Super capacitor and preparation method and application thereof
By mixing polyvinyl alcohol, conductive carbon material and surfactant to prepare a spinning solution and assemble it with polyvinyl alcohol electrolyte, the problem of low output energy density in the deformation state of flexible fibrous supercapacitor is solved, and the problem of low output energy density in the deformation state is realized. High bending resistance, suitable for new flexible and wearable electronic devices.
Patent Information
- Application Number
- CN202411349567.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing flexible fibrous supercapacitors have low output energy density in a deformed state and the electrode and electrolyte structure are inevitably displaced relative to each other, resulting in equipment failure, making it difficult to meet the power supply needs of new flexible and wearable electronic devices, and limiting their industrial development.
The spinning solution is prepared by mixing polyvinyl alcohol, conductive carbon materials, energy storage materials and surfactant. The fibrous electrode is prepared by wet spinning, and cross-linking reaction is carried out after assembly with the polyvinyl alcohol electrolyte to form an interfaceless structure. Improve the length specific capacity and bending resistance of supercapacitors.
The interface between the electrode and the electrolyte is effectively eliminated, and covalent bonds are formed by cross-linking, which improves the length specific capacity and bending resistance of the supercapacitor, meeting the power supply needs of flexible electronic equipment.
Smart Images

Figure CN119069267A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of energy storage technology, and in particular to a supercapacitor and a preparation method and application thereof. Background Art
[0002] The emergence of new flexible and wearable electronic devices has greatly promoted the rapid development of flexible supercapacitors that can power them. The development of high-performance flexible supercapacitors has become a hot issue. Flexible supercapacitors should have the ability to stably output electrical energy under various deformation states. Compared with traditional block supercapacitors and new thin-film flexible supercapacitors, fibrous supercapacitors have great application potential in wearable technology, smart textiles and other fields due to their unique advantages, such as small size, light weight and the ability to be co-woven with other functional fibers into smart fabrics through textile technology. At present, classic flexible fibrous supercapacitors usually include main components such as flexible fibrous electrode materials that can serve as both positive and negative electrodes and electrolytes. The fibrous electrode materials, electrolytes and fibrous electrode materials are assembled in a parallel configuration to form a fibrous supercapacitor. However, due to the obvious interface between the fibrous electrode|electrolyte|fibrous electrode, the parallel-configured fibrous supercapacitor has a low actual output energy density, and the fibrous electrode|electrolyte|fibrous electrode construction structure will inevitably undergo relative displacement and fibrous electrode delamination under repeated deformation, causing the fibrous supercapacitor to fail. This makes it difficult to meet the power supply needs of new flexible and wearable electronic devices, limiting the industrial development of fibrous supercapacitors.
[0003] Therefore, it is necessary to develop a method for preparing a supercapacitor so that the prepared supercapacitor has excellent mechanical properties and deformation resistance. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a method for preparing a supercapacitor, and the supercapacitor prepared by the method has excellent mechanical properties and deformation resistance.
[0005] The second aspect of the present invention also provides a supercapacitor.
[0006] The third aspect of the present invention also provides an application of a supercapacitor.
[0007] According to a first aspect of the present invention, an embodiment provides a method for preparing a supercapacitor, comprising the following steps:
[0008] S1, mixing polyvinyl alcohol, a conductive carbon material, an energy storage material, a surfactant, a first solvent and a second solvent to obtain a spinning solution, and preparing a fibrous electrode I and a fibrous electrode II by wet spinning the spinning solution;
[0009] S2, mixing polyvinyl alcohol and a second solvent to obtain a polyvinyl alcohol solution; applying the polyvinyl alcohol solution to the surfaces of the fiber electrode I and the fiber electrode II and assembling them, removing the second solvent by heat treatment, and obtaining an intermediate I;
[0010] S3, cross-linking the intermediate I with a cross-linking agent to obtain an intermediate II;
[0011] S4, immersing the intermediate II in an aqueous electrolyte, and then encapsulating to obtain a supercapacitor;
[0012] The fibrous electrode I is the same as the fibrous electrode II.
