Method for preparing photo-induced hydrogenated black battery and photo-induced hydrogenated black battery

By performing photohydrogenation of finished crystalline silicon batteries, the Si-H bond fracture is controlled by differential bond energy of the silicon nitride film layer, the problems of insufficient appearance and light absorption intensity of black crystalline silicon batteries in the prior art are solved, and the problem of insufficient appearance and light absorption intensity of black crystalline silicon batteries in the prior art is realized. Efficient light absorption and black appearance significantly reduce reflectivity.

CN119069570APending Publication Date: 2024-12-03HENGDIAN GRP DMEGC MAGNETICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310639839.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art is difficult to develop black crystalline silicon batteries with beautiful appearance and strong light absorption, and it is impossible to effectively realize the appearance of all-black solar photovoltaic modules.

Method used

By performing photohydrogenation treatment on finished silicon cells, the difference in bond energy breaks between Si-H bonds and N-H bonds in the silicon nitride film layer can control the breakage of Si-H bonds and suppress the breakage of N-H bonds, thereby improving nitriding of nitriding The Si+ content in the silicon film layer changes the refractive index of the silicon nitride film layer, forming a photohydrogenated black cell with beautiful and strong light absorption.

Benefits of technology

The reflectivity of the battery is significantly reduced, especially in the short wavelength range of 300nm to 500nm, and the light absorption intensity is improved, so that the battery appearance is black, with aesthetics and consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069570A_ABST
    Figure CN119069570A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a photo-induced hydrogenated black cell and the photo-induced hydrogenated black cell, and the method comprises the following steps: (1) depositing a silicon nitride film layer on at least one surface of a silicon wafer to obtain a finished crystalline silicon cell; and (2) carrying out photo-induced hydrogenation treatment on the finished crystal silicon battery to obtain the photo-induced hydrogenation black battery. According to the invention, photo-hydrotreating is carried out on the finished crystal silicon cell, and the bond energy fracture difference of Si-H bonds and N-H bonds in the silicon nitride film layer is utilized, so that the fracture of part of Si-H bonds is controlled, the fracture of N-H bonds is inhibited, the content of Si + in the silicon nitride film layer is improved, the refractive index of the silicon nitride film layer is changed, and the refractive index of the silicon nitride film layer is improved. And finally, the photo-induced hydrogenated black battery which is attractive in appearance and high in light absorption is obtained. Besides, compared with a conventional battery, the light-induced hydrogenated black battery has the advantages that the reflectivity of the light-induced hydrogenated black battery is remarkably reduced, especially in the wavelength range of 300-500 nm, the reflectivity is reduced by nearly 5%, and the light absorption intensity of the battery is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar single crystal cells, and in particular relates to a method for preparing a photo-induced hydrogenated black cell and a photo-induced hydrogenated black cell. Background Art

[0002] The global energy system is transforming towards low-carbonization. Large-scale utilization of renewable energy and clean low-carbonization of conventional energy will be the basic trend. Accelerating the development of renewable energy has become the mainstream direction of global energy transformation, and photovoltaic power generation has also become a key area of ​​competition among major countries. Solar cells are mainly large-area semiconductor photodiodes, which are electronic components that directly convert sunlight energy into electrical energy due to the photovoltaic effect. They can convert light energy into electrical energy by utilizing the photoelectric effect after photoelectric materials absorb light energy. Therefore, solar power generation is also called photovoltaic power generation.

[0003] As a clean energy source, the research and development of solar energy has entered a new stage, and more and more end customers have begun to pay attention to the appearance of battery components. Especially in Europe and the United States, all-black solar photovoltaic components are becoming more and more popular among the public due to their consistency and beauty. In some areas, all-black components are even sold at a premium that is significantly higher than regular components.

