reduced pressure distillation using an evaporator.

[0186] The weight average molecular weight (Mw) of the polymer contained in the polymer component obtained by gel permeation chromatography (GPC) in terms of polystyrene is preferably 2,000 or more. If Mw is 2,000 or more, a cured film having sufficiently high heat resistance or chemical resistance and showing good developability can be obtained, which is preferred in terms of the above aspects. The Mw of the polymer is more preferably 5,000 or more, further preferably 6,000 or more, and particularly preferably 7,000 or more. In addition, from the perspective of making the film-forming property good, Mw is preferably 50,000 or less, more preferably 30,000 or less, further preferably 20,000 or less, and particularly preferably 15,000 or less.

[0187] In addition, the molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight Mw to the number average molecular weight Mn is preferably 4.0 or less, more preferably 3.0 or less, and further preferably 2.5 or less. In addition, when the base polymer comprises two or more polymers, it is preferred that the Mw and Mw / Mn of each polymer satisfy the above ranges.

[0188] (Siloxane polymer (A-2))

[0189] The siloxane polymer (A-2) is not particularly limited as long as it can form a cured film by hydrolysis and condensation. The siloxane polymer (A-2) is preferably a polymer obtained by hydrolyzing a hydrolyzable silane compound represented by the following formula (4).

[0190] (R 21 ) r Si(OR 22 ) 4-r (4)

[0191] (In formula (4), R 21 It is a non-hydrolyzable monovalent group. 22 is an alkyl group having 1 to 4 carbon atoms. r is an integer from 0 to 3. When r is 2 or 3, the multiple R 21When r is 0 to 2, the multiple R 22 Same or different from each other)

[0192] As R 21 Examples thereof include an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a group having a (meth)acryloyl group, and a group having an epoxy group.

[0193] As R 22 , methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, etc. are listed. Among these, R 22 Preferred is methyl or ethyl.

[0194] r is preferably 0 to 2, more preferably 0 or 1, and further preferably 1.

[0195] Specific examples of monomers constituting the siloxane polymer are:

[0196] Examples of the silane compound having four hydrolyzable groups include tetramethoxysilane, tetraethoxysilane, triethoxymethoxysilane, tetrabutoxysilane, tetraphenoxysilane, tetrabenzyloxysilane, and tetra-n-propoxysilane;

[0197] Examples of the silane compound having three hydrolyzable groups include methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, methyltributoxysilane, phenyltrimethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltriisopropoxysilane, ethyltributoxysilane, butyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, and 3-(meth)acryloxypropyltriethoxysilane.

[0198] Examples of the silane compound having two hydrolyzable groups include dimethyldimethoxysilane and diphenyldimethoxysilane;

[0199] Examples of the silane compound having one hydrolyzable group include trimethylmethoxysilane and trimethylethoxysilane.

[0200] The siloxane polymer can be obtained by hydrolyzing and condensing one or more of the hydrolyzable silane compounds with water, preferably in the presence of a suitable catalyst and an organic solvent. During the hydrolysis and condensation reaction, the hydrolyzable group (-OR 22) is 1 mol, and the usage ratio of water is preferably 0.1 mol to 3 mol, more preferably 0.2 mol to 2 mol, and further preferably 0.5 mol to 1.5 mol. By using such an amount of water, the reaction rate of the hydrolysis condensation can be optimized.

[0201] As the catalyst used in the hydrolysis and condensation reaction, for example, there can be mentioned: acid, alkali metal compound, organic base, titanium compound, zirconium compound, etc. The amount of the catalyst used varies depending on the type of catalyst, reaction conditions such as temperature, etc., and can be appropriately set, but is preferably 0.0001 mol to 0.2 mol, more preferably 0.0005 mol to 0.1 mol, relative to 1 mol of the hydrolyzable silane compound.

[0202] As the organic solvent used in the hydrolysis and condensation reaction, for example, hydrocarbons, ketones, esters, ethers, alcohols, etc. are mentioned. Among these, it is preferred to use a water-insoluble or poorly water-soluble organic solvent, for example, ethylene glycol monoalkyl ether acetate, diethylene glycol dialkyl ether, propylene glycol monoalkyl ether, propylene glycol monoalkyl ether acetate, propionate compounds, etc. The use ratio of the organic solvent is preferably 10 to 10,000 parts by mass, and more preferably 50 to 1,000 parts by mass, relative to a total of 100 parts by mass of the hydrolyzable silane compound used in the reaction.

[0203] During the hydrolysis and condensation reaction, the reaction temperature is preferably set to 130°C or less, more preferably 40°C to 100°C. The reaction time is preferably set to 0.5 hours to 24 hours, more preferably 1 hour to 12 hours. During the reaction, the mixed solution may be stirred or placed under reflux. After the hydrolysis and condensation reaction, a dehydrating agent may be added to the reaction solution, followed by evaporation, thereby removing water and the generated alcohol from the reaction system.

[0204] For siloxane polymers, the weight average molecular weight (Mw) converted to polystyrene obtained by GPC is preferably 500 or more. If Mw is 500 or more, a cured film having sufficiently high heat resistance or solvent resistance and showing good developability can be obtained, which is preferred in terms of the above aspects. Mw is more preferably 1000 or more. In addition, from the perspective of making film-forming properties good and suppressing the reduction of radiation sensitivity, Mw is preferably 10000 or less, and more preferably 5000 or less. In addition, the molecular weight distribution (Mw / Mn) is preferably 4.0 or less, more preferably 3.0 or less, and further preferably 2.5 or less.

[0205] The content of the silicon-containing polymer (A) is preferably 20% by mass or more, more preferably 30% by mass or more, and further preferably 50% by mass or more relative to the total amount of solid components contained in the radiation-sensitive composition (i.e., the total mass of components other than the solvent in the radiation-sensitive composition). In addition, the content of the polymer (A) is preferably 99% by mass or less, more preferably 95% by mass or less relative to the total amount of solid components contained in the radiation-sensitive composition. By setting the content of the polymer (A) to the above range, a cured film having sufficiently high heat resistance and chemical resistance and showing good developability and transparency can be obtained.

[0206] <Epoxy group-containing compound (B)>

[0207] The radiation-sensitive composition contains the silicon-containing polymer (A) and the epoxy-containing compound (B). The epoxy-containing compound (B) is not particularly limited as long as it has one or more ring structures and two or more epoxy groups. The silicon-containing polymer (A) is excluded. The epoxy-containing compound (B) has two or more epoxy groups and is therefore a component that causes a cross-linking reaction and promotes the curing reaction of the radiation-sensitive composition.

[0208] The epoxy group-containing compound (B) may be a low molecular weight compound (for example, a molecular weight of less than 1000) or a high molecular weight compound (for example, a molecular weight of 1000 or more, and in the case of a polymer, a weight average molecular weight of 1000 or more).

[0209] The number of epoxy groups in the epoxy-group-containing compound (B) may be two or more, and is preferably three or more from the viewpoint of substrate adhesion.

[0210] The number of the ring structures of the epoxy-containing compound (B) may be one or more, and is preferably three or more from the viewpoint of substrate adhesion.

[0211] The ring structure may be any one of an alicyclic structure, an aromatic ring structure, a heterocyclic structure or a combination thereof. In the case of a combination, the ring structure may be a structure bonded in a chain structure, and two or more ring structures may also form a condensed ring structure or a bridged ring structure. In addition, the hydrogen atoms on the carbon atoms of the ring structure may also be substituted by other substituents.

[0212] Examples of the alicyclic structure include n-valent alicyclic hydrocarbon groups having 3 to 20 carbon atoms. The n-valent alicyclic hydrocarbon group refers to a group obtained by removing n (n is an integer) hydrogen atoms from an alicyclic hydrocarbon. In addition, it may be any of a saturated hydrocarbon group and an unsaturated hydrocarbon group. Examples of the alicyclic hydrocarbon include cycloalkanes such as cyclopropane, cyclobutane, cyclopentane, cyclohexane, norbornane, and adamantane, and cycloalkenes such as cyclopropene, cyclobutene, cyclopentene, cyclohexene, and norbornene.

[0213] Examples of the aromatic ring structure include n-valent aromatic hydrocarbon groups having 6 to 30 carbon atoms. The n-valent aromatic hydrocarbon group refers to a group obtained by removing n (n is an integer) hydrogen atoms from an aromatic hydrocarbon. Examples of the aromatic hydrocarbon include benzene, toluene, xylene, mesitylene, naphthalene, methylnaphthalene, dimethylnaphthalene, anthracene, and the like.

