PL test method for solar thin film photovoltaic semiconductor film layer
By using the barrier protective layer in the PL test of solar thin film photovoltaic semiconductor film layer, the problem of traditional test equipment not being destructively separated and PL technology requires electrical contact, realizing complete non-destructive testing and high-accuracy characterization of the film layer, improving Research on product reliability and PL mechanism.
Patent Information
- Application Number
- CN202411165596.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The PID testing equipment of traditional solar photovoltaic modules cannot be destructively separated from glass and cell cells in high temperature environments, resulting in only a single parallel resistance characterization, and the inability to fully detect electrical performance and imaging characterization. Moreover, PL technology requires electrical contact, which limits its application.
In the PL test method of the solar thin film photovoltaic semiconductor film layer, a barrier protective layer is provided, including a polyethylene terephthalate material or a fluorine-containing polymer, and the protective layer is between the photovoltaic semiconductor film layer and the EVA layer. To ensure that the film layer is intact and lossless after testing, use a PL tester for testing, and obtain the parallel resistance and depth imaging characterization parameters.
It realizes complete non-destructive testing of thin-film photovoltaic semiconductor film layers, improves the accuracy of performance and parameter characterization, enhances product reliability, supports in-depth research on PL mechanisms and improves production processes.
Smart Images

Figure CN119069374A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thin-film photovoltaic nondestructive testing, and in particular to a PL testing method for a solar thin-film photovoltaic semiconductor film layer. Background Art
[0002] The world's social and economic development has an increasing demand for sufficient and cheap electricity, and solar energy, as a representative of renewable energy, can be used as a reliable source of electricity resources. How to improve the efficiency and reliability of solar photovoltaic modules is an important research direction in the industry. Attenuation caused by process defects and application environment and climate erosion, especially the loss of control of quality during the production process and stability of the finished product, will reduce the efficiency of the module and even shorten its service life.
[0003] There are automatic inspection (AOI) methods, visual inspection, thermal imaging, electroluminescence (EL) which can detect different defects under repeatable indoor conditions. Traditional battery-end PID reliability test equipment often requires the use of glass, EVA film (Ethylene-vinyl Acetate Copolymer, EVA, ethylene-vinyl acetate copolymer) and battery stacking structure. The high temperature in the test environment will melt the EVA, and the glass and battery will be bonded together and cannot be separated without loss. This results in only a single parallel resistance characterization after the PID test, and it is impossible to perform comprehensive electrical performance and imaging characterization; the main disadvantage of the most advanced EL technology is that it requires electrical contact, but photoluminescence (PL) imaging is used to determine battery characteristics and defects in the initial stage of production. The use of PL does not require contact circuits, and the luminescence intensity of different batteries is determined by the concentration of minority charge carriers generated by the excitation source. Therefore, correct defect non-destructive detection of PL plays an important role, especially on large-size areas. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a PL testing method for a solar thin-film photovoltaic semiconductor film layer.
[0005] The present invention provides a PL testing method for a solar thin-film photovoltaic semiconductor film layer, the PL testing method comprising the following steps:
[0006] Disposing a barrier protective layer between the surface of the thin-film photovoltaic semiconductor film layer sample to be tested and the EVA layer to obtain a first thin-film photovoltaic semiconductor film layer sample to be tested;
[0007] Transferring the first thin-film photovoltaic semiconductor film layer sample to be tested into a thin-film photovoltaic semiconductor film layer PL tester for PL testing;
[0008] Wherein, the barrier protection layer comprises polyethylene terephthalate material or fluorine-containing high molecular polymer.
[0009] Furthermore, the fluorine-containing high molecular polymer includes at least one of tetrafluoroethylene-ethylene copolymer, ethylene-tetrafluoroethylene copolymer (ETFE) and the like.
