Negative plate of negative-electrode-free lithium metal battery and lithium ion battery
By using a polymer coating with carboxymethylcellulose salt as the main component in a negative electrode-free lithium metal battery, an artificial SEI film is formed, which solves the problems of lithium dendrites growth and electrical performance, and achieves high efficiency and density of lithium metal batteries. Improved deposition and electrochemical performance.
Patent Information
- Application Number
- CN202411193124.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
During the cycle process, the negative electrode lithium metal battery has uneven deposition, high reactivity and large volume changes, resulting in lithium dendrites growing, electrical performance degraded, and the existing solutions are costly and inconvenient to operate.
The negative electrode sheet of lithium metal battery with negative electrodes including negative electrode current collector and polymer coating is used. The polymer coating consists of polymer polymers, mainly carboxymethyl cellulose salts, and is made of artificial The SEI film is used to inhibit the growth of lithium dendrites and to form a dense film layer by hydrogen bond crosslinking.
Effectively inhibit the growth of lithium dendrites, improve the overall electrical performance of lithium metal batteries, simplify the preparation process, reduce costs, and enhance the cycle stability and safety of the battery.
Smart Images

Figure CN119069630A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a negative electrode sheet of a negative electrode-free lithium metal battery and a lithium ion battery. Background Art
[0002] In recent years, as the requirements for energy density and safety of lithium-ion batteries continue to increase, lithium metal anodes with ultra-high theoretical specific capacity have become a research hotspot. Based on limiting the amount of lithium used, researchers have proposed "anode-free" lithium metal batteries, which have the advantages of high energy density, low cost, and high safety.
[0003] "Non-anode" lithium metal batteries refer to batteries that only use negative electrode current collectors and do not add active materials as negative electrodes during the production process. On the one hand, the manufacturing process of "non-anode" lithium metal batteries is relatively simplified, and ultra-thin lithium metal is not required, which is conducive to increasing the volume and weight energy density of lithium-ion batteries. On the other hand, there is no free lithium metal in the assembly process of "non-anode" lithium metal batteries, which improves battery life and safety. However, "non-anode" lithium metal batteries are still limited by the problems faced by lithium metal negative electrodes in practical applications. For example, the metallic lithium deposited on the negative electrode has high reaction activity and large volume changes during the cycle, which leads to the growth of lithium dendrites and the decline of electrical performance. Most of the current research is based on the construction of a three-dimensional copper foil skeleton, which requires the addition of special processes, is costly, and is not easy to operate. Generally speaking, roughening or alloying the copper foil surface is one of the key and efficient strategies to reduce the nucleation overpotential of lithium metal and inhibit the growth of lithium dendrites. It has great application potential, but its cost is high, and special processes need to be added to the existing preparation process. In addition, poor interface contact may lead to problems such as uneven lithium deposition. Summary of the invention
[0004] To address the problems in the prior art of negative electrode-free lithium metal batteries, such as uneven deposition of negative electrode metal lithium, high reaction activity and large volume changes during the cycle process, which lead to growth of lithium dendrites and degradation of electrical performance, a negative electrode sheet for a negative electrode-free lithium metal battery and a lithium ion battery are provided.
[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0006] On the one hand, the present invention provides a negative electrode sheet for a negative electrode-free lithium metal battery, comprising a negative electrode current collector and a polymer coating, wherein the polymer coating is coated on the surface of the negative electrode current collector, the polymer coating comprises a high molecular polymer, and the high molecular polymer comprises carboxymethyl cellulose salt.
[0007] Optionally, based on the total mass of the polymer coating being 100%, the mass percentage of the carboxymethyl cellulose salt is 90% or more.
[0008] Optionally, the degree of substitution of the carboxymethyl cellulose salt is 0.5 to 1.5.
[0009] Optionally, the molecular weight of the high molecular weight polymer is 20-30W.
[0010] Optionally, the carboxymethyl cellulose salt includes one or more of lithium carboxymethyl cellulose, sodium carboxymethyl cellulose and potassium carboxymethyl cellulose.
[0011] Optionally, the negative electrode current collector is copper foil.
[0012] Optionally, the polymer coating has a thickness of 0.5 μm to 3 μm.
[0013] Optionally, the thickness of the negative electrode current collector is 8 μm to 9 μm.