[0214] As the heterocyclic structure, a group obtained by removing n hydrogen atoms from an aromatic heterocyclic structure and a group obtained by removing n hydrogen atoms from an alicyclic heterocyclic structure can be cited. By introducing a heteroatom, an aromatic structure having a 5-membered ring with aromaticity is also included in the heterocyclic structure. As the heteroatom, an oxygen atom, a nitrogen atom, a sulfur atom, etc. can be cited.

[0215] Examples of the aromatic heterocyclic structure include: aromatic heterocyclic structures containing oxygen atoms such as furan, pyran, benzofuran, and benzopyran; aromatic heterocyclic structures containing nitrogen atoms such as pyrrole, imidazole, pyridine, pyrimidine, pyrazine, indole, quinoline, isoquinoline, acridine, phenazine, and carbazole; and aromatic heterocyclic structures containing sulfur atoms such as thiophene.

[0216] Aromatic heterocyclic structures containing multiple heteroatoms such as thiazole, benzothiazole, thiazine, and oxazine.

[0217] Examples of the alicyclic heterocyclic structure include: an alicyclic heterocyclic structure containing an oxygen atom such as tetrahydrofuran, tetrahydropyran, dioxolane, and dioxane; an alicyclic heterocyclic structure containing a nitrogen atom such as aziridine, pyrrolidine, piperidine, and piperazine; an alicyclic heterocyclic structure containing a sulfur atom such as thietane, thiolane, and thiazane; an alicyclic heterocyclic structure containing multiple heteroatoms such as morpholine, 1,2-oxathiolane, and 1,3-oxathiolane; a lactone structure, a cyclic carbonate structure, and a sultone structure.

[0218] The ring structure is preferably an n-valent alicyclic hydrocarbon group having 3 to 20 carbon atoms or an n-valent aromatic hydrocarbon group having 6 to 30 carbon atoms. The alicyclic hydrocarbon is preferably cyclohexane, and the aromatic hydrocarbon is preferably benzene.

[0219] Specific examples of the epoxy group-containing compound (B) include: bisphenol A type epoxy compounds, hydrogenated bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, hydrogenated bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, hydrogenated bisphenol S type epoxy compounds, bisphenol AD ​​type epoxy compounds, hydrogenated bisphenol AD ​​type epoxy compounds, novolac type epoxy compounds, cyclic aliphatic epoxy compounds, heterocyclic epoxy compounds, glycidyl ester type compounds, tetraglycidylamine type epoxy compounds, tetraphenylethane type epoxy compounds , epoxidized oils, epoxy novolac compounds and their bromides; trisphenol type epoxy compounds; tris(glycidylphenyl)methane, triglycidyl isocyanurate and other epoxy-containing compounds; 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexane-m-dioxane, bis(3,4-epoxycyclohexylmethyl)adipate, vinylcyclohexene dioxide, bis(3,4-epoxy-6-methylcyclohexyl)methacrylate Alicyclic epoxy compounds such as 1,4-butylene glycol diglycidyl ether, 1,6-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,6-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,6-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,6-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,6-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,6-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,4-butylene glycol diglycidyl ether, 1,6 - Polyglycidyl ethers of polyhydric alcohols such as hexanediol diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, polyethylene glycol diglycidyl ether, and polypropylene glycol diglycidyl ethers; diglycidyl esters of aliphatic long-chain dibasic acids; monoglycidyl ethers of aliphatic higher alcohols; monoglycidyl ethers of phenol, cresol, butylphenol, or polyether alcohols obtained by adding alkylene oxide to these; glycidyl esters of higher fatty acids; epoxidized soybean oil, butyl epoxystearate, octyl epoxystearate, epoxidized linseed oil, etc. Among these, at least one selected from the group consisting of novolac type epoxy compounds, bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, tetraglycidylamine type epoxy compounds, tetraphenylethane type epoxy compounds, hydrogenated bisphenol A type epoxy compounds, and trisphenol type epoxy compounds is preferred from the viewpoint of solubility in an alkaline developer.

[0220] As the epoxy equivalent of the epoxy-containing compound (B), it is not particularly limited, preferably 80g / equivalent or more, more preferably 100g / equivalent or more. In addition, it is preferably 1000g / equivalent or less, more preferably 800g / equivalent or less, and further preferably 500g / equivalent or less. By the epoxy equivalent of the epoxy-containing compound (B) being in the range, a cured film with low water absorption and excellent thermal crosslinking can be obtained, so it is preferred. The epoxy equivalent here can be measured according to JISK7236.

[0221] The epoxy group-containing compound (B) preferably contains at least one compound selected from the group consisting of compounds represented by the following formula (B1) to formula (B8).

[0222] [Chemistry 19]

[0223]

[0224]

[0225] (In formula (B3), i is an integer from 0 to 300)

[0226] [Chemistry 20]

[0227]

[0228] (In formula (B4), j is an integer from 0 to 300)

[0229] [Chemistry 21]

[0230]

[0231] (In formula (B5), R 11 independently represent a hydrogen atom, a halogen atom or a methyl group, and k is an integer from 0 to 100)

[0232] [Chemistry 22]

[0233]

[0234] [Chemistry 23]

[0235]

[0236] (In formula (B7), m is an integer from 0 to 50)

[0237] [Chemistry 24]

[0238]

[0239] (In formula (B8), p is an integer from 0 to 300)

[0240] The compounds represented by the formula (B3) to (B5), (B7) and (B8) may be mixtures of two or more compounds having different values ​​of i, j, k, m or p.

[0241] Examples of commercially available products of the formula (B1) include JER1032H60 (manufactured by Mitsubishi Chemical Corporation), examples of commercially available products of the formula (B2) include YH-434 (manufactured by Nippon Steel Chemical & Materials Corporation), examples of commercially available products of the formula (B3) include JER834, JER828, and JER1001 (all manufactured by Mitsubishi Chemical Corporation), and examples of commercially available products of the formula (B4) include YX8000 (manufactured by Mitsubishi Chemical Corporation). As a commercial product of the formula (B5), JER152 (manufactured by Mitsubishi Chemical Co., Ltd.) can be cited, as a commercial product of the formula (B6), JER1031S (manufactured by Mitsubishi Chemical Co., Ltd.) can be cited, as a commercial product of the formula (B7), JER157S65 (manufactured by Mitsubishi Chemical Co., Ltd.) can be cited, and as a commercial product of the formula (B8), JER806 (manufactured by Mitsubishi Chemical Co., Ltd.) can be cited. The epoxy group-containing compound (B) can be used alone or in combination of two or more.

[0242] Relative to 100 parts by mass of silicon-containing polymer (A), the content of epoxy-containing compound (B) (total content in the case of containing multiple) is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 5 parts by mass or more. In addition, relative to 100 parts by mass of silicon-containing polymer (A), preferably 50 parts by mass or less, more preferably 30 parts by mass or less, further preferably 20 parts by mass or less, particularly preferably 15 parts by mass or less. By setting the addition amount of epoxy-containing compound (B) to the range, the overall effects of sensitivity, substrate adhesion and outgassing can be balanced, which is preferred from the viewpoint.

[0243] <Photoacid generator (C)>

[0244] The radiation-sensitive composition contains the polymer (A), the epoxy-containing compound (B), and the photoacid generator (C) together.

[0245] The photoacid generator (C) is not particularly limited as long as it is a compound that generates an acid by radiation irradiation. Examples of the photoacid generator (C) include oxime sulfonate compounds, onium salts, sulfonimide compounds, halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonate compounds, carboxylate compounds, and quinonediazide compounds.

[0246] Specific examples of oxime sulfonate compounds, onium salts, sulfonimide compounds, halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonate compounds, and carboxylate compounds include compounds described in paragraphs

[0078] to

[0106] of Japanese Patent Application Laid-Open No. 2014-157252, compounds described in International Publication No. 2016 / 124493, etc. As the photoacid generator, from the viewpoint of radiation sensitivity, it is preferred to use at least one selected from the group consisting of oxime sulfonate compounds and sulfonimide compounds.

[0247] The oxime sulfonate compound is preferably a compound having a sulfonate group represented by the following formula (5).