[0013] The preparation method according to the embodiment of the present invention has at least the following beneficial effects:
[0014] The present invention mixes polyvinyl alcohol, conductive carbon material, energy storage material and surfactant to obtain a spinning solution, and prepares fiber-shaped electrode I and fiber-shaped electrode II by wet spinning; then assembles them with polyvinyl alcohol electrolyte to form an intermediate, and further obtains a supercapacitor by cross-linking reaction, thereby improving the length specific capacity and bending resistance of the fiber-shaped supercapacitor.
[0015] This is because the present invention uses polyvinyl alcohol and a cross-linking agent for cross-linking, and the cross-linking occurs not only at the interface between the fibrous electrode and the electrolyte, but also inside the fibrous electrode and the electrolyte. Therefore, the interface between the electrode and the electrolyte is effectively eliminated, forming an electrode and electrolyte interface-free structure, so that the two layers are tightly combined through the covalent bonds formed by cross-linking, thereby improving the length-specific capacity of the supercapacitor and the bending resistance of the supercapacitor.
[0016] According to some embodiments of the present invention, in step S1, the mass ratio of the conductive carbon material, polyvinyl alcohol and energy storage material in the spinning solution is 1:(1-2):(0.07-0.2).
[0017] According to some embodiments of the present invention, in step S1, the mass ratio of the surfactant to the conductive carbon material in the spinning solution is 1:(20-1000).
[0018] According to some embodiments of the present invention, in step S1, the mass ratio of the total mass of the first solvent and the second solvent to the mass of the conductive carbon material is (20-40):1.
[0019] According to some embodiments of the present invention, in step S1, the first solvent is selected from at least one of dimethyl sulfoxide, glycerol, and N,N-dimethylformamide.
[0020] According to some embodiments of the present invention, in step S2, the second solvent is selected from water and / or phenol.
[0021] According to some embodiments of the present invention, in step S2, the temperature of the heat treatment is 45-85°C.
[0022] According to some embodiments of the present invention, in step S2, the heat treatment time is 1 to 20 minutes.
[0023] According to some embodiments of the present invention, in step S3, the temperature of the cross-linking reaction is 20-80°C.
[0024] According to some embodiments of the present invention, in step S3, the cross-linking reaction time is 1 to 48 hours.
[0025] According to some embodiments of the present invention, in step S1, the stirring speed is 400-1000 r / min.
[0026] According to some embodiments of the present invention, in step S1, the stirring time is 60 to 360 minutes.
[0027] According to some embodiments of the present invention, the cross-linking agent is a dialdehyde compound.
[0028] According to some embodiments of the present invention, the dialdehyde compound includes at least one of glutaraldehyde, glyoxal, and succinaldehyde.
[0029] According to some embodiments of the present invention, the conductive carbon material includes at least one of carbon nanotubes, graphene, porous carbon, carbon black or carbon fiber.
[0030] According to some embodiments of the present invention, the energy storage material is selected from conductive polymers or metal oxides.
[0031] According to some embodiments of the present invention, the surfactant includes at least one of sodium dodecylbenzene sulfonate, sodium octadecyl sulfate, sodium stearate, dodecyltrimethylammonium bromide or octoxynol.
[0032] According to some embodiments of the present invention, in step S4, the concentration of the aqueous electrolyte is 1-3M.
[0033] According to some embodiments of the present invention, the aqueous electrolyte includes sulfuric acid.
[0034] According to some embodiments of the present invention, in step S2, the concentration of the polyvinyl alcohol solution is 0.1-0.15 g / g.
[0035] According to some embodiments of the present invention, the amount of the cross-linking agent is 5 to 10 mL.
[0036] According to some embodiments of the present invention, the parameters of the wet spinning include: spinning needle size of 14-30G, spinning speed of 80-130ml / h, coagulation bath: 0°C anhydrous ethanol, fiber drying temperature: 50-70°C.
[0037] According to some embodiments of the present invention, the operation of preparing a fibrous electrode by wet spinning the spinning solution includes: controlling the injection speed of the spinning solution through a high-precision micro-injection pump to extrude it from a spinning needle into a 0°C anhydrous ethanol coagulation bath, and standing for 5-15 minutes to form it; then transferring the formed material to an anhydrous ethanol solution and placing it in a refrigerator, freezing it at -5°C to -15°C for 5-15 minutes to fix the shape; and finally placing it in a 50-70°C oven and drying it for 20-40 seconds to obtain a fibrous electrode.