[0014] On the other hand, the present invention provides a method for preparing a negative electrode sheet of a negative electrode-free lithium metal battery, comprising the following operations:
[0015] S1: obtaining a polymer solution containing carboxymethyl cellulose salt;
[0016] S2: Applying the high molecular polymer solution to the surface of the negative electrode current collector, and after drying, obtaining a negative electrode sheet for a negative electrode-free lithium metal battery.
[0017] Optionally, the solid content of the polymer in the polymer solution is 1.0% to 4%.
[0018] Optionally, S1 comprises: mixing carboxymethyl cellulose salt with a solvent to obtain a high molecular polymer solution containing carboxymethyl cellulose salt, the mixing rate being 600 to 1000 rpm and the mixing time being 30 to 60 min;
[0019] In S2, the drying time is 12 to 24 hours and the drying temperature is 60 to 80°C.
[0020] On the other hand, the present invention provides a lithium ion battery, comprising the negative electrode sheet of the negative electrode-free lithium metal battery.
[0021] The beneficial effects of the present invention are:
[0022] The negative electrode sheet of a negative electrode-free lithium metal battery provided by the present invention comprises a negative electrode current collector and a polymer coating, wherein the polymer coating is coated on the surface of the negative electrode current collector, the polymer coating comprises a high molecular polymer, and the high molecular polymer comprises a carboxymethyl cellulose salt; the polymer coating serves as an artificial SEI film of the negative electrode, and the carboxymethyl cellulose salt in the polymer coating has a high ion transfer number, which provides diffusion channels for lithium ions and redistributes lithium ion flux at the same time, thereby realizing dense deposition of lithium metal and inhibiting the growth of lithium dendrites; secondly, the carboxymethyl cellulose salt forms a uniform and dense film layer through hydrogen bond cross-linking, has a high Young's modulus, and can inhibit the penetration of lithium dendrites; in addition, the carboxymethyl cellulose salt has a low swelling rate in the electrolyte, which can avoid the reaction of active lithium metal with the electrolyte, reduce the loss of irreversible lithium source in the lithium metal battery, solve the problems of uneven lithium deposition and large volume change in the negative electrode-free lithium metal battery, can effectively improve the overall electrical performance of the lithium metal battery, and the preparation method is simple and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a topographical image of a negative electrode sheet to which a high molecular polymer solution is applied provided in Example 1 of the present invention;
[0024] Figure 2 This is a morphology diagram of the negative electrode sheet provided in Comparative Example 1 of the present invention without applying the high molecular polymer solution. DETAILED DESCRIPTION
[0025] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] The invention provides a negative electrode sheet for a negative electrode-free lithium metal battery, comprising a negative electrode current collector and a polymer coating, wherein the polymer coating is coated on the surface of the negative electrode current collector, the polymer coating comprises a high molecular polymer, and the high molecular polymer comprises a carboxymethyl cellulose salt.
[0027] The negative electrode sheet of a negative electrode-free lithium metal battery provided by the present invention comprises a negative electrode current collector and a polymer coating, wherein the polymer coating is coated on the surface of the negative electrode current collector, the polymer coating comprises a high molecular polymer, and the high molecular polymer comprises a carboxymethyl cellulose salt; the polymer coating serves as an artificial SEI film of the negative electrode, and the carboxymethyl cellulose salt in the polymer coating has a high ion transfer number, which provides diffusion channels for lithium ions and redistributes lithium ion flux at the same time, thereby realizing dense deposition of lithium metal and inhibiting the growth of lithium dendrites; secondly, the carboxymethyl cellulose salt forms a uniform and dense film layer through hydrogen bond cross-linking, has a high Young's modulus, and can inhibit the penetration of lithium dendrites; in addition, the carboxymethyl cellulose salt has a low swelling rate in the electrolyte, which can avoid the reaction of active lithium metal with the electrolyte, reduce the loss of irreversible lithium source in the lithium metal battery, solve the problems of uneven lithium deposition and large volume change in the negative electrode-free lithium metal battery, can effectively improve the overall electrical performance of the lithium metal battery, and the preparation method is simple and easy to operate.
[0028] In some embodiments, based on the total mass of the polymer coating being 100%, the mass percentage of the carboxymethyl cellulose salt is 90% or more.
[0029] In some embodiments, the degree of substitution of the carboxymethyl cellulose salt is 0.5-1.5.