[0010] Furthermore, the first thin-film photovoltaic semiconductor film layer sample to be tested includes a photovoltaic semiconductor film layer, and the surface of the photovoltaic semiconductor film layer is sequentially provided with a barrier protective layer, an EVA layer and a photovoltaic glass sheet, and the vertical projection of the barrier protective layer on the plane where the photovoltaic semiconductor film layer is located covers the vertical projection of the EVA layer on the plane where the photovoltaic semiconductor film layer is located.
[0011] Furthermore, a barrier protective layer is provided between the surface of the thin-film photovoltaic semiconductor film layer sample to be tested and the EVA layer, and the step of obtaining the first thin-film photovoltaic semiconductor film layer sample to be tested includes the following process:
[0012] Select TCO conductive glass as the substrate;
[0013] Conductive layer coating is performed on the substrate to obtain a solar photovoltaic semiconductor film layer;
[0014] Disposing the barrier protection layer on the solar photovoltaic semiconductor film layer;
[0015] After the barrier protective layer is completed, a packaging EVA film and a photovoltaic glass sheet are added on the barrier protective layer in sequence.
[0016] Furthermore, the EVA layer includes a first side and a second side that are adjacent to each other, the length of the first side is a, and the length of the second side is b; the barrier protection layer includes a third side and a fourth side that are adjacent to each other, the length of the third side is c, and the length of the fourth side is d; wherein c>a, d>b.
[0017] Furthermore, the side length a of the first side satisfies: 50 mm ≤ a ≤ 300 mm, and the side length b of the second side satisfies: 50 mm ≤ b ≤ 300 mm.
[0018] Further, the step of transferring the first thin-film photovoltaic semiconductor film layer sample to be tested into a thin-film photovoltaic semiconductor film layer PL tester for PL testing includes the following process:
[0019] The first thin-film photovoltaic semiconductor film layer sample to be tested is placed between a voltage application plate and a heating platform, and then the equipment parameters of a thin-film photovoltaic semiconductor film layer PL tester are adjusted to perform the test. After the PL test is completed, the first thin-film photovoltaic semiconductor film layer sample to be tested is removed from the thin-film photovoltaic semiconductor film layer PL tester, and the performance parameters of the photovoltaic semiconductor film layer are extracted, and the performance of the photovoltaic semiconductor film layer is evaluated according to the performance parameters;
[0020] Among them, the equipment parameters of the thin-film photovoltaic semiconductor film layer PL tester include:
[0021] 1) Temperature range: 25-120℃;
[0022] 2) Heating and cooling rate: Test conventional component products from 20°C to 80°C and keep it constant for ≤20min; cool from 80°C to 20°C and keep it constant for ≤40min, no load, no light;
[0023] 3) Temperature fluctuation: no-load, constant state: ≤±0.5℃; full load of 6 pieces of samples, no light constant state: ≤±1℃; full load of 6 pieces of samples, light constant state: ≤±4℃;
[0024] 4) Temperature uniformity of the entire surface: no-load, constant state: ≤2°C; full load of 6 pieces of samples, no light constant state: ≤3°C; full load of 6 pieces of samples, light constant state: ≤8°C;
[0025] 5) Temperature deviation: no-load, constant state: ≤±2.0℃;
[0026] 6) Radiation intensity range: 300W / m 2 ~1200W / m 2 ;
[0027] 7) Spectral matching: CLASS B AM1.5G;
[0028] 8) Irradiation non-uniformity: CLASS B ≤ 5%;
[0029] 9) Radiation instability: CLASSA level ≤ 2%;
[0030] 10) Irradiation distance: 1500mm;
[0031] 11) Setting the illumination area of the light source excitation unit to ensure full illumination of the photovoltaic module with an area of 1-3 square meters;
[0032] 12) Set the angle of a single LED module in the camera unit to 30-60° and the intensity to +16.7W / ㎡ to 67.7W / ㎡; the distance between the camera and the LED to the photovoltaic module is 200 cm to 600 cm, and the integration time is 5-120 milliseconds.
[0033] Furthermore, the performance parameters include: electrical performance parameters, depth imaging characterization parameters and interface appearance component parameters.
