Injection molding method of metal soft magnetic powder core

Through injection molding, the aerosolized iron-silicon alloy powder is treated with surfactant and resin solution, which solves the problems of high energy consumption and insufficient shape complexity of the molding equipment, and realizes a high density and high resistivity metal soft magnetic powder core Molding reduces molding pressure and eddy current losses, and improves product quality and production efficiency.

CN119069249AActive Publication Date: 2024-12-03HEFEI UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411520411.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-12-03
Estimated Expiration
2044-10-29

AI Technical Summary

Technical Problem

The existing molding method has problems such as high energy consumption of equipment, severe mold wear, excessive pressure, resulting in damage to the insulating coating, contact of magnetic powder particles, reduced resistivity and increased eddy current loss in the production of metal soft magnetic powder cores, and it is difficult to meet the problem. Forming of products with complex shapes.

Method used

By injection molding, the aerosolized iron-silicon alloy powder of -80 is sieved into different particle sizes, grading and coating are performed, and surfactant and resin solution are added, forming is achieved through ultrasonic vibration and air drying, reducing pores and difficult to demold.

Benefits of technology

It significantly improves molding density, fluidity and resistivity, reduces molding pressure and eddy current losses, reduces cracks and deformation defects, improves product quality and production efficiency, and can meet the molding needs of complex shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069249A_ABST
    Figure CN119069249A_ABST
Patent Text Reader

Abstract

The invention discloses an injection molding method of a metal soft magnetic powder core, and belongs to the technical field of material science. The method comprises the following specific operation steps: (1) screening-80-mesh gas-atomized iron-silicon alloy powder into three kinds of gas-atomized iron-silicon alloy powder with different particle sizes, and uniformly mixing the three kinds of powder with different particle sizes to obtain graded powder; (2) adding ethanol, tetraethyl orthosilicate, deionized water and ammonia water into the graded powder, and uniformly stirring under a water bath condition to obtain insulating powder; (3) adding a surfactant and water into the insulating powder, and uniformly stirring to obtain powder slurry; (4) uniformly mixing the powder slurry with a resin solution to obtain a forming material; and (5) the formed material is poured into a cylindrical silica gel mold, ultrasonic vibration treatment, drying and demolding are conducted, and the metal soft magnetic powder core is obtained. According to the surfactant disclosed by the invention, the use amount of water is reduced by 50%; through the synergistic effect of the polyester substances and the polyether substances, the comprehensive performance of the metal soft magnetic powder core is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material science, and particularly relates to a method for improving the injection molding performance of a metal soft magnetic powder core by utilizing a surfactant. Background Art

[0002] Metal soft magnetic powder cores are widely used in electronic components. At present, the mainstream molding method of metal soft magnetic powder cores is compression molding, and its operation steps include first insulating and coating the metal soft magnetic powder, adding a binder, and then loading the pretreated powder into a mold, and applying pressure through a press to press the powder into a relatively simple shape blank; then, the pressed blank needs to be heat treated before the product can be obtained. However, the compression molding method has obvious defects. For example, the pressing tonnage of the press is large, the energy consumption of the equipment is large, and the mold wear is serious; when the pressure of the press is too high, the insulating coating will be destroyed, and the insulating coating between the magnetic powder particles will fall off, which will cause the magnetic powder particles to directly contact each other, resulting in a decrease in the resistivity of the soft magnetic composite material and an increase in eddy current loss; compression molding can only meet the molding of products with a relatively simple appearance and a single shape. Summary of the invention

[0003] In order to effectively reduce defects such as cracks and deformation of metal soft magnetic powder core products and realize the production and demoulding of metal soft magnetic powder cores with different shapes, the present invention provides an injection molding method for metal soft magnetic powder cores.