[0030] It should be noted that the -H on the carboxymethyl chain of carboxymethyl cellulose can be replaced by Na / Li / K ions, and the degree of substitution (DS) determines the performance of the carboxymethyl cellulose film and the conductivity of Li+. The lower the degree of substitution of carboxymethyl cellulose, the more intermolecular hydrogen bonds, the stronger the molecular cross-linking effect, and the excessive viscosity leads to the problem of easy shrinkage of the coating after coating. On the contrary, the higher the degree of substitution, the fewer intermolecular hydrogen bonds, the weaker the cross-linking, the lower the viscosity, and the current collector foil is exposed, which is not conducive to the uniformity of the coating. The substitution of different ions in carboxymethyl cellulose will also affect the electrical properties of the coating. The degree of substitution of carboxymethyl cellulose salt directly affects its physical and chemical properties such as solubility, viscosity, and stability. By precisely controlling the reaction conditions, material ratios, and post-treatment methods, the degree of substitution of carboxymethyl cellulose can be effectively adjusted to meet different application requirements. For example, in battery manufacturing, carboxymethyl cellulose with a low degree of substitution can provide better electrode bonding performance and electrochemical stability.
[0031] Specifically, the carboxymethyl cellulose salt is a derivative of carboxymethyl cellulose. When the degree of substitution is in the range of 0.5 to 1.5, the formed polymer coating has good adhesion and good ionic conductivity, thereby stabilizing the negative electrode interface, reducing the lithium nucleation barrier, promoting the uniform deposition of lithium ions, and improving the electrochemical performance; specifically, the degree of substitution of the carboxymethyl cellulose salt can be 0.5, 0.8, 1.0, 1.2 or 1.5. In a preferred embodiment, the degree of substitution of the carboxymethyl cellulose salt is 0.8 to 1.2.
[0032] In some embodiments, the molecular weight of the high molecular weight polymer is 20-30W.
[0033] In some embodiments, the carboxymethylcellulose salt includes one or more of lithium carboxymethylcellulose, sodium carboxymethylcellulose, and potassium carboxymethylcellulose.
[0034] It should be noted that lithium carboxymethyl cellulose (CMC-Li) is the product of sodium carboxymethyl cellulose (CMC-Na) acidified and then neutralized with lithium hydroxide. When applied to lithium-ion batteries, it can effectively inhibit the growth of lithium dendrites and thus improve battery performance. Potassium carboxymethyl cellulose (CMC-K) is also a derivative of carboxymethyl cellulose. Potassium carboxymethyl cellulose is a potassium salt form of carboxymethyl cellulose generated by the reaction of natural cellulose with chloroacetic acid under alkaline conditions. Its viscosity depends on the molecular weight and degree of substitution of the polymer.
[0035] The potassium carboxymethyl cellulose has good viscosity and adhesion. In the preparation of the polymer coating, it exerts its stable viscosity and adhesion, thereby helping to improve the cycle performance of the battery and increase the charge and discharge stability and life of the battery; the lithium carboxymethyl cellulose has a high ion transfer number, a high Young's modulus of 24.6 GPa and good lithium affinity, and can achieve ultra-high density lithium deposition on a copper current collector, thereby significantly improving the cycle stability and safety of lithium metal batteries; the sodium carboxymethyl cellulose helps to maintain the porosity and microstructure of the electrode, provides a good channel for ion transmission, improves the rate performance and charge and discharge efficiency of the battery, and the stable viscosity and good adhesion help to improve the cycle performance of the battery.
[0036] Specifically, taking the preparation of the lithium carboxymethyl cellulose as an example, the preparation principle is as follows: CMC-Na is acidified under the action of HCl to generate an acidic form of CMC, and then reacts with lithium hydroxide to replace sodium ions with lithium ions to form CMC-Li, and the degree of substitution DS of lithium ions can be adjusted and controlled by the amount of LiOH solution; CMC-Li has a relatively high Young's modulus of up to 25 Gpa, which can inhibit the penetration of lithium dendrites.
[0037] In some embodiments, the polymer coating has a thickness of 0.5 μm to 3 μm.
[0038] Specifically, the polymer coating needs to have both strong adhesion and excellent ionic conductivity. If the polymer coating is too thin, the polymer may phase separate during the drying process, resulting in the absence of polymer coating in some areas of the negative electrode current collector, causing local current density unevenness. If the polymer coating is too thick, the migration speed of lithium ions is slow, which may increase polarization. When the thickness of the polymer coating is controlled at 0.5μm to 3μm, it has good adhesion, which is beneficial to improve the interface contact between the polymer coating and the negative electrode current collector, and helps to increase the migration speed of ions.