[0248] [Chemistry 25]

[0249]

[0250] (In formula (5), R 23 It is a monovalent hydrocarbon group, or a monovalent group in which a part or all of the hydrogen atoms of the hydrocarbon group are substituted by a substituent. "*" represents a bond)

[0251] In the formula (5), R 23 Examples of the monovalent hydrocarbon group include alkyl groups having 1 to 20 carbon atoms, cycloalkyl groups having 4 to 12 carbon atoms, and aryl groups having 6 to 20 carbon atoms. Examples of the substituent include alkyl groups having 1 to 5 carbon atoms, alkoxy groups having 1 to 5 carbon atoms, pendant oxygen groups, and halogen atoms.

[0252] Examples of oxime sulfonate compounds include (5-propylsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (5-octylsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (camphorsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (5-p-toluenesulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (2-[2-(4-methylphenylsulfonyloxyimino)]-2,3-dihydrothiophen-3-ylidene)-2-(2-methylphenyl)acetonitrile, 2-(octylsulfonyloxyimino)-2-(4-methoxyphenyl)acetonitrile, and compounds described in International Publication No. 2016 / 124493. Examples of commercially available products of the oxime sulfonate compound include Irgacure PAG121 manufactured by BASF.

[0253] Examples of sulfonyl imide compounds include N-(trifluoromethylsulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, N-(4-methylphenylsulfonyloxy)succinimide, N-(2-trifluoromethylphenylsulfonyloxy)succinimide, N-(4-fluorophenylsulfonyloxy)succinimide, N-(trifluoromethylsulfonyloxy)phthalimide, N-(camphorsulfonyloxy)phthalimide, imide, N-(2-trifluoromethylphenylsulfonyloxy)phthalimide, N-(2-fluorophenylsulfonyloxy)phthalimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(camphorsulfonyloxy)diphenylmaleimide, N-(4-methylphenylsulfonyloxy)diphenylmaleimide, trifluoromethanesulfonic acid-1,8-naphthalimide (N-hydroxynaphthalimide trifluoromethanesulfonate).

[0254] As the photoacid generator (C), one or more of oxime sulfonate compounds, onium salts, sulfonimide compounds, halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonate compounds, and carboxylate compounds may be used in combination with the quinonediazide compound. Alternatively, the quinonediazide compound may be used alone.

[0255] Quinonediazide compounds are radiation-sensitive acid generators that generate carboxylic acids by irradiation with radiation. Examples of quinonediazide compounds include condensates of phenolic compounds or alcoholic compounds (hereinafter also referred to as "mother core") and o-naphthoquinonediazide compounds. Among these, the quinonediazide compound used is preferably a condensate of a compound having a phenolic hydroxyl group as a mother core and an o-naphthoquinonediazide compound. As specific examples of the mother core, for example, compounds described in paragraphs 0065 to 0070 of Japanese Patent Laid-Open No. 2014-186300 can be cited. The o-naphthoquinonediazide compound is preferably 1,2-naphthoquinonediazidesulfonyl halide.

[0256] As the quinonediazide compound, a condensate of a phenolic compound or an alcoholic compound as a mother core and 1,2-naphthoquinonediazidesulfonyl halide can be preferably used, and a condensate of a phenolic compound and 1,2-naphthoquinonediazidesulfonyl halide can be more preferably used.

[0257] Specific examples of quinonediazide compounds include 4,4'-dihydroxydiphenylmethane, 2,3,4,2',4'-pentahydroxybenzophenone, 2,3,4,4'-tetrahydroxybenzophenone, tris(p-hydroxyphenyl)methane, 1,1,1-tris(p-hydroxyphenyl)methane, 1,1,1-tris(p-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,3-bis[1-(4-hydroxyphenyl)-1-methane] An ester compound of a phenolic hydroxyl group-containing compound among 1,4-bis[1-(4-hydroxyphenyl)-1-methylethyl]benzene, 1,4-bis[1-(4-hydroxyphenyl)-1-methylethyl]benzene, 4,6-bis[1-(4-hydroxyphenyl)-1-methylethyl]-1,3-dihydroxybenzene and 4,4'-[1-[4-[1-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol and 1,2-naphthoquinonediazide-4-sulfonyl chloride or 1,2-naphthoquinonediazide-5-sulfonyl chloride.

[0258] In the condensation reaction for obtaining the condensate, regarding the ratio of the mother core to the 1,2-naphthoquinonediazidesulfonyl halide, the amount of the 1,2-naphthoquinonediazidesulfonyl halide used is set to an amount corresponding to preferably 30 mol% to 85 mol%, more preferably 50 mol% to 70 mol%, relative to the number of OH groups in the mother core. In addition, the condensation reaction can be carried out according to a known method.

[0259] Relative to 100 parts by mass of the silicon-containing polymer (A), the content of the photoacid generator (C) (the total content when multiple types are included) is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and further preferably 0.1 parts by mass or more. In addition, relative to 100 parts by mass of the silicon-containing polymer (A), the content of the photoacid generator (C) is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and further preferably 5 parts by mass or less. If the content of the photoacid generator (C) is set to 0.01 parts by mass or more, the acid is fully generated by the irradiation of radiation, and the difference in solubility in alkaline solution between the irradiated part and the unirradiated part of the radiation can be fully increased. Thus, good patterning can be performed, so it is preferred. In addition, the amount of acid participating in the reaction with the polymer component can be increased, and heat resistance and solvent resistance can be fully ensured, so it is preferred. On the other hand, by setting the content of the photoacid generator (C) to 20 parts by mass or less, the amount of unreacted photoacid generator after exposure can be sufficiently reduced, and a decrease in developability due to the remaining photoacid generator (C) can be suppressed, which is preferred.

[0260] The radiation-sensitive composition of the present invention may contain the silicon-containing polymer (A), the epoxy-containing compound (B), and the photoacid generator (C), and other components are not particularly limited. For example, from the viewpoint of improving substrate adhesion, it is preferred to contain a adhesion aid (D) or an orthoester compound (E), and from the viewpoint of coating properties, it is preferred to contain a solvent (F).

[0261] <Adhesion aid (D)>

[0262] The adhesion aid (D) is a component that improves the adhesion between the cured film formed using the radiation sensitive composition and the substrate. As the adhesion aid (D), for example, a cardo compound having a cardo structure or a functional silane coupling agent having a reactive functional group can be preferably used.

[0263] (Functional silane coupling agent)

[0264] Examples of the reactive functional group possessed by the functional silane coupling agent include a carboxyl group, a (meth)acryloyl group, an epoxy group, a vinyl group, and an isocyanate group.

[0265] Specific examples of the functional silane coupling agent include trimethoxysilylbenzoic acid, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, vinyltriacetoxysilane, vinyltrimethoxysilane, and 3-isocyanatopropyltriethoxysilane.

[0266] (Cardo compounds)

[0267] The cardo compound has at least one functional group (X) selected from the group consisting of an alkoxysilyl group, an oxirane group, an oxetane group, a mercapto group, a (meth)acryloyl group, a vinyl group, and an amino group, and a cardo structure.

[0268] The cardo structure has a first ring structure, a second ring structure and a third ring structure, and has a structure in which the second ring structure and the third ring structure are directly bonded to the same carbon atom contained in the ring skeleton of the first ring structure. Specifically, the cardo structure can be represented by the following formula (10).

[0269] [Chemistry 26]

[0270]

[0271] (In formula (10), A 10 For A 11 and A 12 The carbon atoms bonded together form a cyclic group. 11 and A12 are independently divalent cyclic groups. "*" represents a bond)

[0272] In the formula (10), A 11 and A 12 The divalent cyclic group represented may be any of an alicyclic group and an aromatic ring group. The alicyclic group is a group obtained by removing two hydrogen atoms from the ring part of a substituted or unsubstituted aliphatic hydrocarbon ring, and may be any of a monocyclic hydrocarbon group and a polycyclic hydrocarbon group. In the case where the divalent alicyclic group is a polycyclic hydrocarbon group, the polycyclic hydrocarbon group may be any of a bridged alicyclic hydrocarbon group and a condensed alicyclic hydrocarbon group, and may also be any of a saturated hydrocarbon group and an unsaturated hydrocarbon group. In addition, the so-called condensed alicyclic hydrocarbon group refers to a polycyclic alicyclic hydrocarbon group composed of a plurality of alicyclic rings sharing a side (a bond between two adjacent carbon atoms).