[0004] A method for injection molding of a metal soft magnetic powder core, the operating steps are as follows: (1) Screening -80 mesh aerosolized iron-silicon alloy powder into three types of aerosolized iron-silicon alloy powders with different particle sizes, namely, primary powder, secondary powder and dust removal powder; mixing the primary powder, secondary powder and dust removal powder evenly in a mass ratio of 6:1:3 to obtain graded powder; (2) Add 100 ml of ethanol, 16 ml of tetraethyl orthosilicate, 16 ml of deionized water and 4 ml of ammonia water to 10 g of graded powder and stir evenly in a water bath to obtain silicon dioxide (SiO 2 ) Insulation powder coated; (3) Adding a surfactant in an amount of 0.6 to 0.8% by weight of the insulating powder and adding water in an amount of 9 to 10% by weight of the insulating powder to the insulating powder, stirring evenly to obtain a powder slurry; (4) mixing the powder slurry with the resin solution at a mass ratio of 20:1 to 1.5, stirring evenly to obtain a molding material with adhesiveness; (5) pouring the molding material into a cylindrical rubber mold, vibrating it in an ultrasonic cleaning machine for a certain period of time to reduce pores, and then drying it in the air, demolding it, and obtaining a metal soft magnetic powder core; The density of the metal soft magnetic powder core is 6.76-6.79 g / cm 3 , resistivity is 0.381~0.493kΩ·m.

[0005] The further technical solution is as follows: In step (1), the primary powder is a powder of -800 to +200 meshes, the secondary powder is a powder of -400 to +600 meshes, and the dust removal powder is a powder of -1000 to +5000 meshes.

[0006] In step (2), the water bath temperature is 50° C. and the stirring time is 4 h.

[0007] In step (3), the surfactant is prepared by uniformly mixing a polyester material and a polyether material in a mass ratio of 1:1.

[0008] The polyester material is polyethylene terephthalate (PET), and the polyether material is polyethylene glycol (PEG).

[0009] In step (4), the resin solution is prepared by uniformly mixing bisphenol A liquid epoxy resin (e44 epoxy resin), polyamide resin curing agent (593 curing agent) and 99.7% ethanol solution in a mass ratio of 3:1:4.

[0010] In step (5), the ultrasonic cleaning temperature is room temperature, the ultrasonic frequency is 75 KHz, and the ultrasonic time is 10 min.

[0011] The beneficial technical effects of the present invention are embodied in the following aspects: 1. The powder slurry used for injection molding in the present invention is added with a surfactant, which not only reduces the amount of water used by 50%, but also significantly improves the fluidity, molding density, molding pressure and other key properties of the powder slurry during the molding process. Polyethylene terephthalate (PET), as a polyester material, mainly improves the molding performance of the metal soft magnetic powder core by enhancing the mechanical strength of the material, improving the adhesion, improving the heat resistance and insulation, ensuring the stability of the material structure and reducing the eddy current loss. Polyethylene glycol (PEG), as a polyether material, has good fluidity and lubricity, can effectively reduce the friction between powder particles, enhance the dispersibility and filling of the slurry, reduce molding defects and cracks, and reduce molding pressure, improve molding efficiency and product quality. The synergistic effect of these two substances significantly improves the comprehensive performance of the powder core molding process. Therefore, the powder slurry used for injection molding in the present invention has the following advantages: (1) Higher fluidity: Improves the fluidity of the molding material, so that the powder can better fill the mold. (2) Improved molding density: Improved molding density is conducive to improving the magnetic properties of the powder core. (3) Reduce defects: defects such as cracks and deformation are significantly reduced, and the qualified rate of products is improved. (4) Reduce molding pressure: The pressure required for molding is reduced, saving energy. The density and resistivity of the injection molding samples were compared with those of the ordinary compression molding process samples. The data showed that the density of the metal soft magnetic powder core prepared by the method of the present invention was 6.76-6.79 g / cm³ and the resistivity was 0.381-0.493 kΩ·m. Compared with the samples prepared by compression molding, the density reached 98.9%-99.4%, while the resistivity was equivalent to 50%-64.7% of the compression molding samples. This shows that the method of the present invention can achieve the processing of high-density and high-resistivity metal soft magnetic powder core products while meeting the needs, and the efficiency is improved, and the equipment is simple and the cost is low.

[0012] The present invention adopts an injection molding method using a silicone mold for rapid molding, protects the insulating layer, has a high production speed, can meet complex geometric shapes, is convenient for demoulding, and can also select different thermoplastic and thermosetting plastics for injection molding according to specific requirements of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a graph showing the variation of magnetic permeability of three different metal soft magnetic powder cores with frequency.

[0014] Figure 2 These are the loss diagrams for three different metal soft magnetic powder cores. DETAILED DESCRIPTION

[0015] The present invention will be further described below by way of embodiments in conjunction with the accompanying drawings. Example

[0016] The operation steps of injection molding of a metal soft magnetic powder core are as follows: (1) The -80 mesh aerosolized iron-silicon alloy powder was sieved into three types of aerosolized iron-silicon alloy powders with different particle sizes, namely, a primary powder of -800 to +200 mesh, a secondary powder of -400 to +600 mesh, and a dust removal powder of -1000 to +5000 mesh; the primary powder, the secondary powder, and the dust removal powder were uniformly mixed in a mass ratio of 6:1:3 to obtain a graded powder.