[0039] In some embodiments, the negative electrode current collector is copper foil.
[0040] Specifically, the thickness of the polymer coating may be 0.5 μm, 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm or 3.0 μm. In a preferred embodiment, the thickness of the polymer coating is 1.0 μm to 2 μm.
[0041] In some embodiments, the thickness of the negative electrode current collector is 8 μm to 9 μm.
[0042] Specifically, in a preferred embodiment, the thickness of the negative electrode current collector is 9 μm.
[0043] Specifically, the negative electrode current collector is selected from copper foil.
[0044] Another embodiment of the present invention provides a method for preparing a negative electrode sheet of a negative electrode-free lithium metal battery, comprising the following operations:
[0045] S1: obtaining a polymer solution containing carboxymethyl cellulose salt;
[0046] S2: Applying the high molecular polymer solution to the surface of the negative electrode current collector, and after drying, obtaining a negative electrode sheet for a negative electrode-free lithium metal battery.
[0047] Specifically, the polymer is mixed with a solvent until the polymer powder is completely dissolved to obtain a polymer solution, and in order to avoid bubbles in the polymer solution that affect the coating effect, a vacuum degassing treatment is performed;
[0048] The high molecular polymer solution is evenly applied on the surface of the copper foil, the coating speed is 8 mm / s, the scraper gap is 50 μm, and after the coating is completed, the solvent is baked to remove the negative electrode of the lithium metal battery without a negative electrode of uniform thickness.
[0049] In a preferred embodiment, the solvent is deionized water.
[0050] Specifically, the high molecular polymer solution can be attached to the surface of the copper foil by spraying, shower coating and dipping.
[0051] In some embodiments, the solid content of the polymer in the polymer solution is 1.0% to 4%.
[0052] It should be noted that a low solid content of the polymer in the polymer solution may cause uneven shrinkage of the material during the drying or film-forming process, and an excessively high solid content may increase the crystallinity of the polymer and may cause inorganic fillers to agglomerate and block ion transport channels. In addition, an excessively high solid content of the polymer in the polymer solution leads to reduced flexibility of the electrolyte membrane, which affects its interfacial contact with the electrode material and further affects the cycle stability of the battery. That is, a high or low solid content of the polymer in the polymer solution will have many adverse effects on the cycle performance of the battery. Therefore, when designing and preparing the polymer in the polymer solution, the solid content should be reasonably controlled to optimize the overall performance of the battery.
[0053] Specifically, the solid content of the polymer in the polymer solution may be 1.0%, 1.2%, 1.5%, 2%, 2.5%, 3% or 4%. In a preferred embodiment, the solid content of the polymer in the polymer solution is 1.2% to 2%.
[0054] In some embodiments, S1 comprises: mixing carboxymethyl cellulose salt with a solvent to obtain a polymer solution containing carboxymethyl cellulose salt, the mixing rate being 600 to 1000 rpm and the mixing time being 30 to 60 min;
[0055] In S2, the drying time is 12 to 24 hours and the drying temperature is 60 to 80°C.
[0056] Specifically, in a preferred embodiment, in S1, the mixing rate is 600 rpm and the mixing time is 30 min;
[0057] In S2, the drying temperature is 60°C.
[0058] Another embodiment of the present invention provides a lithium-ion battery, comprising the negative electrode sheet of the negative electrode-free lithium metal battery.
[0059] Specifically, a lithium-ion battery provided in another embodiment of the present invention further includes a positive electrode sheet, a separator and a shell, wherein the positive electrode sheet, the negative electrode sheet and the separator are stacked to obtain a bare battery cell placed in the inner cavity of the shell; the lithium-ion battery includes the negative electrode-free lithium metal battery negative electrode sheet provided by the present invention, including a negative electrode current collector and a polymer coating, wherein the polymer coating is coated on the surface of the negative electrode current collector, wherein the polymer coating includes a high molecular polymer, and the polymer coating serves as an artificial SEI film of the negative electrode, has a high ion transfer number, provides a diffusion channel for lithium ions, and redistributes the lithium ions through the negative electrode current collector. The amount of lithium metal can be deposited densely to inhibit the growth of lithium dendrites. Secondly, the high molecular polymer in the polymer coating forms a uniform and dense film layer through hydrogen bond cross-linking, which has a high Young's modulus and can inhibit the penetration of lithium dendrites. In addition, the high molecular polymer in the polymer coating has a low swelling rate in the electrolyte, which can avoid the reaction of active lithium metal with the electrolyte and reduce the loss of irreversible lithium source in the lithium metal battery, solving the problems of uneven lithium deposition and large volume change in negative electrode-free lithium metal batteries, which can effectively improve the overall electrical performance of lithium metal batteries, and the preparation method is simple and easy to operate.