[0273] Specific examples of monocyclic alicyclic hydrocarbon groups include cyclopentanediyl, cyclohexanediyl, cycloheptanediyl, and cyclooctanediyl as saturated hydrocarbon groups; cyclopentenyl, cyclohexenyl, cycloheptenediyl, cyclooctenyl, cyclopentadienyl, and cyclohexadienyl as unsaturated hydrocarbon groups. Specific examples of polycyclic alicyclic hydrocarbon groups include bicyclo[2.2.1]heptane-2,2-diyl (norbornane-2,2-diyl), bicyclo[2.2.2]octane-2,2-diyl, and tricyclo[3.3.1.1 3,7 ]decane-2,2-diyl (adamantane-2,2-diyl) and the like; examples of the condensed alicyclic hydrocarbon group include decahydronaphthalenediyl and the like.

[0274] The divalent aromatic ring group is a group obtained by removing two hydrogen atoms from a substituted or unsubstituted aromatic ring, and may be either monocyclic or polycyclic. When the divalent aromatic ring group is a polycyclic hydrocarbon group, the polycyclic hydrocarbon group may be either a bridged aromatic hydrocarbon group or a condensed aromatic hydrocarbon group.

[0275] Specific examples of the monocyclic aromatic hydrocarbon group include phenylene, etc. The polycyclic aromatic hydrocarbon group is preferably a condensed aromatic ring hydrocarbon group, and examples thereof include naphthalenediyl, anthracenediyl, fluorenediyl, and phenenediyl.

[0276] When the divalent alicyclic group and the aromatic ring group have a substituent in the ring portion, examples of the substituent include an alkyl group having 1 to 6 carbon atoms, a halogen atom, a cyano group, and the like.

[0277] Among them, A 11 and A 12 The divalent cyclic group represented is preferably a divalent aromatic cyclic group, and particularly preferably a substituted or unsubstituted phenylene group.

[0278] A 10For A 11 and A 12 The carbon atoms bonded together form a cyclic group. 10 Specific examples of the cyclic group represented by include the following: 11 and A 12 The divalent alicyclic group and the divalent aromatic ring group exemplified as the divalent cyclic group represented by 10 Preferred specific examples of the cyclic group represented by include groups represented by the following formulae (10a-1) to (10a-6) and groups in which a substituent is introduced into the ring part of these groups.

[0279] [Chemistry 27]

[0280]

[0281] (Wherein, “*” represents a bond)

[0282] In the above, as A 10 The cyclic group represented is preferably a group represented by the formula (10a-1) to the formula (10a-3) respectively and a group having a substituent introduced into the ring part of these, and is particularly preferably a group having a fluorene structure (that is, a group represented by the formula (10a-1) and a group having a substituent introduced into the ring part).

[0283] In terms of high effects of improving substrate adhesion and cured adhesion of a film obtained using the composition of the present invention, the cardo structure represented by the formula (10) is preferably a structure represented by the following formula (10-1).

[0284] [Chemistry 28]

[0285]

[0286] (In formula (10-1), Ar 11 and Ar 12 are each independently a divalent aromatic ring group. 68 and R 69 Each of a1 and a2 is independently an integer of 0 to 3. When a1 is 2 or 3, a plurality of R 68 The same or different. When a2 is 2 or 3, multiple R 69 Same or different. "*" indicates a bond)

[0287] The functional group (X) possessed by the cardo compound is at least one selected from the group consisting of an alkoxysilyl group, an oxirane group, an oxetane group, a mercapto group, a (meth)acryloyl group, a vinyl group, and an amino group.

[0288] The alkoxysilyl group may have a structure in which an alkoxy group is bonded to a silicon atom, for example, the formula "-Si(R 61 )(R 62 )(R 63 Here, R 61 , R 62 and R 63 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group, and R 61 , R 62 and R 63 At least one of them is an alkoxy group having 1 to 6 carbon atoms. Specific examples of the alkoxysilyl group include the same groups as those represented by the above formula (1). 61 , R 62 and R 63 Preferably, one is an alkoxy group having 1 to 6 carbon atoms and the rest are alkoxy groups having 1 to 6 carbon atoms or alkyl groups having 1 to 10 carbon atoms. Among them, R is preferably 61 , R 62 and R 63 One of the groups is an alkoxy group having 1 to 3 carbon atoms, and the rest are alkoxy groups having 1 to 3 carbon atoms or alkyl groups having 1 to 3 carbon atoms.

[0289] In terms of making the substrate adhesion and curing adhesion of the film obtained using the composition of the present invention better, the functional group (X) is preferably at least one selected from the group consisting of an alkoxysilyl group, an oxirane group, an oxetane group and a (meth)acryloyl group, and is particularly preferably an alkoxysilyl group.

[0290] The cardo compound contained in the present composition only needs to have one or more cardo structures and functional groups (X) in one molecule, and the structures of other parts are not particularly limited. As cardo compounds, for example, oligomers containing structural units having a cardo structure and silane coupling agents having a cardo structure can be listed. Specifically, cardo compounds can include compounds represented by the following formula (11) and compounds represented by the following formula (12). In addition, as cardo compounds, photosensitive resins obtained by adding carboxylic acid-reactive (meth)acrylate compounds to polymer compounds obtained by reacting a compound having a fluorene skeleton with a tetrabasic acid dianhydride as described in International Publication No. 2009 / 119622 can be used. For example, the photosensitive resin (A2) described in Example 2 of the said gazette can be used.

[0291] [Chemistry 29]

[0292]

[0293] (In formula (11), Y 61 and Y 62 Each independently represents a divalent organic group having 1 or more carbon atoms. 61 and X 62 b1 and b2 are each independently an integer of 1 to 5. Ar 11 ,Ar 12 , R 68 , R 69 , a1 and a2 have the same meaning as in the formula (10-1))

[0294] [Chemistry 30]

[0295]

[0296] (In formula (12), Y 63 and Y 64 Each independently represents a divalent organic group having 1 or more carbon atoms. 61 and X 63 Each of Ar is independently an alkoxysilyl group, an oxirane group, an oxetanyl group, a mercapto group, a (meth)acryloyl group, a vinyl group or an amino group. n1 is an integer of 2 to 100. 11 ,Ar 12 , R 68 , R 69 , a1 and a2 have the same meaning as in the formula (10-1))

[0297] In the above formula (11) and formula (12), Y 61 ~Y 64 The divalent organic group represented by the formula (I) may be a divalent hydrocarbon group having 1 to 40 carbon atoms, or a divalent group in which at least one methylene group of the hydrocarbon group is substituted by a heteroatom-containing group. Examples of the heteroatom-containing group include -O-, -S-, -CO-, -COO-, -OCO-, -NR 67 CO-、-CONR 67 -、-NR 67 -COO-, -OCO-NR 67 - etc. (where R 67 is a hydrogen atom or an alkyl group).

[0298] In terms of further improving the substrate adhesion and cured adhesion of the film formed from the composition of the present invention, the cardo compound is preferably a compound represented by the formula (11), and particularly preferably X in the formula (11): 61 and X 62 An alkoxysilyl compound.

[0299] As the cardo compound, a commercially available product may be used. Commercially available products of the cardo compound include, by trade name, Ogsol SC-001, Ogsol EA-0200, Ogsol EA-0300, and Ogsol CR1030 (all manufactured by Osaka Gas Chemical Co., Ltd.); WR-301 (manufactured by ADEKA Co., Ltd.); V-259ME (manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.); Oncoat EX series (manufactured by Nagase Chemtex Co., Ltd.); and the like.

[0300] In the case of mixing a close contact aid (D) in the radiation-sensitive composition of the present invention, the content of the close contact aid (D) (the total content when multiple materials are included) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and further preferably 1 part by mass or more, and particularly preferably 3 parts by mass or more, relative to 100 parts by mass of the silicon-containing polymer (A). In addition, the content of the close contact aid (D) is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and further preferably 10 parts by mass or less, relative to 100 parts by mass of the silicon-containing polymer (A). By setting the content of the close contact aid (D) to the range, the substrate adhesion of the film formed by the composition of the present invention is further improved, so it is preferred.