[0034] Furthermore, after the first thin-film photovoltaic semiconductor film layer sample to be tested is moved into a thin-film photovoltaic semiconductor film layer PL tester for PL testing, the method further includes:
[0035] Acquire test data, wherein the test data includes parallel resistance test data; and evaluate the PL test effect of the photovoltaic semiconductor film layer according to the parallel resistance test data.
[0036] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0037] An embodiment of the present invention provides a PL testing method for a solar thin-film photovoltaic semiconductor film layer. The present invention sets a barrier protective layer between the surface of a thin-film photovoltaic semiconductor film layer sample to be tested in the PL test and the EVA layer, so that the film layer can be taken out intact after the PL test and further characterized, thereby realizing the possibility and repeatability of PL test characterization of the thin-film photovoltaic semiconductor film layer, improving the accuracy of performance and parameter characterization, improving the ultimate reliability of the product, and playing a positive role in in-depth research on the PL mechanism and improving the production process. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0040] Figure 1 A schematic structural diagram of a first thin-film photovoltaic semiconductor film layer sample to be tested in a PL testing method for a solar thin-film photovoltaic semiconductor film layer provided in an embodiment of the present invention.
[0041] Figure 2 A structural schematic diagram of the PL setting in a PL testing method for a solar thin-film photovoltaic semiconductor film layer and a light uniformity diagram provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0044] The present invention provides a PL testing method for a solar thin-film photovoltaic semiconductor film layer, the PL testing method comprising the following steps:
[0045] Disposing a barrier protective layer between the surface of the thin-film photovoltaic semiconductor film layer sample to be tested and the EVA layer to obtain a first thin-film photovoltaic semiconductor film layer sample to be tested;
[0046] Transferring the first thin-film photovoltaic semiconductor film layer sample to be tested into a thin-film photovoltaic semiconductor film layer PL tester for PL testing;
[0047] Wherein, the barrier protection layer comprises polyethylene terephthalate material or fluorine-containing high molecular polymer.
[0048] An embodiment of the present invention provides a PL testing method for a solar thin-film photovoltaic semiconductor film layer. The present invention sets a barrier protective layer between the surface of a thin-film photovoltaic semiconductor film layer sample to be tested in the PL test and the EVA layer, so that the film layer can be taken out intact after the PL test and further characterized, thereby realizing the possibility and repeatability of PL test characterization of the thin-film photovoltaic semiconductor film layer, improving the accuracy of performance and parameter characterization, improving the ultimate reliability of the product, and playing a positive role in in-depth research on the PL mechanism and improving the production process.
[0049] Thin-film photovoltaics (PV) using CdTe, Cu(In1-xGax)Se2 (CIGS), and perovskite absorbers have achieved efficiencies approaching those of crystalline silicon wafer-based PV. Thin-film PV has the potential to meet the rapidly growing demand for clean electricity with low production costs and ease of manufacturing. CdTe PV has achieved the greatest commercial success among thin-film technologies, with a market share of ~5% and a record power conversion efficiency of 22.1%. Further improvements in the efficiency of CdTe PV to 25% require a comprehensive understanding of the recombination mechanisms that limit efficiency. Bulk, interfacial, and surface recombination reduce minority carrier lifetimes, thereby reducing photovoltage, photocurrent, and fill factor. Advanced detection tools are developed to measure carrier dynamics and provide an understanding of recombination rates and mechanisms, while also serving as in-line detection tools to monitor products at all stages in real time, improve line yield, and accelerate the development of thin-film PV technology. Time-resolved photoluminescence (TRPL) spectroscopy has been the benchmark technology in the photovoltaic community to study photoexcited carrier dynamics. In TRPL measurements, a material is excited by short (typically nanosecond) laser pulses of light and the transient emission of photons is recorded via the radiative recombination of electron-electron-hole pairs.
