Low-impedance single-crystal positive electrode material, preparation method thereof, positive plate and lithium ion battery

By covering the first cladding layer of the spinel-shaped structure and the second cladding layer of the fast ion conductor on the positive electrode material of the lithium battery, the problem of degradation of the performance of the lithium battery at low temperatures is solved, and the low under high voltages is achieved Impedance and long cycle life, suitable for power lithium batteries for new energy vehicles.

CN119069671APending Publication Date: 2024-12-03TIANJIN B&M SCI & TECH LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411190261.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The performance of lithium batteries deteriorates under low temperature conditions. The accumulation of structural stress of traditional secondary particle materials leads to capacity attenuation and increase impedance, which is difficult to meet the low-temperature working requirements of new energy vehicles for powered lithium batteries.

Method used

Using low-impedance single crystal positive electrode material, the structure and thermal stability of the material are improved by covering the first and second cladding layers with different functions, reducing interface side reactions, improving interface impedance, and increasing capacity at high voltages. and cycle performance.

Benefits of technology

It achieves low impedance, long cycle life and low DCR growth rate of lithium-ion batteries at high voltages of 4.35V and 4.40V, and is suitable for normal temperature and low temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069671A_ABST
    Figure CN119069671A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion battery positive electrode materials, in particular to a low-impedance single-crystal positive electrode material, a preparation method thereof, a positive electrode plate and a lithium ion battery. The low-impedance single-crystal positive electrode material comprises a base material, a first coating layer and a second coating layer, wherein the first coating layer and the second coating layer sequentially coat the surface of the base material; the chemical formula of the base material is Li < 1 + a > Ni < x > Co < y > Mn < z > A < w > O < 2 >, and A comprises at least one of Zr, Al, Ti, Sr, W, Mg and La elements; the first coating layer comprises a compound with a spinel type structure and comprises Co element and / or Mn element; the second coating layer comprises a fast ion conductor coating layer and comprises at least one of W, Ta, Mo, Al, Zr, Sr, Nb, B, Ca, Mg, La and Ti elements. The positive electrode material can reduce generation of interface side reactions, improve interface impedance, improve capacity and cycle performance under high voltage, and reduce normal temperature and low temperature DCR.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a low-impedance single crystal positive electrode material and a preparation method thereof, a positive electrode sheet and a lithium ion battery. Background Art

[0002] As global carbon emission regulation is strengthened, the demand for new energy vehicles will grow steadily. In recent years, as electric vehicles have been promoted and applied in cold regions, higher requirements have been placed on the low-temperature performance of the power lithium batteries used in them: power lithium batteries are required to be able to work normally under ultra-low temperature conditions of ≤0℃ or even -30℃ to -40℃. However, the performance of lithium batteries is greatly affected by the ambient temperature. Under low-temperature conditions, the internal chemical reaction rate of lithium batteries slows down, the polarization strength is high, the migration of electrons and lithium ions becomes more difficult, and the impedance increases.

[0003] Traditional secondary particle materials are polycrystalline materials containing countless grain boundaries. During the lithium ion deintercalation process, particles are prone to anisotropic expansion and contraction, resulting in structural stress accumulation and layered structure collapse, which leads to rapid capacity decay and a sharp deterioration in DCR (direct current resistance). Combined with the high voltage requirements for ternary single crystal materials, the phase change of the positive electrode material is more serious under high voltage conditions, and the surface interface stability is worse.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The first purpose of the present invention is to provide a low-impedance single-crystal positive electrode material, which has a single-crystal morphology with dispersed particles and fewer grain boundaries. By coating a first coating layer and a second coating layer with different functions, the structure and thermal stability of the material can be improved, the occurrence of interface side reactions can be reduced, the interface impedance can be improved, the capacity and cycle performance under high voltage can be improved, and the DCR at room temperature and low temperature can be reduced.

[0006] The second object of the present invention is to provide a method for preparing a low-impedance single-crystal positive electrode material, which has simple operation, short process and is suitable for mass production.