[0017] (2) Add 1000 ml of ethanol, 160 ml of tetraethyl orthosilicate, 160 ml of deionized water and 40 ml of ammonia water to 100 g of graded powder and stir in a 50°C water bath for 4 hours to obtain silicon dioxide (SiO 2 ) coated with insulating powder.

[0018] (3) Add a surfactant in an amount of 0.6% by weight of the insulating powder and water in an amount of 10% by weight of the insulating powder to the insulating powder, and stir evenly to obtain a powder slurry.

[0019] The surfactant is prepared by uniformly mixing polyethylene terephthalate (PET) and polyethylene glycol (PEG) in a mass ratio of 1:1.

[0020] (4) The powder slurry is mixed with the resin solution in a mass ratio of 20:1, and stirred evenly to obtain a molding material with adhesiveness.

[0021] Bisphenol A liquid epoxy resin (e44 epoxy resin), polyamide resin curing agent (593 curing agent) and ethanol are uniformly mixed in a mass ratio of 3:1:4 to prepare a resin solution.

[0022] (5) Pour the above powder molding material into a cylindrical silicone mold, and ultrasonically clean it in an ultrasonic cleaning machine at a frequency of 75KHz for 10 minutes at room temperature to reduce pores, then dry it in the air, and demold it to obtain a metal soft magnetic powder core product. The product was tested for density and resistivity, and the density of the product was 6.76 g / cm 3 , resistivity is 0.381 kΩ*m. Example

[0023] The operation steps of injection molding of a metal soft magnetic powder core are as follows: (1) The -80 mesh aerosolized iron-silicon alloy powder was sieved into three types of aerosolized iron-silicon alloy powders with different particle sizes, namely, a primary powder of -800 to +200 mesh, a secondary powder of -400 to +600 mesh, and a dust removal powder of -1000 to +5000 mesh; the primary powder, the secondary powder, and the dust removal powder were uniformly mixed in a mass ratio of 6:1:3 to obtain a graded powder.

[0024] (2) Add 1000 ml of ethanol, 160 ml of tetraethyl orthosilicate, 160 ml of deionized water and 40 ml of ammonia water to 100 g of graded powder and stir in a 50°C water bath for 4 hours to obtain silicon dioxide (SiO 2 ) coated with insulating powder.

[0025] (3) Adding a surfactant in an amount of 0.8% by weight of the insulating powder and adding water in an amount of 9% by weight of the insulating powder to the insulating powder, stirring evenly to obtain a powder slurry; (4) The powder slurry is mixed with the resin solution in a mass ratio of 20:1.5, and stirred evenly to obtain a molding material with adhesiveness.

[0026] Bisphenol A liquid epoxy resin (e44 epoxy resin), polyamide resin curing agent (593 curing agent) and ethanol are uniformly mixed in a mass ratio of 3:1:4 to prepare a resin solution.

[0027] (5) Pour the above powder molding material into a cylindrical silicone mold, vibrate it in an ultrasonic cleaning machine with an ultrasonic frequency of 75KHz for 10 minutes at room temperature to reduce pores, and then dry it in the air and demold it to obtain a metal soft magnetic powder core product. The product was tested for density and resistivity, and the density of the product was 6.79 g / cm 3 , resistivity is 0.493 kΩ*m.

[0028] See also Figure 1 , wherein A is a conventional compression-molded metal soft magnetic powder core sample, B is a metal soft magnetic powder core sample prepared in Example 1, and C is a metal soft magnetic powder core sample prepared in Example 2.

[0029] Depend on Figure 1 It can be seen that the magnetic permeability of the three metal soft magnetic powder cores has good stability in the frequency range of 100-1000KHz, and does not change much with the increase of frequency. The magnetic permeability of the metal soft magnetic powder core A sample molded by conventional process is the highest, between 60.06-60.60; the magnetic permeability of the metal soft magnetic powder core B sample prepared in Example 1 is the lowest, between 56-56.19. Compared with the metal soft magnetic powder core C sample prepared in Example 2, the density of the metal soft magnetic powder core B sample of the present invention is the lowest due to the small amount of surface additives, large amount of water added, and low injection molding pressure of the metal soft magnetic powder core B sample of the present invention. Figure 1 The magnetic permeability of the metal soft magnetic powder core sample prepared in Example 2 in C is between 56.72 and 57.11, and the magnetic permeability of the three metal soft magnetic powder core samples is consistent with the change trend of density.