[0004] To obtain a fully black component, on the one hand, the component materials can be realized by auxiliary means such as black busbars and coated glass. On the other hand, the key material is the battery. The core of the black battery needs to be well controlled at the battery production and manufacturing end. This is the core key point of the black component. For example, CN103000741A discloses a black heterogeneous crystalline silicon battery, which includes a first metal electrode, a first conductive film, a P-type amorphous silicon layer, a first intrinsic amorphous silicon layer, a silicon wafer, a second intrinsic amorphous silicon layer, an N-type amorphous silicon layer, a second conductive film, and a second metal electrode in sequence; the first conductive film and the second conductive film are polycrystalline boron-doped ZnO films. The manufacturing method includes the following steps: pretreatment of the silicon wafer surface; coating of the intrinsic amorphous silicon layer deposited on both sides; deposition of a P-type amorphous silicon layer on the front side and deposition of an N-type amorphous silicon layer on the back side; growth of a ZnO film on the front and back sides of the battery cell, and screen printing of metal grid lines on the conductive films on the front and back sides. This invention realizes light absorption through the velvet light-trapping structure and the surface growth of TCO conductive film layer, thereby forming a so-called black heterogeneous crystalline silicon cell, but it cannot achieve the effect of a black cell. CN102290496A discloses a method for preparing a heterojunction black silicon solar cell, the preparation method comprising the following steps: treating the surface of a silicon wafer to form black silicon; placing the black silicon in a reaction chamber of an atomic layer deposition device; growing a layer of nickel metal on the surface of the black silicon; introducing hydrocarbon substances into the reaction chamber of the atomic layer deposition device to form carbon atoms through plasma discharge, and the carbon atoms spontaneously accumulate on the surface of the nickel metal to form a carbon nanotube structure; coating the surface of the carbon nanotube with a reflective anti-reflection film to form a heterojunction black silicon solar cell. This invention mainly utilizes the light-trapping state of the silicon wafer surface to realize the incident absorption of sunlight, thereby forming the so-called visual black silicon, but it cannot achieve the effect of a black cell.

[0005] Therefore, how to develop a black crystalline silicon battery with beautiful appearance and strong light absorption is a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing a photohydrogenated black cell and a photohydrogenated black cell. The present invention performs photohydrogenation treatment on the finished crystalline silicon cell, and utilizes the difference in bond energy breakage between Si-H bonds and NH bonds in the silicon nitride film layer to control the breakage of some Si-H bonds, while inhibiting the breakage of NH bonds, thereby increasing the Si-H bond energy in the silicon nitride film layer. + The content of silicon nitride changes the refractive index of the silicon nitride film layer, and finally a photo-induced hydrogenated black battery with beautiful appearance and strong light absorption is obtained.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a photo-induced hydrogenated black battery, the method comprising the following steps:

[0009] (1) depositing a silicon nitride film layer on at least one side of a silicon wafer to obtain a finished crystalline silicon cell;

[0010] (2) The finished crystalline silicon cell is subjected to a photo-induced hydrogenation treatment to obtain the photo-induced hydrogenation black cell.

[0011] The present invention performs photoinduced hydrogenation treatment on the finished crystalline silicon cell, and utilizes the difference in bond energy breakage between Si-H bonds and NH bonds in the silicon nitride film layer, thereby controlling the breakage of some Si-H bonds and inhibiting the breakage of NH bonds, thereby increasing the Si in the silicon nitride film layer. + The content of silicon nitride changes the refractive index of the silicon nitride film layer, and finally a photo-induced hydrogenated black battery with beautiful appearance and strong light absorption is obtained.

[0012] In the present invention, the silicon nitride film layer is an indispensable material for solar cells. The dark blue anti-reflection film silicon nitride film is deposited on the surface of the solar cell. It has excellent antioxidant and insulating properties, and has good ability to block sodium ions, mask metal and water vapor diffusion; its chemical stability is also very good. Except for hydrofluoric acid and hot phosphoric acid that can slowly corrode it, other acids basically have no effect on it.

[0013] It should be noted that the bond energy of Si-H is 320KJ·mol -1 The bond energy of NH is 389 kJ·mol -1 Under certain conditions, by utilizing the different dissociation bond energies of Si-H bonds and NH bonds, some Si-H bonds can be dissociated, allowing some H- ions to escape, while the refractive index of the silicon nitride film layer can be changed, thereby further enhancing light absorption and ultimately forming a black battery.

[0014] As a preferred technical solution of the present invention, before the photohydrogenation treatment in step (2), the finished crystalline silicon cell is preheated, and the preheating temperature is 30-50°C, for example, 30°C, 40°C or 50°C.