[0038] According to a second aspect of the present invention, an embodiment provides a supercapacitor, which is prepared by the preparation method described in the first aspect of the present invention.
[0039] A third aspect of the present invention provides an application of the supercapacitor described above in a flexible electronic device or a wearable electronic device.
[0040] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0042] Figure 1 is a scanning electron microscope image of the fiber-shaped electrode of Example 2, wherein a is the surface morphology, b is the cross-sectional morphology, c is the surface high-resolution image, and d is the cross-sectional high-resolution image;
[0043] Figure 2 This is a scanning electron microscope image of the interface-free fibrous supercapacitor of Example 2, wherein a is the overall cross-sectional morphology, and b and c are enlarged images of the interface;
[0044] Figure 3 The ultra-depth three-dimensional microscope images of the fiber-shaped supercapacitor prepared in Example 2 and Comparative Example 1, wherein a and b are Comparative Example 1, and c and d are Example 2;
[0045] Figure 4 The stress-strain curves and elastic modulus, tensile strength and elongation at break of the cross-linked fiber electrodes prepared in Examples 1, 2 and 3 are compared;
[0046] Figure 5This is the stress-strain diagram of the interface-free fibrous supercapacitor prepared in Example 2;
[0047] Figure 6 The electrochemical performance comparison diagram of the fiber-shaped supercapacitors prepared in Examples 1, 2 and 3, wherein a is a comparison of the specific capacitance changes at different scan rates, b is a comparison of the specific capacitance at the same scan rate, and c is a comparison of the rate performance;
[0048] Figure 7 The electrochemical test diagram of Example 2, wherein a is a linear sweep voltammetry image, and b is a constant current charge-discharge test method image;
[0049] Figure 8 The cyclic stability diagram of the fiber-shaped supercapacitor prepared in Example 2, wherein a is the corresponding cyclic voltammetry curve after 1, 200, 400, 600, 800 and 1000 cycles of charge and discharge, and b is a dotted line diagram of the specific capacitance retention rate after 1, 200, 400, 600, 800 and 1000 cycles of charge and discharge;
[0050] Fig. 9 The cyclic stability diagram of the fiber-shaped supercapacitor prepared in Comparative Example 1, wherein a is the corresponding cyclic voltammetry curve after 1, 200, 400, 600, 800 and 1000 cycles of charge and discharge, and b is a dotted line diagram of the specific capacitance retention rate after 1, 200, 400, 600, 800 and 1000 cycles of charge and discharge;
[0051] Fig.10 This is a graph of the bending resistance of the fibrous supercapacitor prepared in Example 2, wherein a is the corresponding cyclic voltammetry curves for bending deformations of 1, 1000, 2000, 3000, 4000 and 5000 times, and b is a dotted line graph of the specific capacitance retention rate after bending deformations of 1, 1000, 2000, 3000, 4000 and 5000 times. DETAILED DESCRIPTION
[0052] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0053] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0054] Example 1
[0055] Embodiment 1 provides a supercapacitor, and its preparation method is as follows:
[0056] S1, 0.01g surfactant octoxynol, 14g dimethyl sulfoxide and 6g deionized water were mixed and mechanically stirred at 450r / min for 5min, 0.046g polyaniline and 0.3g multi-walled carbon nanotubes were added and mechanically stirred at 450r / min for 30min, ultrasonically dispersed for 30min, and then 0.3g multi-walled carbon nanotubes were added, mechanically stirred at 450r / min for 30min, and ultrasonically dispersed for 30min; 0.9g polyvinyl alcohol was added to the mixture, and mechanically stirred at 80°C for 30min. The mixture was stirred at 450 r / min for 6 hours; finally, the mixed solution was ultrasonically dispersed for 30 minutes, and mechanically stirred at 450 r / min for 220 minutes to obtain an electrode spinning solution; the injection speed of the spinning solution was controlled by a high-precision micro-injection pump, and it was extruded from a 20G needle into a 0°C anhydrous ethanol coagulation bath, and allowed to stand for 10 minutes to form; after the spinning was completed, the fibrous electrode material was transferred to an anhydrous ethanol solution and placed in a refrigerator at -10°C for 10 minutes to fix the shape; finally, it was placed in a 60°C oven and dried for 30 seconds to obtain fibrous electrodes I and fibrous electrodes II;
[0057] S2, applying a saturated polyvinyl alcohol solution (solvent is water, concentration is 0.11 g / g) on the fibrous electrode I and the fibrous electrode II respectively, attaching and fixing the fibrous electrode I and the fibrous electrode II, and drying them to obtain an intermediate I;
[0058] S3, placing intermediate I in a vacuum dryer filled with saturated glutaraldehyde (10 mL) and hydrochloric acid (10 mL) vapor, cross-linking glutaraldehyde with polyvinyl alcohol at 25° C. for 18 h under the catalysis of hydrochloric acid to obtain intermediate II;
[0059] S4. Immerse the intermediate II in a 1M sulfuric acid aqueous solution for 30 minutes and encapsulate to obtain a supercapacitor device.