[0030] See also Figure 2, wherein A is a conventional compression-molded metal soft magnetic powder core sample, B is a metal soft magnetic powder core sample prepared in Example 1, and C is a metal soft magnetic powder core sample prepared in Example 2.

[0031] Depend on Figure 2 It can be seen that the losses of the three metal soft magnetic powder cores increase with the increase of frequency in the frequency range of 1-3MHz, because the hysteresis loss and eddy current loss, which are the main components of the metal soft magnetic powder core loss, increase with the increase of frequency. Among them, the loss increase rate of the conventional molded metal soft magnetic powder core sample A is the slowest, the loss increase rate of the metal soft magnetic powder core sample B prepared by the present invention is the fastest, and the loss increase rate of the metal soft magnetic powder core sample C prepared in Example 2 is between the two.

[0032] It will be easily understood by those skilled in the art that the above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for injection molding of a metal soft magnetic powder core, characterized in that: The steps are as follows: (1) Screening -80 mesh aerosolized iron-silicon alloy powder into three types of aerosolized iron-silicon alloy powders with different particle sizes, namely, primary powder, secondary powder and dust removal powder; mixing the primary powder, secondary powder and dust removal powder evenly in a mass ratio of 6:1:3 to obtain graded powder; (2) Add 100 ml of ethanol, 16 ml of tetraethyl orthosilicate, 16 ml of deionized water and 4 ml of ammonia water to 10 g of graded powder, stir evenly in a water bath to obtain insulating powder coated with silicon dioxide (SiO2); (3) Adding a surfactant in an amount of 0.6 to 0.8% by weight of the insulating powder and adding water in an amount of 9 to 10% by weight of the insulating powder to the insulating powder, stirring evenly to obtain a powder slurry; (4) mixing the powder slurry with the resin solution at a mass ratio of 20:1 to 1.5, stirring evenly to obtain a molding material with adhesiveness; (5) pouring the molding material into a cylindrical rubber mold, vibrating it in an ultrasonic cleaning machine for a certain period of time to reduce pores, and then drying it in the air, demolding it, and obtaining a metal soft magnetic powder core; The density of the metal soft magnetic powder core is 6.76-6.79 g / cm 3 , resistivity is 0.381~0.493kΩ·m.

2. A method for injection molding of a metal soft magnetic powder core as claimed in claim 1, characterized in that: In step (1), the primary powder is a powder of -800 to +200 meshes, the secondary powder is a powder of -400 to +600 meshes, and the dust removal powder is a powder of -1000 to +5000 meshes.

3. A method for injection molding of a metal soft magnetic powder core as claimed in claim 1, characterized in that: In step (2), the water bath temperature is 50° C. and the stirring time is 4 h.

4. A method for injection molding of a metal soft magnetic powder core as claimed in claim 1, characterized in that: In step (3), the surfactant is prepared by uniformly mixing a polyester material and a polyether material in a mass ratio of 1:

1.

5. A method for injection molding of a metal soft magnetic powder core as claimed in claim 4, characterized in that: The polyester material is polyethylene terephthalate (PET), and the polyether material is polyethylene glycol (PEG).

6. A method for injection molding of a metal soft magnetic powder core as claimed in claim 1, characterized in that: In step (4), the resin solution is prepared by uniformly mixing bisphenol A liquid epoxy resin (e44 epoxy resin), polyamide resin curing agent (593 curing agent) and 99.7% ethanol solution in a mass ratio of 3:1:

4.

7. A method for injection molding of a metal soft magnetic powder core as claimed in claim 1, characterized in that: In step (5), the ultrasonic cleaning temperature is room temperature, the ultrasonic frequency is 75 KHz, and the ultrasonic time is 10 min.

Citation Information

Patent Citations

  • Soft magnetic powder composition and manufacturing method for magnetic element

    CN106531391A

  • Preparation method of soft magnetic powder core formed through vibration

    CN114141525A

  • Insulating film, powder for magnetic core, powder magnetic core and method for forming them or method for producing them

    JP2008088505A

  • Electronic device and method for manufacturing the same

    KR1020240109912A

  • Inductor manufacturing method

    WO2016192094A1