[0015] In this aspect, the purpose of preheating the finished crystalline silicon cells is to prevent the cells from breaking.

[0016] As a preferred technical solution of the present invention, during the photohydrogenation treatment in step (2), the light intensity is 5-20 sun, for example, it can be 5 sun, 6 sun, 7 sun, 8 sun, 9 sun, 10 sun, 11 sun, 12 sun, 13 sun, 14 sun, 15 sun, 16 sun, 17 sun, 18 sun, 19 sun or 20 sun, etc.

[0017] In the present invention, if the light intensity is too low during the photohydrogenation treatment, the Si-H bonds will not be fully dissociated, the refractive index of silicon nitride will be too large, and the battery will appear blue after lamination. If the light intensity is too high during the photohydrogenation treatment, the Si-H bonds will be excessively dissociated, resulting in a significant decrease in the refractive index of silicon nitride, and the battery will appear gray-brown after lamination.

[0018] As a preferred technical solution of the present invention, during the photohydrogenation treatment in step (2), the temperature is 40-60°C, for example, it can be 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, etc.

[0019] In the present invention, if the temperature is too low during the photohydrogenation treatment, the Si-H bonds will not be fully dissociated, the refractive index of silicon nitride will be too large, and the battery will appear blue after lamination. If the temperature is too high during the photohydrogenation treatment, the Si-H bonds will be excessively dissociated, resulting in a significant decrease in the refractive index of silicon nitride, and the battery will appear gray-brown after lamination.

[0020] As a preferred technical solution of the present invention, the time for the photohydrogenation treatment in step (2) is 40-80s, for example, it can be 40s, 42s, 44s, 46s, 48s, 50s, 52s, 54s, 56s, 58s, 60s, 62s, 64s, 66s, 68s, 70s, 72s, 74s, 76s, 78s or 80s.

[0021] In the present invention, if the photohydrogenation treatment time is too short, the Si-H bonds will not be fully dissociated, the refractive index of silicon nitride will be too large, and the battery will present a blue color after lamination to the component; if the photohydrogenation treatment time is too long, the Si-H bonds will be excessively dissociated, resulting in a significant decrease in the refractive index of silicon nitride, and the battery will present a gray-brown color after lamination to the component.

[0022] As a preferred technical solution of the present invention, after the photo-induced hydrogenation treatment in step (2), the refractive index of the silicon nitride film layer is 1.9-2.1, for example, it can be 1.9, 1.95, 2, 2.05 or 2.1.

[0023] In the present invention, if the refractive index of the silicon nitride film layer after photohydrogenation treatment is too large, the battery will appear blue after lamination; if the refractive index of the silicon nitride film layer after photohydrogenation treatment is too small, the battery will appear gray-brown after lamination.

[0024] As a preferred technical solution of the present invention, before depositing the silicon nitride film layer on the silicon wafer in step (1), the following steps are first performed:

[0025] The silicon wafer is textured, boron-diffused, phosphorus-diffused and an aluminum oxide passivation layer is deposited.

[0026] As a preferred technical solution of the present invention, the thickness of the silicon nitride film layer in step (1) is 45-60 nm, for example, 45 nm, 50 nm, 55 nm or 60 nm.

[0027] As a preferred technical solution of the present invention, the method of depositing the silicon nitride film layer in step (1) includes a plasma CVD method.

[0028] The present invention is not limited to the plasma CVD method, and illustratively, it may be a plasma enhanced CVD method.

[0029] Preferably, the specific step of depositing the silicon nitride film layer includes: ionizing a silicon source and a nitrogen source, and depositing the silicon nitride film layer on at least one side of a silicon wafer.

[0030] As a preferred technical solution of the present invention, the silicon source includes any one of SiH4, SiCl3H, SiF4, SiCl4 or SiH2Cl2, or a combination of at least two thereof.

[0031] Preferably, the nitrogen source includes any one of NH3, N2, NO or NO2, or a combination of at least two of them.

[0032] In the present invention, the deposition principle of the silicon nitride film layer is as follows: 4NH3+3SiH4→Si3N4+12H2↑.