[0301] <Orthoester compound (E)>

[0302] As the orthoester compound (E), it is a compound having three groups "-OR 30 ”(Among them, R 30 A compound having a structure in which a monovalent hydrocarbon group is bonded to the same carbon, and having the general formula: R 31 -C(OR 30 )3 represents. Here, R 31 It is a hydrogen atom or a monovalent organic group. The orthoester compound (E) exhibits water absorption in the presence of an acid and becomes an ester after hydrolysis. By including such an orthoester compound (E) together with the silicon-containing polymer (A) in the radiation-sensitive composition, the water absorption effect of the orthoester compound (E) is exhibited by utilizing the acid generated by the self-photoacid generator (C) (in other words, irradiation with radiation), and the water absorption effect of the orthoester compound (E) can be used to improve the development adhesion of the coating film, so it is preferred. In addition, the orthoester compound (E) is stable to an alkaline developer, is hydrophobic, and has a small effect on the unexposed part (for example, the effect on the sensitivity).

[0303] As the orthoester compound has the group "-OR 30", for example, methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, tert-butoxy, n-pentyloxy, phenoxy, methylphenyl, etc. Among these, the group "-OR 30 " is preferably an alkoxy group, and more preferably an alkoxy group having 1 to 4 carbon atoms. In addition, the three groups "-OR 30 " are the same group or different groups.

[0304] As R 31 , for example, a hydrogen atom, a monovalent chain hydrocarbon group, a halogenated chain hydrocarbon group in which at least one hydrogen atom of the chain hydrocarbon group is substituted by a halogen atom, a monovalent aromatic ring group, etc. 31 Preferred are hydrogen atoms, monovalent chain hydrocarbon groups or monovalent aromatic ring groups, and specific examples thereof include hydrogen atoms, alkyl groups having 1 to 20 carbon atoms, alkenyl groups having 2 to 20 carbon atoms, and aryl groups having 6 to 20 carbon atoms.

[0305] Specific examples of the orthoester compound (E) include triethyl orthochloroacetate, trimethyl orthoformate, triethyl orthoformate, tripropyl orthoformate, triisopropyl orthoformate, tributyl orthoformate, diethylphenyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, triethyl orthodichloroacetate, trimethyl orthobutyrate, triethyl orthobutyrate, trimethyl orthopropionate, triethyl orthopropionate, trimethyl orthovalerate, triethyl orthovalerate, trimethyl orthoisobutyrate, trimethyl orthobenzoate, and triethyl orthobenzoate.

[0306] As the orthoester compound, the compound represented by the following formula (6) can be preferably used among the above.

[0307] R 33 -C-(OR 32 )3(6)

[0308] (In formula (6), R 32 R is an alkyl group having 1 to 4 carbon atoms or a phenyl group. 33 is a hydrogen atom, a monovalent chain hydrocarbon group having 1 to 4 carbon atoms, or a monovalent aromatic ring group having 6 to 12 carbon atoms. 32 are the same group or different groups)

[0309] In the formula (6), R 32 The alkyl group in R may be linear or branched. In terms of improving the development adhesion of the coating film and having a smaller influence on the sensitivity, R 32 Preferred is a methyl group, an ethyl group or a phenyl group, and more preferred is a methyl group or an ethyl group.

[0310] R 33 The chain hydrocarbon group in is preferably a chain or branched alkyl group having 1 to 4 carbon atoms.33 The aromatic ring group in R includes, for example, phenyl, methylphenyl, dimethylphenyl, ethylphenyl, naphthyl, etc. In terms of the high effect of improving the development adhesion of the coating film, R 33 A monovalent aromatic ring group is preferred, and a phenyl group is particularly preferred.

[0311] In order to further improve the development adhesion of the coating film, as the orthoester compound (E), a compound having an aromatic ring group can be preferably used. Specific examples of the compound having an aromatic ring group include: 32 and R 33 In addition, when the orthoester compound (E) has an aromatic ring, the orthoester compound (E) is likely to remain in the film due to the improved hydrophobicity of the orthoester compound (E), which is believed to be caused by sufficient dehydration of the end of the unexposed part.

[0312] Specific examples of the orthoester compound (E) having an aromatic ring group include trimethyl orthobenzoate, triethyl orthobenzoate, diethylphenyl orthoformate, etc. Among these, trimethyl orthobenzoate and triethyl orthobenzoate are particularly preferred in terms of their high effect of improving the development adhesion of the coating film and the ability to better maintain sensitivity.

[0313] The orthoester compound (E) preferably has a boiling point higher than the prebaking temperature. By using an orthoester compound (E) having a sufficiently high boiling point relative to the prebaking temperature, the development adhesion of the coating film can be further improved. Specifically, the boiling point of the orthoester compound (E) is preferably above 105°C, more preferably above 110°C, and further preferably above 115°C. In addition, when the boiling point of the orthoester compound (E) is sufficiently high relative to the prebaking temperature, the volatilization of the orthoester compound (E) is suppressed during prebaking, and the orthoester compound (E) is easily retained in the film even after prebaking, which is believed to be caused by sufficient dehydration of the end of the unexposed portion.

[0314] Specific examples of the orthoester compound (E) having a boiling point of 105° C. or higher include triethyl orthoformate, tripropyl orthoformate, tributyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, triethyl orthodichloroacetate, trimethyl orthobutyrate, trimethyl orthopropionate, triethyl orthopropionate, trimethyl orthovalerate, trimethyl orthobenzoate, triethyl orthobenzoate, etc. In addition, in this specification, the boiling point is a value at one atmospheric pressure.

[0315] When an orthoester compound (E) is added to the radiation-sensitive composition of the present invention, the content of the orthoester compound (E) (the total content when multiple types are included) is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and further preferably 10 parts by mass or more, relative to 100 parts by mass of the silicon-containing polymer (A). In addition, the content of the orthoester compound (E) is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and further preferably 20 parts by mass or less, relative to 100 parts by mass of the silicon-containing polymer (A). By setting the content of the orthoester compound (E) to the above range, the substrate adhesion of the film formed by the composition of the present invention is further improved, so it is preferred.

[0316] <Solvent (F)>

[0317] The radiation sensitive composition of the present invention is a liquid composition in which the formulated components are preferably dissolved or dispersed in a solvent (F). The solvent (F) used is preferably an organic solvent that dissolves the components formulated in the radiation sensitive composition of the present invention and does not react with the components.

[0318] Specific examples of the solvent (F) include: alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; esters such as ethyl acetate, butyl acetate, ethyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, 3-methoxypropionic acid methyl ester, and 3-ethoxypropionic acid ethyl ester; ethers such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, ethylene glycol ethyl methyl ether, diethylene glycol ethyl methyl ether, dimethylene glycol dimethyl ether, diethylene glycol dimethyl ether, and diethylene glycol ethyl methyl ether; amides such as dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene. Among these, the solvent (F) preferably contains at least one selected from the group consisting of ethers and esters, and more preferably contains at least one selected from the group consisting of ethylene glycol alkyl ether acetate, diethylene glycols, propylene glycol monoalkyl ether, and propylene glycol monoalkyl ether acetate.

[0319] The radiation sensitive composition of the present invention may appropriately contain, for example, an acid diffusion controller in addition to the above-mentioned components.

[0320] <Acid diffusion control agent>

[0321] The acid diffusion controller is a component that controls the diffusion length of the acid generated from the photoacid generator (C) by exposure. By adding the acid diffusion controller to the radiation sensitive composition, the diffusion length of the acid can be appropriately controlled, and the pattern developing property can be improved, which is preferred.

[0322] As the acid diffusion control agent, any one of the basic compounds used in the chemically amplified resist can be selected and used. Examples of the basic compound include fatty acid amines, aromatic amines, heterocyclic amines, quaternary ammonium hydroxides, quaternary ammonium carboxylates, and the like. Specific examples of the basic compound include compounds described in

[0128] to

[0147] of Japanese Patent Laid-Open No. 2011-232632. As the acid diffusion control agent, at least one selected from the group consisting of aromatic amines and heterocyclic amines can be preferably used.