[0050] In some specific embodiments, the fluorine-containing polymer includes at least one of tetrafluoroethylene-ethylene copolymer and ethylene-tetrafluoroethylene copolymer (ETFE).
[0051] In some specific embodiments, the thin-film photovoltaic semiconductor film layer PL tester may adopt existing testing equipment from equipment manufacturers such as Horiba, Renishaw, and Ocean Optics.
[0052] In some specific embodiments, Figure 1 As shown, the first thin-film photovoltaic semiconductor film layer sample to be tested includes a photovoltaic semiconductor film layer, and the surface of the photovoltaic semiconductor film layer is sequentially provided with a barrier protective layer, an EVA layer and a photovoltaic glass sheet, and the vertical projection of the barrier protective layer on the plane where the photovoltaic semiconductor film layer is located covers the vertical projection of the EVA layer on the plane where the photovoltaic semiconductor film layer is located.
[0053] In some specific embodiments, a barrier protective layer is provided between the surface of the thin film photovoltaic semiconductor film layer sample to be tested and the EVA layer, and the step of obtaining the first thin film photovoltaic semiconductor film layer sample to be tested includes the following process:
[0054] (1) selecting a TCO conductive glass (i.e., transparent conductive oxide coated glass, preferably but not limited to FTO glass-fluorine-doped tin oxide glass, which is a subdivided product of TCO glass and is a conductive glass made of fluorine-doped tin oxide as a base material) as a substrate;
[0055] (2) coating a conductive layer on the substrate to obtain a solar photovoltaic semiconductor film layer;
[0056] (3) providing a barrier protection layer on the solar photovoltaic semiconductor film layer;
[0057] (4) After the barrier protective layer is completed, the encapsulation EVA film and the photovoltaic glass sheet are added to the barrier protective layer in turn; Operation parameters: EVA film thickness: Generally determined according to the design requirements of the battery module, the common thickness is between 0.3mm and 0.7mm. Too thin thickness may affect the bonding strength, while too thick thickness may increase light loss and component weight; Lamination temperature and pressure: During the lamination process, the temperature and pressure must be precisely controlled to ensure that the EVA film is fully melted and bonded to each layer of material. The temperature is generally between 130℃ and 150℃, and the pressure is adjusted according to the laminator model and component size; Lamination time: Determined according to the melting characteristics of the EVA film and the performance of the equipment, generally ranging from a few minutes to more than ten minutes. Ensure that the EVA film is completely cured and bonded to each layer of material; Cleanliness: Before encapsulation, each layer of material must be strictly cleaned to remove impurities such as dust and oil. The cleaning solvent and cleaning method must be determined according to the material characteristics. At the same time, it is also crucial to maintain the cleanliness of the production environment.
[0058] It should be noted that the present invention is directed to a PL testing method for solar thin-film photovoltaic semiconductor film layers. For the operating parameters not specifically described in the preparation process of the thin-film photovoltaic semiconductor film layer samples to be tested, such as encapsulating EVA adhesive film and photovoltaic glass sheet, conventional methods in the art may be used, and the present invention document will not describe them one by one.
[0059] In some specific embodiments, the EVA layer includes a first side and a second side that are adjacent to each other, the length of the first side is a, and the length of the second side is b; the barrier protection layer includes a third side and a fourth side that are adjacent to each other, the length of the third side is c, and the length of the fourth side is d; wherein c>a, d>b.
[0060] In some specific embodiments, the side length a of the first side satisfies: 50 mm ≤ a ≤ 300 mm, and the side length b of the second side satisfies: 50 mm ≤ b ≤ 300 mm.