[0033] As a preferred technical solution of the present invention, the method comprises the following steps:

[0034] (I) using a plasma enhanced CVD method, ionizing a silicon source and a nitrogen source, and depositing a silicon nitride film layer on the front and back of a silicon wafer;

[0035] (II) setting the light intensity of the photohydrogenation furnace to 5-20 sun and the temperature of the photohydrogenation furnace to 40-60°C;

[0036] (III) sending the finished crystalline silicon cell to a photohydrogenation furnace for 40-80 seconds of photohydrogenation treatment;

[0037] (IV) Cooling the processed finished crystalline silicon cell to room temperature to obtain the photoinduced hydrogenated black cell.

[0038] It should be noted that the present invention does not specifically limit the room temperature. For example, it can be 20°C, 22°C, 24°C, 26°C, 28°C or 30°C.

[0039] In a second aspect, the present invention provides a photo-induced hydrogenated black cell, which is prepared by the method described in the first aspect.

[0040] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] (1) The present invention performs photoinduced hydrogenation treatment on the finished crystalline silicon cell and utilizes the difference in bond energy breakage between Si-H bonds and NH bonds in the silicon nitride film layer, thereby controlling the breakage of some Si-H bonds and inhibiting the breakage of NH bonds, thereby improving the Si-H bond breakage in the silicon nitride film layer. + The content of silicon nitride changes the refractive index of the silicon nitride film layer, and finally a photo-induced hydrogenated black battery with beautiful appearance and strong light absorption is obtained.

[0043] (2) Compared with conventional batteries, the reflectivity of the photo-induced hydrogenated black battery prepared by the present invention is significantly reduced, especially in the short wavelength range of 300nm to 500nm, the reflectivity value is reduced by nearly 5%, which effectively improves the light absorption intensity of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 Schematic diagram of the principle of photo-induced hydrogenation treatment in Example 1 of the present invention.

[0045] Figure 2 This is a process flow chart for preparing a photo-induced hydrogenated black battery in Example 1 of the present invention.

[0046] Figure 3 This is a schematic diagram of the photo-induced hydrogenated black battery prepared in Example 1 of the present invention.

[0047] Figure 4 This is a schematic diagram of a conventional crystalline silicon cell prepared in Comparative Example 1 of the present invention.

[0048] Figure 5 The reflectivity curves of the photohydrogenated black cell prepared in Example 1 of the present invention and the conventional crystalline silicon cell prepared in Comparative Example 1 are shown. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0050] In the following examples, room temperature refers to 25°C.

[0051] Example 1

[0052] This embodiment provides a method for preparing a photo-induced hydrogenated black battery. The process flow chart of the method is as follows: Figure 2 As shown, the method comprises the following steps:

[0053] (1) The silicon wafer is sequentially subjected to texturing, boron diffusion, SE laser doping, high-temperature advancement (i.e., high-temperature repair of the doped area at 900°C), chain BSG removal (i.e., removal of the BSG of the edge and back), groove back polishing (i.e., alkaline etching of the edge and back), preparation of a tunneling oxide layer and a doped polysilicon layer (i.e., preparation of a TOPCon tunneling structure), phosphorus diffusion, chain PSG removal (i.e., removal of the PSG of the front side and the PSG of the edge), groove poly removal and RCA cleaning (i.e., alkaline polishing to remove the poly of the edge of the front side and HF to remove the BSG of the front side), and deposition of an aluminum oxide passivation layer;

[0054] The boron diffusion temperature is 975° C., the boron source is BCl 3 , the method for preparing the tunneling oxide layer and the doped polysilicon layer is the LPCVD method, and the method for depositing the aluminum oxide passivation layer is the ALD method.

[0055] (2) using plasma enhanced CVD to ionize a silicon source and a nitrogen source, and depositing a 50 nm thick silicon nitride film layer on the front and back sides of the silicon wafer;

[0056] (3) Printing metal electrodes on the front and back of the silicon wafer respectively, and then sintering in a sintering furnace at 750°C for metal alloying to obtain a finished crystalline silicon cell;

[0057] (4) Set the light intensity of the photohydrogenation furnace to 10 sun and the temperature of the photohydrogenation furnace to 50 °C;

[0058] (5) Place the finished crystalline silicon cell with the front grid line facing upward on a conveyor belt and send it to a photohydrogenation furnace. Preheat the cell to 30° C. in the preheating zone, and then perform a photohydrogenation treatment on the cell for 60 seconds in the photohydrogenation zone, so that the refractive index of the silicon nitride film layer is 1.9;

[0059] (6) The processed finished crystalline silicon battery is sent to a cooling zone, cooled to room temperature, and then discharged to obtain the photoinduced hydrogenated black battery.