[0323] Examples of the aromatic amine and the heterocyclic amine include aniline derivatives such as aniline, N-methylaniline, N-ethylaniline, N-propylaniline, N,N-dimethylaniline, 2-methylaniline, 3-methylaniline, 4-methylaniline, ethylaniline, propylaniline, trimethylaniline, 2-nitroaniline, 3-nitroaniline, 4-nitroaniline, 2,4-dinitroaniline, 2,6-dinitroaniline, 3,5-dinitroaniline, and N,N-dimethyltoluidine; imidazole derivatives such as imidazole, 4-methylimidazole, 4-methyl-2-phenylimidazole, benzimidazole, 2-phenylbenzimidazole, triphenylimidazole, and N-(tert-butoxycarbonyl)-2-phenylbenzimidazole; pyrrole, 2H-pyrrole, 1-methylpyrrole, 2,4-dimethylpyrrole, Pyrrole derivatives such as methylpyrrole, 2,5-dimethylpyrrole, and N-methylpyrrole; pyrrole derivatives such as pyridine, methylpyrrole, ethylpyridine, propylpyridine, butylpyridine, 4-(1-butylpentyl)pyridine, dimethylpyridine, trimethylpyridine, triethylpyridine, phenylpyridine, 3-methyl-2-phenylpyridine, 3-methyl-4-phenylpyridine, 4-tert-butylpyridine, diphenylpyridine, benzylpyridine, methoxypyridine, butoxypyridine, dimethoxypyridine, 1-methyl-2-pyridone, 4-pyrrolidinylpyridine, 1-methyl-4-phenylpyridine, 2-(1-ethylpropyl)pyridine, aminopyridine, dimethylaminopyridine, nicotine, and compounds described in Japanese Patent Laid-Open No. 2011-232632.

[0324] When an acid diffusion controller is added to the radiation-sensitive composition, the content of the acid diffusion controller is preferably 0.001 parts by mass or more, more preferably 0.005 parts by mass or more, and further preferably 0.01 parts by mass or more, relative to 100 parts by mass of the silicon-containing polymer (A). In addition, the content of the acid diffusion controller is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and further preferably 2 parts by mass or less, relative to 100 parts by mass of the silicon-containing polymer (A).

[0325] <Other ingredients>

[0326] The radiation sensitive composition of the present invention may contain, in addition to the above-mentioned components, for example, an antioxidant, a crosslinking agent, etc. as appropriate.

[0327] <Method for preparing radiation-sensitive composition>

[0328] The radiation-sensitive composition can be prepared, for example, by mixing a silicon-containing polymer (A), an epoxy-containing compound (B), a photoacid generator (C), and any other optional components as required in a prescribed ratio. The radiation-sensitive composition is preferably filtered using a filter having a pore size of about 0.05 μm to 0.4 μm after mixing. The solid content concentration of the radiation-sensitive composition (the ratio of the total mass of the components other than the solvent in the radiation-sensitive composition to the total mass of the radiation-sensitive composition) can be appropriately selected in consideration of viscosity or volatility. The solid content concentration of the radiation-sensitive composition is preferably in the range of 5% to 60% by mass, more preferably 10% to 55% by mass, and further preferably 12% to 50% by mass. If the solid content concentration is 5% by mass or more, the film thickness of the coating can be fully ensured when the radiation-sensitive composition is applied to the substrate. In addition, if the solid content concentration is 60% by mass or less, the film thickness of the coating will not be too large, and the viscosity of the radiation-sensitive composition can be appropriately increased, thereby ensuring good coating properties.

[0329] 《Curing film and its manufacturing method》

[0330] The cured film of the present invention is formed by a radiation-sensitive composition prepared as described above. The radiation-sensitive composition has high radiation sensitivity. In addition, by using the radiation-sensitive composition, a pattern film having high adhesion to the substrate and excellent low outgassing can be formed even after development. Therefore, the radiation-sensitive composition can be preferably used as a forming material for, for example, an interlayer insulating film, a planarizing film, a spacer, a protective film, a color pattern film for a color filter, a partition wall, a bank, etc.

[0331] When producing a cured film, the radiation-sensitive composition is used, and thus a positive-type cured film can be formed depending on the type of photosensitizer. The cured film can be produced by a method including, for example, the following steps 1 to 4 using the radiation-sensitive composition.

[0332] (Step 1) A step of forming a coating film using the radiation sensitive composition.

[0333] (Step 2) A step of irradiating at least a portion of the coating film with radiation.

[0334] (Step 3) A step of developing the coating film irradiated with radiation.

[0335] (Step 4) A step of heating the developed coating film.

[0336] Hereinafter, each step will be described in detail.

[0337] [Step 1: coating step]

[0338] In this process, the radiation-sensitive composition is applied to the surface on which the film is to be formed (hereinafter also referred to as the "film-forming surface"), and preferably the solvent is removed by heat treatment (pre-baking) to form a coating on the film-forming surface. The material of the film-forming surface is not particularly limited. For example, in the case of forming an interlayer insulating film, the radiation-sensitive composition is applied to a substrate provided with a switching element such as a thin film transistor (TFT) to form a coating. As the substrate, for example, a glass substrate, a silicon substrate, or a resin substrate is used. On the surface of the substrate on which the coating is to be formed, a metal thin film may be formed according to the application, and various surface treatments such as hexamethyldisilazane (HMDS) treatment may be performed.

[0339] As the coating method of the radiation-sensitive composition, for example, there can be mentioned: spraying, roller coating, spin coating, slit die coating, rod coating, inkjet method, etc. Among these, it is preferably carried out by spin coating, slit die coating or rod coating. The pre-baking conditions also vary according to the types and content ratios of the components of the radiation-sensitive composition, for example, 0.5 minutes to 10 minutes at 60°C to 130°C. The film thickness of the formed coating (i.e., the film thickness after pre-baking) is preferably 0.1μm to 12μm. For the radiation-sensitive composition applied to the film-forming surface, it can also be dried under reduced pressure (vacuum drying (Vacuum Dry, VCD)) before pre-baking.

[0340] [Process 2: Exposure process]

[0341] In this process, at least a portion of the coating formed in the process 1 is irradiated with radiation. At this time, by irradiating the coating with radiation through a mask having a specified pattern, a cured film with a pattern can be formed. As radiation, for example, charged particle beams such as ultraviolet rays, far ultraviolet rays, visible rays, X-rays, and electron beams can be listed. Among these, ultraviolet rays are preferred, for example, g-rays (wavelength 436nm) and i-rays (wavelength 365nm) can be listed. As the exposure amount of radiation, 0.1J / m 2 ~20,000J / m 2 .

[0342] [Process 3: Development process]

[0343] In this process, the coating film irradiated with radiation in the process 2 is developed. Specifically, the coating film irradiated with radiation in the process 2 is developed with a developer to remove the irradiated part of the radiation. As a developer, for example, an aqueous solution of an alkali (alkaline compound) can be cited. As an alkali, for example, sodium hydroxide, tetramethylammonium hydroxide, and the alkali illustrated in paragraph

[0127] of Japanese Patent Laid-Open No. 2016-145913 can be cited. As the alkali concentration of the aqueous alkali solution, from the perspective of obtaining appropriate developability, it is preferably 0.1% by mass to 5% by mass. As a developing method, for example, a suitable method such as a coating method, an immersion method, a shaking immersion method, and a spray method can be cited. The developing time also varies according to the composition of the composition, for example, 30 seconds to 120 seconds. In addition, it is preferred that after the developing process, the patterned coating film is rinsed with running water.

[0344] [Step 4: Heating step]

[0345] In this step, a treatment (post-baking) of heating the developed coating film in the step 3 is performed. Post-baking can be performed using a heating device such as an oven or a hot plate. Regarding the post-baking conditions, the heating temperature is, for example, 120° C. to 250° C. For example, when the heating treatment is performed on a hot plate, the heating time is 5 minutes to 40 minutes, and when the heating treatment is performed in an oven, the heating time is 10 minutes to 80 minutes.

[0346] By carrying out the above-mentioned process, a cured film having a target pattern can be formed on the substrate. The shape of the pattern of the cured film is not particularly limited, and examples thereof include line and space patterns, dot patterns, hole patterns, and lattice patterns.

[0347] Semiconductor Components

[0348] The semiconductor element of the present invention includes a cured film formed using the radiation-sensitive composition. The cured film is preferably an interlayer insulating film for insulating wiring in the semiconductor element. The semiconductor element of the present invention can be manufactured using a known method.

[0349] Display Components

[0350] The display element of the present invention includes a cured film formed using the radiation-sensitive composition. In addition, the display element of the present invention may also include a cured film formed using the radiation-sensitive composition by including the semiconductor element of the present invention. In addition, the display element of the present invention may also include a planarization film formed on a TFT substrate as a cured film formed using the radiation-sensitive composition. As display elements, for example, liquid crystal display elements and organic electroluminescence (EL) display elements can be cited.

[0351] [Example]

[0352] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. In addition, the "parts" and "%" in the examples and comparative examples are based on mass unless otherwise specified. In the present examples, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the polymer are measured by the following method.