[0060] Example 2
[0061] Embodiment 2 provides a supercapacitor, and its preparation method is as follows:
[0062] S1, 0.01g surfactant octoxynol, 14g dimethyl sulfoxide and 6g deionized water were mixed and mechanically stirred at 450r / min for 5min, 0.079g polyaniline and 0.3g multi-walled carbon nanotubes were added and mechanically stirred at 450r / min for 30min, ultrasonically dispersed for 30min, and then 0.3g multi-walled carbon nanotubes were added, mechanically stirred at 450r / min for 30min, and ultrasonically dispersed for 30min; 0.9g polyvinyl alcohol was added to the mixture, and mechanically stirred at 80°C for 30min. The mixture was stirred at 450 r / min for 6 hours; finally, the mixed solution was ultrasonically dispersed for 30 minutes, and mechanically stirred at 450 r / min for 220 minutes to obtain an electrode spinning solution; the injection speed of the spinning solution was controlled by a high-precision micro-injection pump, and it was extruded from a 20G needle into a 0°C anhydrous ethanol coagulation bath, and allowed to stand for 10 minutes to form; after spinning, the fibrous electrode material was transferred to an anhydrous ethanol solution and placed in a refrigerator at -10°C for 10 minutes to fix the shape; finally, it was placed in a 60°C oven and dried for 30 seconds to obtain fibrous electrode I and fibrous electrode II.
[0063] S2, applying a saturated polyvinyl alcohol solution (solvent is water, concentration is 0.11 g / g) on the fibrous electrode I and the fibrous electrode II respectively, attaching and fixing the fibrous electrode I and the fibrous electrode II, and drying them to obtain an intermediate I;
[0064] S3, placing intermediate I in a vacuum dryer filled with saturated glutaraldehyde (10 mL) and hydrochloric acid (10 mL) vapor, cross-linking glutaraldehyde with polyvinyl alcohol at 25° C. for 18 h under the catalysis of hydrochloric acid to obtain intermediate II;
[0065] S4. Immerse the intermediate II in a 1M sulfuric acid aqueous solution for 30 minutes and encapsulate to obtain a supercapacitor device.