[0060] Figure 1 The schematic diagram of the principle of the photoinduced hydrogenation treatment in this embodiment is shown. As can be seen from the figure, the difference in the bond energy of Si-H bonds and NH bonds in the silicon nitride film layer is used to control the breaking of some Si-H bonds and inhibit the breaking of NH bonds, thereby improving the Si in the silicon nitride film layer. + The content of MgO changes the refractive index of the silicon nitride film.

[0061] Figure 3 The schematic diagram of the photo-induced hydrogenated black battery prepared in this embodiment is shown. As can be seen from the figure, the photo-induced hydrogenated black battery prepared in this embodiment has a black appearance.

[0062] Example 2

[0063] This embodiment provides a method for preparing a photo-induced hydrogenated black battery, the method comprising the following steps:

[0064] (1) The silicon wafer is sequentially subjected to texturing, boron diffusion, SE laser doping, high-temperature advancement (i.e., high-temperature repair of the doped area at 800°C), chain BSG removal (i.e., removal of the BSG of the edge and back), groove back polishing (i.e., alkaline etching of the edge and back), preparation of a tunneling oxide layer and a doped polysilicon layer (i.e., preparation of a TOPCon tunneling structure), phosphorus diffusion, chain PSG removal (i.e., removal of the PSG of the front side and the PSG of the edge), groove poly removal and RCA cleaning (i.e., alkaline polishing to remove the poly of the edge of the front side and HF to remove the BSG of the front side), and deposition of an aluminum oxide passivation layer;

[0065] The boron diffusion temperature is 950° C., the boron source is BCl 3 , the method for preparing the tunneling oxide layer and the doped polysilicon layer is the LPCVD method, and the method for depositing the aluminum oxide passivation layer is the ALD method.

[0066] (2) using a plasma enhanced CVD method to ionize a silicon source and a nitrogen source, and depositing a 45 nm thick silicon nitride film layer on the front and back sides of the silicon wafer;

[0067] (3) Printing metal electrodes on the front and back of the silicon wafer respectively, and then sintering in a sintering furnace at 700°C to alloy the metal to obtain a finished crystalline silicon cell;

[0068] (4) Set the light intensity of the photohydrogenation furnace to 5 sun and the temperature of the photohydrogenation furnace to 60 °C;

[0069] (5) Place the finished crystalline silicon cell with the front grid line facing upward on a conveyor belt and send it to a photohydrogenation furnace. Preheat the cell to 30° C. in the preheating zone, and then perform a photohydrogenation treatment on the cell for 40 seconds in the photohydrogenation zone, so that the refractive index of the silicon nitride film layer is 2;

[0070] (6) The processed finished crystalline silicon battery is sent to a cooling zone, cooled to room temperature, and then discharged to obtain the photoinduced hydrogenated black battery.

[0071] Example 3

[0072] This embodiment provides a method for preparing a photo-induced hydrogenated black battery, the method comprising the following steps:

[0073] (1) The silicon wafer is sequentially subjected to texturing, boron diffusion, SE laser doping, high-temperature advancement (i.e., high-temperature repair of the doped area at a temperature of 1000°C), chain BSG removal (i.e., removal of the BSG of the edge and back), groove back polishing (i.e., alkaline etching of the edge and back), preparation of a tunneling oxide layer and a doped polysilicon layer (i.e., preparation of a TOPCon tunneling structure), phosphorus diffusion, chain PSG removal (i.e., removal of the PSG of the front side and the PSG of the edge), groove poly removal and RCA cleaning (i.e., alkaline polishing to remove the poly of the edge of the front side and HF to remove the BSG of the front side), and deposition of an aluminum oxide passivation layer;

[0074] The boron diffusion temperature is 1000°C, the boron source is BCl3, the method for preparing the tunnel oxide layer and the doped polysilicon layer is the LPCVD method, and the method for depositing the aluminum oxide passivation layer is the ALD method.