[0061] In some specific embodiments, the step of transferring the first thin-film photovoltaic semiconductor film layer sample to be tested into a thin-film photovoltaic semiconductor film layer PL tester for PL testing comprises the following process:
[0062] The first thin-film photovoltaic semiconductor film layer sample to be tested is placed between a voltage application plate and a heating platform, and then the equipment parameters of a thin-film photovoltaic semiconductor film layer PL tester are adjusted to perform the test. After the PL test is completed, the first thin-film photovoltaic semiconductor film layer sample to be tested is removed from the thin-film photovoltaic semiconductor film layer PL tester, and the performance parameters of the photovoltaic semiconductor film layer are extracted, and the performance of the photovoltaic semiconductor film layer is evaluated according to the performance parameters;
[0063] Among them, the equipment parameters of the thin-film photovoltaic semiconductor film layer PL tester include:
[0064] 1) Temperature range: 25-120℃;
[0065] 2) Heating and cooling rate: Test conventional component products from 20°C to 80°C and keep it constant for ≤20min; cool from 80°C to 20°C and keep it constant for ≤40min, no load, no light;
[0066] 3) Temperature fluctuation: no-load, constant state: ≤±0.5℃; full load of 6 pieces of samples, no light constant state: ≤±1℃; full load of 6 pieces of samples, light constant state: ≤±4℃;
[0067] 4) Temperature uniformity of the entire surface: no-load, constant state: ≤2°C; full load of 6 pieces of samples, no light constant state: ≤3°C; full load of 6 pieces of samples, light constant state: ≤8°C;
[0068] 5) Temperature deviation: no-load, constant state: ≤±2.0℃;
[0069] 6) Radiation intensity range: 300W / m 2 ~1200W / m 2 ;
[0070] 7) Spectral matching: CLASS B AM1.5G;
[0071] 8) Irradiation non-uniformity: CLASS B ≤ 5%;
[0072] 9) Radiation instability: CLASSA level ≤ 2%;
[0073] 10) Irradiation distance: 1500mm;
[0074] 11) Setting the illumination area of the light source excitation unit to ensure full illumination of the photovoltaic module with an area of 1-3 square meters;
[0075] 12) Set the angle of a single LED module in the camera unit to 30-60° and the intensity to +16.7W / ㎡ to 67.7W / ㎡; the distance between the camera and the LED to the photovoltaic module is 200 cm to 600 cm, and the integration time is 5-120 milliseconds.
[0076] A schematic diagram of the structure of a PL setting in a PL testing method for a solar thin-film photovoltaic semiconductor film layer provided by an embodiment of the present invention ( Figure 2 As shown in the upper middle) and the illumination uniformity diagram ( Figure 2 As shown in the lower middle, the horizontal axis represents the horizontal distance and the vertical axis represents the light intensity) Figure 2As shown, the PL tester setup consists of an excitation unit (light source) and a camera unit. The excitation unit allows full-area illumination of PV modules with an area of about 1-3 square meters. Multiple low-weight on-chip LED modules are used. High uniformity can be achieved by adjusting the angle and intensity of the individual LED modules; camera resolution greater than 2048x2048 pixels is sufficient.
[0077] In front of each LED module, a short-pass filter with a certain cutoff wavelength is used according to the characteristics of the semiconductor film layer to be measured. Through these two filters, the excitation light is suppressed and it cannot reach the detector of the camera. The distance between the camera and the LED to the photovoltaic module is 200 cm to 600 cm, the integration time is 5-120 milliseconds, and the aperture is adjusted according to the usage scenario.
[0078] The test parameters of the thin-film photovoltaic semiconductor film layer PL tester are set, and the thin-film photovoltaic semiconductor film layer PL tester is started to perform PL test on the solar cell; the test parameters include cracks, film surface contamination, welding or ribbon interconnection failures and chemical corrosion (snail footprints), PID, battery mismatch and short-circuited bypass diodes, etc.
[0079] Temperature deviation refers to the difference between the set temperature inside the device and the actual measured temperature. It is usually measured at a specific point or multiple points inside the device after the device is working stably, and then compared with the set temperature to obtain the deviation value. Temperature deviation reflects the accuracy of the device's temperature control system, that is, whether the device can reach and maintain the set temperature. Temperature uniformity refers to the temperature difference between different locations inside the device after the device is working stably. It is usually determined by measuring the temperature at multiple measuring points evenly distributed inside the device, and then calculating the maximum and minimum temperature differences between these measuring points. Temperature uniformity reflects the consistency of temperature everywhere inside the device, that is, whether the device can provide a relatively consistent temperature environment throughout the entire working space.