[0353] [Weight average molecular weight (Mw) and number average molecular weight (Mn)]

[0354] The Mw and Mn of the polymer were measured by the following method.

[0355] ·Determination method: Gel permeation chromatography (GPC)

[0356] · Equipment: GPC-101 manufactured by Showa Denko Co., Ltd.

[0357] ·GPC column: Combination of GPC-KF-801, GPC-KF-802, GPC-KF-803 and GPC-KF-804 manufactured by Shimadzu GLC Co., Ltd.

[0358] Mobile phase: Tetrahydrofuran

[0359] Column temperature: 40℃

[0360] Flow rate: 1.0mL / min

[0361] Sample concentration: 1.0 mass%

[0362] Sample injection volume: 100μL

[0363] Detector: Differential refractometer

[0364] ·Standard material: monodisperse polystyrene

[0365] <Monomers constituting polymer (A)>

[0366] The abbreviations of monomers used in the synthesis of the polymer (A) are as follows.

[0367] (Providing a monomer of structural unit (I))

[0368] ·MPTMS: 3-methacryloxypropyltrimethoxysilane

[0369] ·MPTES: 3-methacryloxypropyltriethoxysilane

[0370] ·STMS: p-phenylenedimethoxysilane

[0371] ·SDMS: p-Styrene dimethoxy hydroxy silane

[0372] ·STES: p-Styrene triethoxysilane

[0373] (Providing a monomer of structural unit (II))

[0374] MA: Methacrylic acid

[0375] MI: Maleimide

[0376] (Providing a monomer of structural unit (III))

[0377] OXMA: OXE-30 (3-ethyloxetane-3-yl)methyl methacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.)

[0378] ·GMA: Glycidyl methacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.)

[0379] EDCPMA: methacrylic acid [3,4-epoxytricyclic (5.2.1.0 2,6 )decane-9-yl] ester

[0380] (Providing a monomer of structural unit (IV))

[0381] MMA: Methyl methacrylate

[0382] ·ST:Styrene

[0383] <Synthesis of polymer (A)>

[0384] [Synthesis Example 1] Synthesis of polymer (A-1)

[0385] Into a flask equipped with a cooling tube and a stirrer, 10 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) and 200 parts of diethylene glycol methyl ether were added. Subsequently, 20 parts of 3-methacryloxypropyltrimethoxysilane, 15 parts of methacrylic acid, 30 parts of (3-ethyloxetane-3-yl)methyl methacrylate, 30 parts of glycidyl methacrylate, and 5 parts of methyl methacrylate were added, and after nitrogen substitution, the temperature of the solution was raised to 70°C while slowly stirring, and the temperature was maintained for 5 hours, thereby obtaining a polymer solution containing polymer (A-1). The solid content concentration of the polymer solution was 34.0% by mass, and the Mw of the polymer (A-1) was 10,800, and the molecular weight distribution (Mw / Mn) was 2.1.

[0386] [Synthesis Examples 2 to 14, Comparative Synthesis Examples 1, Comparative Synthesis Examples 2] Synthesis of Polymers (A-2) to (A-14), Polymer (CA-1), Polymer (CA-2)

[0387] The same method as in Synthesis Example 1 was used except that the components of the types and blending amounts (parts by mass) shown in Table 1 were used to obtain polymer solutions containing polymers (A-2) to (A-14), polymer (CA-1), and polymer (CA-2) having the same solid content concentration, weight average molecular weight, and molecular weight distribution as polymer (A-1). In addition, "-" in Table 1 indicates that the corresponding component was not used.

[0388] [Table 1]

[0389]

[0390] [Synthesis Example 15] Synthesis of polymer (A-15)

[0391] Into a flask equipped with a cooling tube and a stirrer, 24 parts of propylene glycol monomethyl ether, 39 parts of methyltrimethoxysilane and 18 parts of 3-methacryloxypropyltrimethoxysilane were added, and the solution temperature was heated to 60°C. After the solution temperature reached 60°C, 0.1 parts of formic acid and 19 parts of water were added, and the solution temperature was raised to 75°C while slowly stirring, and the temperature was maintained for 2 hours. After cooling to 45°C, 28 parts by mass of trimethyl orthoformate was added as a dehydrating agent, and the solution was stirred for 1 hour. The solution temperature was further brought to 40°C, and the solution was evaporated while maintaining the temperature to remove water and methanol generated in the hydrolysis and condensation, thereby obtaining a polymer solution containing a polymer (A-15). The solid content concentration of the polymer solution was 35% by mass, and the weight average molecular weight (Mw) of the polymer (A-15) was 1,800, and the molecular weight distribution (Mw / Mn) was 2.2.

[0392] [Synthesis Example 16] Synthesis of polymer (A-16)

[0393] A polymer (A-16) having the same solid content concentration, weight average molecular weight and molecular weight distribution as those of the polymer (A-15) was obtained by the same method as in Synthesis Example 1, except that the monomers used were changed to 39 parts of phenyltrimethoxysilane and 18 parts of 3-methacryloxypropyltrimethoxysilane.

[0394] <Preparation of radiation-sensitive composition>

[0395] The polymer (A), epoxy group-containing compound (B), photoacid generator (C), and additive (X) used for preparing the radiation-sensitive composition are shown below.

[0396] (Polymer (A))

[0397] A-1 to A-16: polymers (A-1) to (A-16) synthesized in Synthesis Examples 1 to 16

[0398] CA-1 to CA-2: polymer (CA-1) and polymer (CA-2) synthesized in Comparative Synthesis Examples 1 to 2

[0399] (Epoxy-containing compound (B))

[0400] B-1: JER834 (manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent: 230-270, a compound corresponding to formula (B3))

[0401] B-2: JER828 (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 184 to 194, a compound corresponding to formula (B3))

[0402] B-3: JER1001 (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 475, a compound corresponding to formula (B3))

[0403] B-4: JER152 (manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent: 176-178, a compound corresponding to formula (B5))

[0404] B-5: JER1031S (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 180 to 220, a compound corresponding to formula (B6))

[0405] B-6: JER1032H60 (manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent: 163-175, compound corresponding to formula (B1))

[0406] B-7: JER157S65 (manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent: 210, a compound corresponding to formula (B7))

[0407] B-8: YX8000 (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 205, a compound corresponding to formula (B4))

[0408] B-9: YH-434 (manufactured by Nippon Steel Chemical & Materials Co., Ltd., epoxy equivalent: 115-119, a compound corresponding to formula (B2))

[0409] B-10: JER806 (manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent: 160-170, a compound corresponding to formula (B8))

[0410] (Photoacid generator (C))

[0411] C-1: OS-17 described in International Publication No. 2016 / 124493

[0412] [Chemistry 31]

[0413]

[0414] C-2: OS-25 described in International Publication No. 2016 / 124493

[0415] [Chemistry 32]

[0416]

[0417] C-3: Irgacure PAG121 (manufactured by BASF)

[0418] C-4: NIT (N-hydroxynaphthalene dicarboxylic acid imide trifluoromethanesulfonate)

[0419] C-5: B-9 of Japanese Patent No. 5914663

[0420] [Chemistry 33]

[0421]

[0422] Ts:tosyl group

[0423] C-6: A-1 of Japanese Patent No. 5650078

[0424] [Chemistry 34]

[0425]

[0426] (Other additives)

[0427] X-1: Cardo compound (WR-301, manufactured by ADEKA Co., Ltd.)

[0428] X-2: Cardo compound (Ogsol CR1030, manufactured by Osaka Gas Chemical Co., Ltd.)

[0429] X-3: Cardo compound (V-259ME, manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.)

[0430] X-4: Cardo compound (Ogsol SC001, manufactured by Osaka Gas Chemical Co., Ltd.)

[0431] X-5: Succinic acid-modified pentaerythritol triacrylate (Aronix TO-756, manufactured by Toa Gosei Co., Ltd.)

[0432] [Example 1]

[0433] In the polymer solution containing the polymer (A-1) obtained in the above-mentioned Synthesis Example 1, 5 parts of the epoxy group-containing compound (B-1), 1 part of the photoacid generator (C-1), 10 parts of trimethyl orthoformate, and 5 parts of trimethyl orthobenzoate were mixed in an amount corresponding to 100 parts (solid content) of the polymer (A-1), and diethylene glycol ethyl methyl ether and propylene glycol monomethyl ether were added at a mass ratio of 1:1 so that the final solid content concentration became 20% by mass. Then, the mixture was filtered using a membrane filter having a pore size of 0.2 μm to prepare a radiation-sensitive composition.