[0075] (2) using a plasma enhanced CVD method to ionize a silicon source and a nitrogen source, and deposit a 60 nm thick silicon nitride film layer on the front and back sides of the silicon wafer;

[0076] (3) Printing metal electrodes on the front and back of the silicon wafer respectively, and then sintering in a sintering furnace at 750°C for metal alloying to obtain a finished crystalline silicon cell;

[0077] (4) Setting the light intensity of the photohydrogenation furnace to 20 suns and the temperature of the photohydrogenation furnace to 40°C;

[0078] (5) Place the finished crystalline silicon cell with the front grid line facing upward on a conveyor belt and send it to a photohydrogenation furnace. Preheat the cell to 30° C. in the preheating zone, and then perform a photohydrogenation treatment on the cell for 80 seconds in the photohydrogenation zone, so that the refractive index of the silicon nitride film layer is 1.95;

[0079] (6) The processed finished crystalline silicon battery is sent to a cooling zone, cooled to room temperature, and then discharged to obtain the photoinduced hydrogenated black battery.

[0080] Example 4

[0081] The difference between this embodiment and embodiment 1 is that in step (4), the light intensity of the photohydrogenation furnace is set to 3 sun.

[0082] The rest of the preparation methods and parameters were the same as those in Example 1.

[0083] Example 5

[0084] The difference between this embodiment and embodiment 1 is that the light intensity of the photohydrogenation furnace is set to 23 sun in step (4).

[0085] The rest of the preparation methods and parameters were the same as those in Example 1.

[0086] Example 6

[0087] The difference between this embodiment and embodiment 1 is that the temperature of the photohydrogenation furnace is set to 35° C. in step (4).

[0088] The rest of the preparation methods and parameters were the same as those in Example 1.

[0089] Example 7

[0090] The difference between this embodiment and embodiment 1 is that the temperature of the photohydrogenation furnace is set to 65° C. in step (4).

[0091] The rest of the preparation methods and parameters were the same as those in Example 1.

[0092] Example 8

[0093] The difference between this embodiment and embodiment 1 is that the time of the photo-induced hydrogenation treatment in step (5) is 30 seconds.

[0094] The rest of the preparation methods and parameters were the same as those in Example 1.

[0095] Example 9

[0096] The difference between this embodiment and embodiment 1 is that the time of the photo-induced hydrogenation treatment in step (5) is 90 seconds.

[0097] The rest of the preparation methods and parameters were the same as those in Example 1.

[0098] Comparative Example 1

[0099] The difference between this comparative example and Example 1 is that steps (4) to (6) are not performed, that is, a conventional crystalline silicon cell is prepared in this comparative example.

[0100] The rest of the preparation methods and parameters were the same as those in Example 1.

[0101] Figure 4 A schematic diagram of the photo-hydrogenated black battery prepared in this comparative example is shown. As can be seen from the figure, the photo-hydrogenated black battery prepared in this comparative example has a blue appearance.

[0102] Figure 5 The reflectivity curves of the photohydrogenated black cell prepared in Example 1 and the conventional crystalline silicon cell prepared in Comparative Example 1 are shown. It can be seen that the reflectivity of the cell treated by photohydrogenation shows an obvious downward trend compared with the conventional cell, especially in the short wavelength range of 300nm to 500nm, where the reflectivity value drops by nearly 5%.

[0103] Performance Testing

[0104] The photo-hydrogenated black cells prepared in Examples 1-9 and the conventional crystalline silicon cells prepared in Comparative Example 1 were subjected to reflectivity tests to detect the intensity of the cells' light absorption.

[0105] The test results are shown in Table 1.

[0106] Table 1

[0107]

[0108]

[0109] analyze:

[0110] As can be seen from the above table, the present invention performs photohydrogenation treatment on the finished crystalline silicon cells to obtain photohydrogenated black cells with excellent light absorption performance and a black appearance, so that the photovoltaic module has an excellent consistent black appearance and aesthetics.