[0080] The camera unit is suitable for both EL and PL images. The indoor PL images shown in this publication were all recorded with a front-illuminated silicon charge-coupled device (CCD) camera GEFI20482048 from greateyes GmbH, Germany, with a resolution of 2048x2048 pixels. The outdoor PL images shown in this publication were all recorded with an InGaAs camera, either the Ninox640 or the Owl1280 from RaptorPhotonics Ltd., Northern Ireland. In addition, these InGaAs cameras allow movie recordings. A comparison of different cameras is discussed in. A short-pass filter KG5 with a cut-off wavelength of 800 nm from SCHOTT, Germany, is used in front of each LED module and a custom-made long-pass filter with a cut-off wavelength of 970 nm is used in front of the camera. By these two filters, the excitation light is suppressed and it cannot reach the detector of the camera.
[0081] For outdoor applications, the excitation and camera units are mounted on a prototype tilting cart. In initial field tests, we manually moved the cart in front of a row of panels and achieved a throughput of 37 PV panels per minute. For future implementations, a mobile power source is under development.
[0082] In some specific embodiments, the performance parameters include: electrical performance parameters, depth imaging characterization parameters and interface appearance composition parameters.
[0083] In some specific embodiments, after the first thin-film photovoltaic semiconductor film layer sample to be tested is moved into a thin-film photovoltaic semiconductor film layer PL tester for PL testing, the method further includes:
[0084] Acquire test data, wherein the test data includes parallel resistance test data; and evaluate the PL test effect of the photovoltaic semiconductor film layer according to the parallel resistance test data.
[0085] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0086] Example
[0087] This example provides a PL testing method for a solar thin-film photovoltaic semiconductor film layer, comprising the following steps:
[0088] Select TCO conductive glass as a substrate; perform film coating of a conductive layer on the substrate to obtain a solar photovoltaic semiconductor film layer; arrange the barrier protective layer on the solar photovoltaic semiconductor film layer; after completing the barrier protective layer, sequentially add an encapsulating EVA adhesive film and a photovoltaic glass sheet on the barrier protective layer to obtain a first thin-film photovoltaic semiconductor film layer sample to be tested; wherein the EVA layer comprises a first side and a second side arranged adjacently, the side length of the first side is a, and the side length of the second side is b; the barrier protective layer comprises a third side and a fourth side arranged adjacently, the side length of the third side is c, and the side length of the fourth side is d; wherein c>a, d>b; the side length a of the first side satisfies: 50mm≤a≤300mm, and the side length b of the second side satisfies 50mm≤b≤300mm;
[0089] The first thin-film photovoltaic semiconductor film layer sample to be tested is placed between a voltage application plate and a heating platform, and then the equipment parameters of a thin-film photovoltaic semiconductor film layer PL tester are adjusted to perform the test. After the PL test is completed, the first thin-film photovoltaic semiconductor film layer sample to be tested is removed from the thin-film photovoltaic semiconductor film layer PL tester, and the performance parameters of the photovoltaic semiconductor film layer are extracted, and the performance of the photovoltaic semiconductor film layer is evaluated according to the performance parameters;
[0090] Among them, the equipment parameters of the thin-film photovoltaic semiconductor film layer PL tester include:
[0091] 1) Temperature range: 25-120℃;
[0092] 2) Heating and cooling rate: Test conventional component products from 20°C to 80°C and keep it constant for ≤20min; cool from 80°C to 20°C and keep it constant for ≤40min, no load, no light;
[0093] 3) Temperature fluctuation: no-load, constant state: ≤±0.5℃; full load of 6 pieces of samples, no light constant state: ≤±1℃; full load of 6 pieces of samples, light constant state: ≤±4℃;
[0094] 4) Temperature uniformity of the entire surface: no-load, constant state: ≤2°C; full load of 6 pieces of samples, no light constant state: ≤3°C; full load of 6 pieces of samples, light constant state: ≤8°C;