[0060] The present invention is further described below by way of examples.
[0061] Example 1
[0062] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes the following operating steps:
[0063] S1: The carboxymethyl group in carboxymethyl cellulose is replaced by carboxymethyl lithium, that is, CMC-Na is acidified with HCl and then neutralized with lithium hydroxide to obtain CMC-Li, with a degree of substitution of 0.8;
[0064] S2: CMC-Li and water are mixed at 600 rpm for 30 min until the powder is completely dissolved to obtain a polymer solution, wherein the solid content of CMC-Li in the polymer solution is 1.2% and the molecular weight is 20-30W;
[0065] S3: Take the polymer solution of S2 and apply it on the surface of the negative electrode current collector with a coating thickness of 1 μm. After baking until the solvent evaporates, collect the negative electrode sheet and perform die-cutting (length*width is 51*41mm);
[0066] S4: Assemble the battery to obtain a battery with a designed capacity of 1Ah.
[0067] Example 2
[0068] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0069] The carboxymethyl group in carboxymethyl cellulose is replaced by potassium carboxymethyl.
[0070] Example 3
[0071] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0072] The carboxymethyl group in carboxymethyl cellulose is replaced by sodium carboxymethyl.
[0073] Example 4
[0074] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0075] The coating thickness of the high molecular polymer solution on the surface of the negative electrode current collector is 2 μm.
[0076] Example 5
[0077] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0078] The carboxymethyl group in carboxymethyl cellulose is replaced by carboxymethyl lithium, with a solid content of 1.2% and a degree of substitution of 1.2.
[0079] Example 6
[0080] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0081] The coating thickness of the high molecular polymer solution on the surface of the negative electrode current collector is 3 μm.
[0082] Example 7
[0083] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0084] The carboxymethyl group in carboxymethyl cellulose is replaced by carboxymethyl lithium, with a solid content of 1.2% and a degree of substitution of 1.5.
[0085] Example 8
[0086] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0087] The carboxymethyl group in carboxymethyl cellulose is replaced by carboxymethyl lithium, and the degree of substitution is 0.5.
[0088] Example 9
[0089] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0090] The solid content of the CMC-Li in the high molecular polymer solution is 2%.
[0091] Example 10
[0092] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0093] The solid content of the CMC-Li in the high molecular polymer solution is 4%.
[0094] Embodiment 11
[0095] This embodiment is used to illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0096] The solid content of the CMC-Li in the high molecular polymer solution is 1%.
[0097] Comparative Example 1
[0098] This comparative example is used to compare and illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0099] The surface of the negative electrode current collector is not coated with the polymer coating described in the present application.
[0100] Comparative Example 2
[0101] This comparative example is used to compare and illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0102] The surface of the negative electrode current collector is coated with a PVDF polymer coating.
[0103] Comparative Example 3
[0104] This comparative example is used to compare and illustrate a negative electrode sheet of a lithium metal battery without a negative electrode and a lithium ion battery disclosed in the present invention, and includes most of the operations in Example 1, except that:
[0105] The solid content of the CMC-Li in the high molecular polymer solution is 4.5%.
[0106] Performance Testing
[0107] The following performance tests were performed on Examples 1 to 11 and Comparative Examples 1 to 3 prepared as above:
[0108] Battery room temperature cycle test
[0109] Test method: Place the battery in an environment of 25±2 degrees and perform a standard charge and discharge cycle at a cycle rate of
[0110] 0.1C, charging voltage 4.4V, calculate the capacity retention rate of the battery after the cycle. The calculation formula is as follows:
[0111] The nth cycle capacity retention rate (%) = (nth cycle discharge capacity) / (first cycle discharge capacity)*100%.
[0112] The negative electrode sheets prepared in Example 1 and Comparative Example 1 were observed by microscopic morphology. Figures 1-2 .