[0111] By comparing the data results of Example 1 with those of Examples 4-5, it can be seen that if the light intensity is too low, the Si-H bonds will not be sufficiently cleaved, resulting in the refractive index of the film layer of the treated battery being greater than 2.1, and the battery will appear blue after lamination to the component; if the light intensity is too high, the Si-H bonds will be excessively cleaved, resulting in the refractive index of the film layer of the treated battery being less than 1.9, and the battery will appear gray-brown after lamination to the component.

[0112] By comparing the data results of Example 1 with those of Examples 6-7, it can be seen that if the temperature of the photohydrogenation furnace is too low, the Si-H bonds will not be sufficiently cleaved, resulting in the refractive index of the film layer of the treated battery being greater than 2.1, and the battery will appear blue after lamination to the component; if the temperature of the photohydrogenation furnace is too high, the Si-H bonds will be excessively cleaved, resulting in the refractive index of the film layer of the treated battery being less than 1.9, and the battery will appear gray-brown after lamination to the component.

[0113] By comparing the data results of Example 1 with those of Examples 8-9, it can be seen that if the time of the photohydrogenation treatment is too short, the Si-H bonds will not be sufficiently cleaved, resulting in the refractive index of the film layer of the treated battery being greater than 2.1, and the battery will appear blue after lamination to the component; if the time of the photohydrogenation treatment is too long, the Si-H bonds will be excessively cleaved, resulting in the refractive index of the film layer of the treated battery being less than 1.9, and the battery will appear gray-brown after lamination to the component.

[0114] From the comparison of the data results of Example 1 and Comparative Example 1, it can be seen that compared with the conventional battery, the reflectivity can be seen to have an obvious downward trend, indicating that the photohydrogenated black battery prepared by the present invention has excellent light absorption ability.

[0115] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a photo-induced hydrogenated black battery, It is characterized in that The method comprises the following steps: (1) depositing a silicon nitride film layer on at least one side of a silicon wafer to obtain a finished crystalline silicon cell; (2) The finished crystalline silicon cell is subjected to a photo-induced hydrogenation treatment to obtain the photo-induced hydrogenation black cell.

2. The method according to claim 1, It is characterized in that During the photohydrogenation treatment in step (2), the light intensity is 5-20 sun.

3. The method according to claim 1 or 2, It is characterized in that During the photohydrogenation treatment in step (2), the temperature is 40-60°C.

4. The method according to any one of claims 1 to 3, It is characterized in that The time of the photo-induced hydrogenation treatment in step (2) is 40-80 seconds.

5. The method according to any one of claims 1 to 4, It is characterized in that After the photoinduced hydrogenation treatment in step (2), the refractive index of the silicon nitride film layer is 1.9-2.1, preferably 1.9-2.

6. The method according to any one of claims 1 to 5, It is characterized in that The thickness of the silicon nitride film layer in step (1) is 45-60nm.

7. The method according to any one of claims 1 to 6, It is characterized in that The method for depositing the silicon nitride film layer in step (1) comprises a plasma CVD method; Preferably, the specific step of depositing the silicon nitride film layer comprises: ionizing a silicon source and a nitrogen source, and depositing the silicon nitride film layer on at least one side of a silicon wafer.

8. The method according to claim 7, It is characterized in that The silicon source includes SiH 4 、SiCl 3 H、SiF 4 、SiCl 4 or SiH 2 Cl 2 Any one or a combination of at least two of the following: Preferably, the nitrogen source comprises NH 3 、N 2 , NO or NO 2 Any one or a combination of at least two of the following.

9. The method according to any one of claims 1 to 8, It is characterized in that The method comprises the following steps: (I) using a plasma enhanced CVD method, ionizing a silicon source and a nitrogen source, and depositing a silicon nitride film layer on the front and back of a silicon wafer; (II) setting the light intensity of the photohydrogenation furnace to 5-20 sun and the temperature of the photohydrogenation furnace to 40-60°C; (III) sending the finished crystalline silicon cell to a photohydrogenation furnace for 40-80 seconds of photohydrogenation treatment; (IV) Cooling the processed finished crystalline silicon cell to room temperature to obtain the photoinduced hydrogenated black cell.

10. A photo-induced hydrogen black battery, It is characterized in that The photo-induced hydrogenated black battery is prepared by the method according to any one of claims 1 to 9.