[0095] 5) Temperature deviation: no-load, constant state: ≤±2.0℃;
[0096] 6) Radiation intensity range: 300W / m 2 ~1200W / m 2 ;
[0097] 7) Spectral matching: CLASS B AM1.5G;
[0098] 8) Irradiation non-uniformity: CLASS B ≤ 5%;
[0099] 9) Radiation instability: CLASSA level ≤ 2%;
[0100] 10) Irradiation distance: 1500mm;
[0101] 11) Setting the illumination area of the light source excitation unit to ensure full illumination of the photovoltaic module with an area of 1-3 square meters;
[0102] 12) Setting the angle of a single LED module in the camera unit to 30-60° and the intensity to +16.7W / ㎡ to 67.7W / ㎡; the distance between the camera and the LED to the photovoltaic module to 200 cm to 600 cm, and the integration time to 5-120 milliseconds;
[0103] After the first thin-film photovoltaic semiconductor film layer sample to be tested is moved into the thin-film photovoltaic semiconductor film layer PL tester for PL testing, the method further includes: acquiring test data, the test data including parallel resistance test data; evaluating the PL test effect of the photovoltaic semiconductor film layer according to the parallel resistance test data;
[0104] The principle of the above test process is as follows: Excitation stage: Use a laser of a specific wavelength as an excitation light source to illuminate the solar cell, causing electrons to jump from the valence band to the conduction band; Light emission stage: The excited electrons release photons when they recombine to the valence band, which is photoluminescence; Photon detection: Use a highly sensitive and high-resolution camera to sense and image these released photons; Image analysis: The light intensity after imaging is proportional to the non-equilibrium minority carrier concentration at the corresponding position. The minority carrier concentration in the defective area is reduced, thereby weakening the fluorescence effect, which appears as a dark area on the image; Data processing: Use computer software to analyze the collected image data to evaluate important parameters such as the carrier properties, recombination rate, and defect level of the solar cell.
[0105] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0106] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A PL testing method for a solar thin-film photovoltaic semiconductor film layer, characterized in that: The PL testing method comprises the following steps: Disposing a barrier protective layer between the surface of the thin-film photovoltaic semiconductor film layer sample to be tested and the EVA layer to obtain a first thin-film photovoltaic semiconductor film layer sample to be tested; Transferring the first thin-film photovoltaic semiconductor film layer sample to be tested into a thin-film photovoltaic semiconductor film layer PL tester for PL testing; Wherein, the barrier protection layer comprises polyethylene terephthalate material or fluorine-containing high molecular polymer.
2. The PL testing method of solar thin film photovoltaic semiconductor film layer according to claim 1, characterized in that: The first thin-film photovoltaic semiconductor film layer sample to be tested includes a photovoltaic semiconductor film layer, and a barrier protective layer, an EVA layer and a photovoltaic glass sheet are sequentially arranged on the surface of the photovoltaic semiconductor film layer, and the vertical projection of the barrier protective layer on the plane where the photovoltaic semiconductor film layer is located covers the vertical projection of the EVA layer on the plane where the photovoltaic semiconductor film layer is located.
3. The PL testing method of solar thin film photovoltaic semiconductor film layer according to claim 2, characterized in that: The step of providing a barrier protective layer between the surface of the thin film photovoltaic semiconductor film layer sample to be tested and the EVA layer to obtain the first thin film photovoltaic semiconductor film layer sample to be tested includes the following process: Select TCO conductive glass as the substrate; Conductive layer coating is performed on the substrate to obtain a solar photovoltaic semiconductor film layer; Disposing the barrier protection layer on the solar photovoltaic semiconductor film layer; After the barrier protective layer is completed, a packaging EVA film and a photovoltaic glass sheet are added on the barrier protective layer in sequence.