[0113] Depend on Figures 1-2 From the results of scanning electron microscopy observations, it can be seen that the carboxymethyl cellulose salt in the polymer coating is relatively uniform, which can guide the uniform deposition of lithium, making the deposition of lithium on the negative electrode collector modified with the carboxymethyl cellulose salt more flat and smooth. The surface of the negative electrode collector prepared in Comparative Example 1 is relatively rough, and the subsequent lithium deposits show obvious dendritic morphology.
[0114] The test results obtained are entered in Table 1.
[0115] Table 1
[0116]
[0117] It can be seen from the test results in Table 1 that the cycle capacity retention rates of the lithium ion batteries prepared in Examples 1 to 11 are better than those in Comparative Examples 1 to 2; among the test results of Examples 1 to 11, the test results of Examples 1, 4 and 9 are relatively better, because, in Example 1, when preparing the negative electrode sheet, the coating thickness of the polymer coating is 1 μm, the degree of substitution is 0.8, and the solid content of the polymer in the polymer solution is 1.2%; in Example 4, when preparing the negative electrode sheet, the coating thickness of the polymer coating is 2 μm, the degree of substitution is 0.8, and in Example 9, when preparing the negative electrode sheet, the coating thickness of the polymer coating is 1 μm, the degree of substitution is 0.8, and the solid content of the polymer in the polymer solution is 2%. Compared with other embodiments, the polymer in the negative electrode sheet prepared in this application selects the coating thickness, degree of substitution, and solid content of the polymer in the polymer solution of Examples 1, 4 and 9, which is more conducive to promoting the migration speed of ions, improving ionic conductivity, stabilizing the negative electrode interface, and promoting the uniform deposition of lithium ions, thereby improving the electrochemical performance of the lithium ion battery;
[0118] Among the test results of Examples 1 to 3, the test result of Example 2 is the worst, followed by Example 3. The reason is that after the carboxymethyl group in the carboxymethyl cellulose is replaced by potassium carboxymethyl, the performance of Example 2 in terms of uniform lithium metal deposition and dendrite control is not as good as that of CMC-Li. In Example 3, the carboxymethyl group in the carboxymethyl cellulose is replaced by sodium carboxymethyl, and the binding energy between CMC-Na and Li is larger. The ion migration number during Li transmission is smaller than that of CMC-Li. Therefore, the performance of CMC-Na is slightly worse than that of CMC-Li. The test results of Examples 1 to 3 show that different ion substitutions affect the electrical properties of the polymer coating.
[0119] Compared with Example 1, the test results of Example 5 and Example 7-8 are lower than those of Example 1. The reason is that the degrees of substitution of Example 5 and Example 7 are higher than those of Example 1, and the degree of substitution of Example 8 is lower than that of Example 1. Compared with Example 5, the cycle performance of Example 7 is slightly lower than that of Example 5 because the degree of substitution of carboxymethyl cellulose salt in Example 7 is 1.5, which is slightly higher than that of Example 5. In the overall cycle performance test, it is not as good as that of Example 5. Since the intermolecular hydrogen bonds of the carboxymethyl cellulose salt with a high degree of substitution are reduced, the crosslinking is weakened, and the viscosity is reduced, it is not conducive to the uniformity of the coating, and the current collector foil exposure phenomenon is prone to occur. The more hydrogen bonds between carboxymethyl cellulose salt molecules, the stronger the molecular cross-linking effect, and the excessive viscosity leads to the problem of easy shrinkage of the coating after coating, that is, too high or too low substitution of carboxymethyl cellulose salt is not conducive to the optimization and improvement of the electrical performance of lithium-ion batteries. When the substitution degree of the carboxymethyl cellulose salt is 0.8 to 1.2 within the limit range of this application, it is beneficial to improve the cycle performance of lithium-ion batteries; compared with Example 1 and Example 4, the test result of Example 6 is lower than that of Example 1 and Example 4. The reason is that the thickness of the polymer coating of Example 6 is relatively thick, which affects the migration speed of lithium ions and easily causes the problem of increased polarization, which is not conducive to the improvement of battery cycle performance;
[0120] Compared with Example 1, Example 10 and Comparative Example 3, the cycle performance of Example 1 is significantly better than that of Example 10 and Comparative Example 3 because the solid content of Example 1 is 1.2%, the solid content of Example 10 is 4%, and the solid content of Comparative Example 3 is 4.5%, that is, too high a solid content is not conducive to the improvement of the cycle performance of the lithium ion battery; in the test results of Example 1, Example 9 and Example 11, the cycle performance of Example 1 is not significantly improved compared with the test results of Example 9, and the cycle performance of Example 1 is better than that of Example 11, wherein the solid content of Example 1 is 1.2%, the solid content of Example 9 is 2%, and the solid content of Example 11 is 1%. It can be seen from the test results that a lower solid content is not conducive to the improvement of the cycle performance of the lithium ion battery, that is, when the solid content of the polymer in the polymer solution described in the present application is between 1.2% and 2%, it is beneficial to improve the battery cycle performance;