[0434] [Example 2 to Example 37, Comparative Example 1 to Comparative Example 4]

[0435] Radiation sensitive compositions of Examples 2 to 37 and Comparative Examples 1 to 4 were prepared in the same manner as in Example 1 except that the components were of the types and blending amounts (parts by mass) shown in Table 2. In Table 2, "-" indicates that the corresponding component was not used.

[0436] [Example 38]

[0437] A composition was prepared and evaluated in the same manner as in Example 1 except that the orthoester compound was removed therefrom.

[0438] [Table 2]

[0439]

[0440] <Evaluation>

[0441] The following items were evaluated by the methods described below using the radiation-sensitive compositions of Examples 1 to 38 and Comparative Examples 1 to 4. The evaluation results are shown in Table 3.

[0442] [Radiation sensitivity]

[0443] Using a spinner, the radiation-sensitive composition was applied to a silicon substrate treated with HMDS at 60°C for 60 seconds, and then pre-baked on a hot plate at 90°C for 2 minutes to form a coating with an average film thickness of 3.0 μm. A pattern mask having a line and space pattern with a width of 10 μm was used, and a mercury lamp was used to irradiate the coating with a specified amount of ultraviolet rays. Subsequently, a 2.38% by mass aqueous solution of tetramethylammonium hydroxide was used as a developer, and after a development treatment was performed at 25°C for 60 seconds, ultrapure water was used for 1 minute of running water washing. At this time, the minimum exposure amount that can form a line and space pattern with a width of 10 μm was measured. The minimum amount was measured to be 50 J / m 2 The following situations are judged as "A", which will be greater than 50J / m 2 And 100J / m 2The following situations are judged as "B", which is greater than 100J / m 2 The situation is judged as "C".

[0444] [Evaluation of substrate adhesion (development adhesion)]

[0445] The radiation-sensitive composition was applied to a silicon substrate that had not been treated with HMDS using a spinner, and then pre-baked on a hot plate at 90°C for 2 minutes to form a coating film with an average film thickness of 3.0 μm. The coating film was irradiated with a mercury lamp at an exposure dose of 400 J / m at 365 nm through a pattern mask having a line and space pattern with a width of 1 μm to 50 μm. 2 of ultraviolet rays. Subsequently, a 2.38% by mass aqueous solution of tetramethylammonium hydroxide was used as a developer, and after a development treatment was performed at 25°C for 60 seconds, ultrapure water was used for 1 minute of running water washing. At this time, the minimum width of the line and space pattern that has not been peeled off from the substrate is measured. At this time, the minimum width obtained by measuring the minimum width of the line and space pattern that has not been peeled off from the substrate is judged as "AA" when it is less than 2μm, and the case greater than 2μm and less than 5μm is judged as "A", and the case greater than 5μm and less than 10μm is judged as "B", and the case greater than 10μm is judged as "C". In the case of AA, A or B, it can be evaluated that the substrate adhesion is good, and in the case of C, it can be evaluated that the substrate adhesion is poor.

[0446] [Outgassing characteristics]

[0447] After applying the radiation-sensitive composition on a silicon substrate using a spinner, it was pre-baked on a hot plate at 90°C for 2 minutes to form a coating with an average film thickness of 3.0 μm. Furthermore, an oven heated to 230°C was used to calcine for 30 minutes to form a cured film. Subsequently, the silicon substrate was cut into a size of 1 cm×5 cm, and a P&T-GCMS device including JTD-505 manufactured by Japan Analytical Industry Co., Ltd. and GC-QP-2010 manufactured by Shimadzu Corporation Co., Ltd. was used to bake at 230°C for 15 minutes to obtain a chromatogram. The outgassing amount was calculated by the following formula (I) using the peak area of ​​C18 of the chromatogram measured using the cured film and the peak area of ​​the chromatogram of the standard sample C18 measured using the device. In addition, the so-called "introduction amount of the standard sample" is the introduction amount of the standard sample introduced into the device when the chromatogram of the standard sample C18 is obtained.

[0448] Outgassing amount (μg) = (peak area of ​​chromatogram of cured film / peak area of ​​standard sample) × amount of standard sample introduced (μg)... (I)

[0449] At this time, the case where the outgassing amount was 5 μg or less was determined as "A", the case where it was greater than 5 μg and less than 10 μg was determined as "B", and the case where it was greater than 10 μg was determined as "C".

[0450] [Table 3]

[0451] Radiation sensitivity substrate adhesion Escape Example 1 A A A Example 2 A A A Example 3 A A A Example 4 A A A Example 5 A A A Example 6 A AA A Example 7 A A A Example 8 A A A Example 9 A A A Example 10 A B B Embodiment 11 B AA A Example 12 C AA A Example 13 A AA A Embodiment 14 A AA B Embodiment 15 A AA A Example 16 A AA A Embodiment 17 A AA A Embodiment 18 A AA A Embodiment 19 A AA A Embodiment 20 A AA A Embodiment 21 A AA B Embodiment 22 A AA A Embodiment 23 A AA A Embodiment 24 A AA A Embodiment 25 A AA A Embodiment 26 C B A Embodiment 27 C B A Embodiment 28 B AA A Embodiment 29 B AA A Embodiment 30 B AA A Embodiment 31 B AA A Embodiment 32 B AA A Embodiment 33 A AA A Embodiment 34 A AA A Embodiment 35 A AA A Embodiment 36 B AA A Embodiment 37 A A A Embodiment 38 A B A Comparative Example 1 A C C Comparative Example 2 A C B Comparative Example 3 - - A Comparative Example 4 - - A

[0452] In Table 3, “-” indicates that the sensitivity evaluation was not analyzed and therefore could not be evaluated.

[0453] As shown in Table 3, the radiation sensitivity, substrate adhesion, and outgassing evaluations of practical properties of each radiation-sensitive composition of Examples 1 to 38 were good, and a balance of various properties was achieved. In contrast, substrate adhesion and outgassing were poor in Comparative Examples 1 and 2. No analysis was performed by exposure in Comparative Examples 3 and 4.

Claims

1. A radiation-sensitive composition comprising: a silicon-containing polymer (A) which is at least one selected from the group consisting of a polymer containing a structural unit (I) having a group represented by the following formula (1) and a siloxane polymer; an epoxy group-containing compound (B) having one or more ring structures and two or more epoxy groups; and Photoacid generator (C), The epoxy-containing compound (B) does not include the silicon-containing polymer (A), In formula (1), R 1 , R 2 and R 3 are independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group; wherein, R 1 , R 2 and R 3 At least one of them is an alkoxy group having 1 to 6 carbon atoms; "*" represents a bond.

2. The radiation-sensitive composition according to claim 1, wherein the epoxy-containing compound (B) contains at least one compound selected from the group consisting of novolac epoxy compounds, bisphenol A epoxy compounds, bisphenol F epoxy compounds, tetraglycidylamine epoxy compounds, tetraphenylethane epoxy compounds, hydrogenated bisphenol A epoxy compounds, and trisphenol epoxy compounds.

3. The radiation-sensitive composition according to claim 1, wherein the epoxy-containing compound (B) contains at least one compound selected from the group consisting of compounds represented by the following formula (B1) to formula (B8), In formula (B3), i is an integer from 0 to 300, In formula (B4), j is an integer from 0 to 300, In formula (B5), R 11 independently represent a hydrogen atom, a halogen atom or a methyl group, k is an integer from 0 to 100, In formula (B7), m is an integer from 0 to 50, In formula (B8), p is an integer from 0 to 300. 4 . The radiation sensitive composition according to claim 1 , wherein a content of the epoxy group-containing compound (B) is 1 part by mass or more and 50 parts by mass or less based on 100 parts by mass of the silicon-containing polymer (A).

5. A method for manufacturing a hardened film, comprising: A step of forming a coating film using the radiation-sensitive composition according to any one of claims 1 to 4; a step of irradiating at least a portion of the coating film with radiation; a step of developing the coating film irradiated with radiation; and A step of heating the developed coating film. 6 . A cured film formed using the radiation sensitive composition according to claim 1 . 7 . A semiconductor element comprising the hardened film according to claim 6 . A display element comprising the hardened film according to claim 6 .