4. The PL testing method of solar thin film photovoltaic semiconductor film layer according to claim 2, characterized in that: The EVA layer includes a first side and a second side that are adjacent to each other, the length of the first side is a, and the length of the second side is b; the barrier protection layer includes a third side and a fourth side that are adjacent to each other, the length of the third side is c, and the length of the fourth side is d; wherein c>a, d>b. 5 . The PL testing method for a solar thin-film photovoltaic semiconductor film layer according to claim 4 , wherein the length a of the first side satisfies: 50 mm ≤ a ≤ 300 mm, and the length b of the second side satisfies: 50 mm ≤ b ≤ 300 mm.
6. The PL testing method of solar thin film photovoltaic semiconductor film layer according to claim 1, characterized in that: The step of transferring the first thin-film photovoltaic semiconductor film layer sample to be tested into a thin-film photovoltaic semiconductor film layer PL tester for PL testing comprises the following process: The first thin-film photovoltaic semiconductor film layer sample to be tested is placed between a voltage application plate and a heating platform, and then the equipment parameters of a thin-film photovoltaic semiconductor film layer PL tester are adjusted to perform the test. After the PL test is completed, the first thin-film photovoltaic semiconductor film layer sample to be tested is removed from the thin-film photovoltaic semiconductor film layer PL tester, and the performance parameters of the photovoltaic semiconductor film layer are extracted, and the performance of the photovoltaic semiconductor film layer is evaluated according to the performance parameters; Among them, the equipment parameters of the thin-film photovoltaic semiconductor film layer PL tester include: 1) Temperature range: 25-120℃; 2) Heating and cooling rate: Test conventional component products from 20°C to 80°C and keep it constant for ≤20min; cool from 80°C to 20°C and keep it constant for ≤40min, no load, no light; 3) Temperature fluctuation: no-load, constant state: ≤±0.5℃; full load of 6 pieces of samples, no light constant state: ≤±1℃; full load of 6 pieces of samples, light constant state: ≤±4℃; 4) Temperature uniformity of the entire surface: no-load, constant state: ≤2°C; full load of 6 pieces of samples, no light constant state: ≤3°C; full load of 6 pieces of samples, light constant state: ≤8°C; 5) Temperature deviation: no-load, constant state: ≤±2.0℃; 6) Radiation intensity range: 300W / m 2 ~1200W / m 2 ; 7) Spectral matching: CLASS B AM1.5G; 8) Irradiation non-uniformity: CLASS B ≤ 5%; 9) Radiation instability: CLASSA level ≤ 2%; 10) Irradiation distance: 1500mm; 11) Setting the illumination area of the light source excitation unit to ensure full illumination of the photovoltaic module with an area of 1-3 square meters; 12) Set the angle of a single LED module in the camera unit to 30-60° and the intensity to +16.7W / ㎡ to 67.7W / ㎡; the distance between the camera and the LED to the photovoltaic module is 200 cm to 600 cm, and the integration time is 5-120 milliseconds.
7. The PL testing method of solar thin-film photovoltaic semiconductor film layer according to claim 6, characterized in that: The performance parameters include: electrical performance parameters, depth imaging characterization parameters and interface appearance component parameters.
8. The PL testing method of solar thin-film photovoltaic semiconductor film layer according to claim 6, characterized in that: After the first thin-film photovoltaic semiconductor film layer sample to be tested is moved into a thin-film photovoltaic semiconductor film layer PL tester for PL testing, the method further includes: Acquire test data, wherein the test data includes parallel resistance test data; and evaluate the PL test effect of the photovoltaic semiconductor film layer according to the parallel resistance test data.
Citation Information
Patent Citations
PID test method of solar cell
CN115206818A
Solar cell semi-finished product state evaluation method
CN115565902A
Manufacture of cuinse2 thin-film solar battery
JP1992348542A
Solar cell interconnection, module and panel method
US20110300664A1