[0121] In summary, the polymer coating in the negative electrode sheet of the negative electrode-free lithium metal battery provided by the present invention is used as the artificial SEI film of the negative electrode. The carboxymethyl cellulose salt in the polymer coating has a high ion transfer number, which provides diffusion channels for lithium ions and redistributes the lithium ion flux at the same time, thereby realizing the dense deposition of lithium metal and inhibiting the growth of lithium dendrites. Secondly, the carboxymethyl cellulose salt forms a uniform and dense film layer through hydrogen bond cross-linking, and has a high Young's modulus, which can inhibit the piercing of lithium dendrites. In addition, the swelling rate of the carboxymethyl cellulose salt in the electrolyte is low, which can avoid the reaction of active lithium metal with the electrolyte and reduce the loss of irreversible lithium source in the lithium metal battery, thereby solving the problems of uneven lithium deposition and large volume change in the negative electrode-free lithium metal battery, and can effectively improve the overall electrical performance of the lithium metal battery.
[0122] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A negative electrode sheet for a negative electrode-free lithium metal battery, characterized in that: The invention comprises a negative electrode current collector and a polymer coating, wherein the polymer coating is coated on the surface of the negative electrode current collector, the polymer coating comprises a high molecular polymer, and the high molecular polymer comprises carboxymethyl cellulose salt.
2. The negative electrode sheet of a negative electrode-free lithium metal battery according to claim 1, characterized in that: Taking the total mass of the polymer coating as 100%, the mass percentage of the carboxymethyl cellulose salt is 90% or more.
3. The negative electrode sheet of a negative electrode-free lithium metal battery according to claim 1, characterized in that: The degree of substitution of the carboxymethyl cellulose salt is 0.5 to 1.
5.
4. The negative electrode sheet for a negative electrode-free lithium metal battery according to claim 1, characterized in that: The molecular weight of the high molecular polymer is 20-30W.
5. The negative electrode sheet for a negative electrode-free lithium metal battery according to claim 1, characterized in that: The carboxymethylcellulose salt includes one or more of lithium carboxymethylcellulose, sodium carboxymethylcellulose and potassium carboxymethylcellulose.
6. The negative electrode sheet for a negative electrode-free lithium metal battery according to claim 1, characterized in that: The negative electrode current collector is copper foil.
7. The negative electrode sheet for a negative electrode-free lithium metal battery according to claim 1, characterized in that: The thickness of the polymer coating is 0.5 μm to 3 μm.
8. The negative electrode sheet for a negative electrode-free lithium metal battery according to claim 1, characterized in that: The thickness of the negative electrode current collector is 8 μm to 9 μm.
9. The method for preparing a negative electrode sheet for a negative electrode-free lithium metal battery according to any one of claims 1 to 8, characterized in that: The following operations are included: S1: obtaining a polymer solution containing carboxymethyl cellulose salt; S2: Applying the high molecular polymer solution to the surface of the negative electrode current collector, and after drying, obtaining a negative electrode sheet for a negative electrode-free lithium metal battery.
10. The method for preparing a negative electrode sheet for a negative electrode-free lithium metal battery according to claim 9, characterized in that: The solid content of the high molecular polymer in the high molecular polymer solution is 1.0% to 4%.
11. The method for preparing a negative electrode sheet for a negative electrode-free lithium metal battery according to claim 9, characterized in that: The step S1 comprises: mixing carboxymethyl cellulose salt with a solvent to obtain a high molecular polymer solution containing carboxymethyl cellulose salt, the mixing rate being 600 to 1000 rpm and the mixing time being 30 to 60 min; In S2, the drying time is 12 to 24 hours and the drying temperature is 60 to 80°C.
12. A lithium ion battery, characterized in that: The invention comprises the negative electrode sheet of a negative electrode-free lithium metal battery as described in any one of claims 1 to 11.
Citation Information
Cited By
Interface modification current collector, preparation method and cathode-free lithium metal battery
CN121460590A
Flexible current collector, method for manufacturing the same, and battery
CN122843392A