[0066] Example 3
[0067] Embodiment 3 provides a supercapacitor, and its preparation method is as follows:
[0068] S1, 0.01g surfactant octoxynol, 14g dimethyl sulfoxide and 6g deionized water were mixed and mechanically stirred at 450r / min for 5min, 0.113g polyaniline and 0.3g multi-walled carbon nanotubes were added and mechanically stirred at 450r / min for 30min, ultrasonically dispersed for 30min, and then 0.3g multi-walled carbon nanotubes were added, mechanically stirred at 450r / min for 30min, and ultrasonically dispersed for 30min; 0.9g polyvinyl alcohol was added to the mixture, and mechanically stirred at 80°C for 30min. The mixture was stirred at 450 r / min for 6 hours; finally, the mixed solution was ultrasonically dispersed for 30 minutes, and mechanically stirred at 450 r / min for 220 minutes to obtain an electrode spinning solution; the injection speed of the spinning solution was controlled by a high-precision micro-injection pump, and it was extruded from a 20G needle into a 0°C anhydrous ethanol coagulation bath, and allowed to stand for 10 minutes to form; after the spinning was completed, the fibrous electrode material was transferred to an anhydrous ethanol solution and placed in a refrigerator at -10°C for 10 minutes to fix the shape; finally, it was placed in a 60°C oven and dried for 30 seconds to obtain fibrous electrodes I and fibrous electrodes II;
[0069] S2, applying a saturated polyvinyl alcohol solution (solvent is water, concentration is 0.11 g / g) on the fibrous electrode I and the fibrous electrode II respectively, attaching and fixing the fibrous electrode I and the fibrous electrode II, and drying them to obtain an intermediate I;
[0070] S3, placing intermediate I in a vacuum dryer filled with saturated glutaraldehyde (10 mL) and hydrochloric acid (10 mL) vapor, cross-linking glutaraldehyde with polyvinyl alcohol at 25° C. for 18 h under the catalysis of hydrochloric acid to obtain intermediate II;
[0071] S4. Immerse the intermediate II in a 1M sulfuric acid aqueous solution for 30 minutes and encapsulate to obtain a supercapacitor device.
[0072] Comparative Example 1
[0073] Comparative Example 1 provides a fiber-shaped supercapacitor, and the specific preparation method is as follows:
[0074] S1, 0.01g surfactant octoxynol, 14g dimethyl sulfoxide and 6g deionized water were mixed and mechanically stirred at 450r / min for 5min, 0.079g polyaniline and 0.3g multi-walled carbon nanotubes were added and mechanically stirred at 450r / min for 30min, ultrasonically dispersed for 30min, and then 0.3g multi-walled carbon nanotubes were added, mechanically stirred at 450r / min for 30min, and ultrasonically dispersed for 30min; 0.9g polyvinyl alcohol was added to the mixed solution, and mechanically stirred at 450r / min for 6h under heating conditions of 80°C; finally, the mixed solution was ultrasonically dispersed for 30min, and mechanically stirred at 450r / min for 220min to obtain an electrode spinning solution;
[0075] S2. The spinning solution is injected into a 0°C anhydrous ethanol coagulation bath by controlling the injection speed of the spinning solution through a high-precision micro-injection pump and allowed to stand for 10 minutes to form. After spinning, the fibrous electrode material is transferred to an anhydrous ethanol solution and placed in a refrigerator at -10°C for 10 minutes to fix the shape. Finally, the fibrous electrode material is placed in a 60°C oven and dried for 30 seconds to obtain a fibrous electrode material.
[0076] S3, placing the two fiber electrodes in a vacuum dryer filled with saturated glutaraldehyde and hydrochloric acid vapor, cross-linking glutaraldehyde and polyvinyl alcohol at 25° C. for 18 hours under the catalysis of hydrochloric acid, to obtain a cross-linked fiber electrode;
[0077] S4, taking the two cross-linked fiber electrodes, applying a saturated polyvinyl alcohol solution (concentration of 0.11 g / g) on the two cross-linked fiber electrodes respectively, attaching and fixing the two cross-linked fiber electrodes and drying them to assemble a fiber supercapacitor;
[0078] S5. Immerse the fiber-shaped supercapacitor in a 1M sulfuric acid aqueous solution and encapsulate to obtain a fiber-shaped supercapacitor device.
[0079] Performance Testing
[0080] The morphology of the fiber-shaped electrode prepared in Example 2 was observed using a cold field emission scanning electron microscope. Figure 1 (a is the surface of the fiber electrode, b is the cross section of the fiber electrode, c is the enlarged view of the surface of the fiber electrode, and d is the enlarged view of the cross section of the fiber electrode). It can be seen that the surface of the fiber electrode is flat, the thickness is uniform, the cross-sectional morphology is uniformly round, and the nanofibers are irregularly interwoven together, constructing a conductive framework with a nanoscale porous structure.
[0081] The cross-section of the supercapacitor prepared in Example 2 was observed by cold field emission scanning electron microscopy to observe the morphology of the fiber electrode|electrolyte|fiber electrode interface. Figure 2(a is the morphology of the fiber electrode | electrolyte interface, b and c are the enlarged views of the local interface). It can be seen that the fiber electrode | electrolyte | fiber electrode of the prepared supercapacitor has no obvious interface and has been cross-linked and fused into an integrated structure.
[0082] The supercapacitor prepared in Example 2 and the fiber-shaped supercapacitor prepared in Comparative Example 1 were observed using an ultra-depth 3D microscope to observe the morphology of the fiber-shaped electrode|electrolyte|fiber-shaped electrode interface. Figure 3 (a is comparative example 1, b is a partial enlarged view of comparative example 1, c is embodiment 2, and d is a partial enlarged view of embodiment 2). It can be seen that the fibrous electrode|electrolyte|fibrous electrode of the supercapacitor prepared in embodiment 2 has no obvious interface, and the interface is significantly optimized relative to that of comparative example 1.
[0083] According to GBT 528 standard, the tensile properties of the cross-linked fiber electrodes prepared in Example 1, Example 2 and Example 3 were tested. The stress-strain curves and the calculated elastic modulus, tensile strength and elongation at break are shown in Figure 2. Figure 4 As shown. It can be seen that when the amount of polyaniline is 3%, 5% and 7%, the Young's modulus of Example 1, Example 2 and Example 3 are 309.8, 325.5 and 457.7 MPa, respectively, the elongation at break is 23.5%, 24% and 9.5%, respectively, and the fracture strength is 72.7, 80.1 and 43.4 MPa, respectively. With the continuous change of the amount of polyaniline in the electrode, its Young's modulus is stably maintained in the range of 309.8 to 457.7 MPa, and the fracture strength continues to fluctuate between 43.4 and 80.1 MPa, while the elongation at break is maintained from a maximum of 24% to 9.5%. The increase in Young's modulus and the decrease in fracture strength and elongation at break are in line with the basic law that the increase in filler dosage causes the decrease in mechanical properties of composite materials.
[0084] According to GBT 528 standard, the tensile performance test of the supercapacitor prepared in Example 2 was carried out, and the stress-strain curve is as follows: Figure 5 As shown. It can be seen that when the amount of polyaniline in the fiber electrode is 5%, the Young's modulus of the fiber-shaped flexible supercapacitor is 9.4MPa, the elongation at break is 34.1%, and the breaking strength is 3.2MPa, showing good mechanical properties.
[0085] The electrochemical performance of the supercapacitors prepared in Example 1, Example 2 and Example 3 was tested using an electrochemical workstation. The results are as follows: Figure 6As shown. When the cyclic voltammetry scan rate is 40mV / s, the specific capacitances of Example 1, Example 2 and Example 3 are 0.6, 1.2 and 1.0mF / cm, respectively. As the amount of polyaniline in the fibrous electrode increases, the specific capacitance of the interface-free fibrous supercapacitor in Example 1, Example 2 and Example 3 increases, and the rate performance first increases and then decreases. The specific capacitance of Example 2 is 1.2mF / cm at a scan rate of 40mV / s, and the rate performance is still 51% at a scan rate of 100mV / s, with the best performance. This is attributed to: the amount of polyaniline in the fibrous electrode increases, and higher density electrochemically active substances can participate in the reaction at the same time. However, as the amount of polyaniline continues to increase, the porous network structure of the electrode is blocked, resulting in a slower ion transfer rate, thereby reducing the electrochemical performance of the fibrous interface-free flexible supercapacitor. It shows that the fibrous supercapacitor prepared by the present invention can exhibit excellent length-specific capacitance by optimizing the polyaniline content in the fibrous electrode.
[0086] In order to demonstrate the electrochemical performance of the supercapacitor prepared in Example 2, an electrochemical workstation was used to test the electrochemical performance of the supercapacitor prepared in Example 2. The results are as follows: Figure 7 It can be seen that when the scan rate is 5 mV / s, the length specific capacitance of the supercapacitor prepared in Example 2 can reach 2.8 mF / cm, indicating that the interface-free fibrous supercapacitor prepared in the present invention has excellent area specific capacitance.
[0087] The supercapacitor prepared in Example 2 was tested for charge-discharge cycle stability using an electrochemical workstation. Figure 8 As shown. Figure 8 (a is the corresponding cyclic voltammetry curve after 1, 200, 400, 600, 800 and 1000 cycles of charge and discharge, and b is a dotted line graph of the specific capacitance retention rate after 1, 200, 400, 600, 800 and 1000 cycles of charge and discharge) It can be seen that after 1000 cycles, the rectangular area enclosed by the curve measured by cyclic voltammetry has basically not changed, and the capacitance retention rate is still 99.6%, indicating that the supercapacitor prepared in Example 2 has excellent cycle stability.
[0088] The charge-discharge cycle stability test of the fiber-shaped supercapacitor prepared in Comparative Example 1 was carried out using an electrochemical workstation. The results are as follows: Fig. 9 As shown. Fig. 9(a is the corresponding cyclic voltammogram after 1, 200, 400, 600, 800 and 1000 cycles of charge and discharge, b is a dotted line graph of the specific capacitance retention rate after 1, 200, 400, 600, 800 and 1000 cycles of charge and discharge) It can be seen that the rectangular area enclosed by the curve measured by cyclic voltammetry changes after 1000 cycles, and the capacitance retention rate is only 65.5%, indicating that the fibrous supercapacitor prepared in Comparative Example 1 has general cycle stability.
[0089] The bending deformation resistance test of the supercapacitor in Example 2 was carried out using a flexible electronic tester and an electrochemical workstation. The results are as follows: Fig.10 As shown. Fig.10 (a is the cyclic voltammetry curve corresponding to bending deformation 1, 1000, 2000, 3000, 4000 and 5000 times, b is the point line graph of the specific capacitance retention rate after bending deformation 1, 1000, 2000, 3000, 4000 and 5000 times) It can be seen that the supercapacitor prepared in Example 2 can maintain 92.5% of its capacitance after repeated bending between 0° and 90° for 5000 times. The results show that the supercapacitor prepared in the present invention has excellent bending deformation resistance.
[0090] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A method for preparing a supercapacitor, characterized in that: The steps include: S1, mixing polyvinyl alcohol, a conductive carbon material, an energy storage material, a surfactant, a first solvent and a second solvent to obtain a spinning solution, and preparing a fibrous electrode I and a fibrous electrode II by wet spinning the spinning solution; S2, mixing polyvinyl alcohol and a second solvent with stirring to obtain a polyvinyl alcohol solution; The polyvinyl alcohol solution is applied to the surfaces of the fiber electrode I and the fiber electrode II and the fiber electrode is assembled, and the second solvent is removed by heat treatment to obtain an intermediate I; S3, cross-linking the intermediate I with a cross-linking agent to obtain an intermediate II; S4, immersing the intermediate II in an aqueous electrolyte, and then encapsulating to obtain a supercapacitor; The fibrous electrode I is the same as the fibrous electrode II.
2. The method for preparing a supercapacitor according to claim 1, characterized in that: In step S1, the mass ratio of the conductive carbon material, polyvinyl alcohol and energy storage material in the spinning solution is 1:(1-2):(0.07-0.2).
3. The method for preparing a supercapacitor according to claim 1, characterized in that: In step S1, the mass ratio of the surfactant to the conductive carbon material in the spinning solution is 1:(20-1000).
4. The method for preparing a supercapacitor according to claim 1, characterized in that: In step S1, the mass ratio of the total mass of the first solvent and the second solvent to the mass of the conductive carbon material is (20-40):
1.
5. The method for preparing a supercapacitor according to claim 1, characterized in that: In step S2, the temperature of the heat treatment is 45-85°C.
6. The method for preparing a supercapacitor according to claim 1, characterized in that: In step S3, the temperature of the cross-linking reaction is 20-80°C.
7. The method for preparing a supercapacitor according to claim 1, characterized in that: In step S1, the stirring speed is 400-1000 r / min.
8. The method for preparing a supercapacitor according to claim 1, characterized in that: The cross-linking agent is a dialdehyde compound; Preferably, the conductive carbon material comprises at least one of carbon nanotubes, graphene, porous carbon, carbon black or carbon fiber; Preferably, the energy storage material is selected from conductive polymers or metal oxides.
9. A supercapacitor, characterized in that: The supercapacitor is prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the supercapacitor according to claim 9 in flexible electronic devices or wearable electronic devices.