[0007] The third object of the present invention is to provide a positive electrode sheet, the battery made of the positive electrode sheet has low impedance, high capacity, high initial efficiency and excellent cycle performance.

[0008] The fourth object of the present invention is to provide a lithium ion battery that can operate at high voltages of 4.35V and 4.40V and has the advantages of good capacity and cycle performance, low impedance at room temperature and low temperature, etc.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] The present invention firstly provides a low-impedance single crystal positive electrode material, comprising a base material, and a first coating layer and a second coating layer sequentially coated on the surface of the base material.

[0011] The chemical formula of the matrix material is Li 1+a Ni x Co y Mn z A w O2, wherein 0≤a≤0.1, 0.5≤x≤0.8, 0.05≤y≤0.15, 0.05≤z≤0.4, 0≤w≤0.1, x+y+z+w=1, and A includes at least one of Zr, Al, Ti, Sr, W, Mg and La elements.

[0012] The first coating layer includes a compound having a spinel structure, and the first coating layer includes Co element and / or Mn element.

[0013] The second coating layer includes a fast ion conductor coating layer, and the fast ion conductor coating layer includes at least one of W, Ta, Mo, Al, Zr, Sr, Nb, B, Ca, Mg, La and Ti elements.

[0014] Furthermore, the battery containing the low-impedance single crystal positive electrode material has an initial discharge capacity of ≥197 mAh / g at a voltage of 2.8 to 4.35 V and a discharge capacity of 0.1 C.

[0015] Furthermore, the battery containing the low-impedance single crystal positive electrode material has a first coulombic efficiency of ≥90% at a voltage of 2.8 to 4.35 V and a 0.1C voltage.

[0016] Furthermore, the battery containing the low-impedance single crystal positive electrode material has an initial discharge capacity of ≥202 mAh / g at a voltage of 2.8 to 4.40 V and a discharge capacity of 0.1 C.

[0017] Furthermore, the battery containing the low-impedance single crystal positive electrode material has a first coulombic efficiency of ≥90% at a voltage of 2.8 to 4.40 V and a 0.1C voltage.

[0018] Furthermore, the DC impedance of a battery containing the low-impedance single crystal positive electrode material at SOC50 is ≤20Ω at 25°C.

[0019] Furthermore, the battery containing the low-impedance single crystal positive electrode material has a DC impedance of ≤25Ω at SOC20 at 25°C.

[0020] Furthermore, the DC impedance of a battery containing the low-impedance single crystal positive electrode material at SOC50 is ≤150Ω at -10°C.

[0021] Furthermore, the DC impedance of a battery containing the low-impedance single crystal positive electrode material at SOC20 is ≤270Ω at -10°C.

[0022] Furthermore, the capacity retention rate of a battery containing the low-impedance single crystal positive electrode material after 50 cycles at a voltage of 3.0 to 4.50 V is ≥94%.

[0023] Furthermore, the DC impedance growth rate of a battery containing the low-impedance single crystal positive electrode material when cycled for 50 cycles at a voltage of 3.0 to 4.50 V is ≤85%.

[0024] Furthermore, the first coating layer includes lithium cobalt oxide and / or lithium manganese oxide.

[0025] The present invention further provides a method for preparing the low-impedance single crystal positive electrode material, comprising the following steps:

[0026] A mixed material containing a nickel-cobalt-manganese precursor and a lithium source is sintered to obtain lithium nickel-cobalt-manganese oxide; optionally, the mixed material also includes a dopant containing A, wherein A includes at least one of Zr, Al, Ti, Sr, W, Mg and La elements.

[0027] The lithium nickel cobalt manganese oxide, the first coating agent and the second coating agent are mixed and calcined to obtain the low-impedance single crystal positive electrode material; wherein the first coating agent includes a cobalt-containing compound and / or a manganese-containing compound; and the second coating agent includes a compound of at least one element selected from the group consisting of W, Ta, Mo, Al, Zr, Sr, Nb, B, Ca, Mg, La and Ti.

[0028] Furthermore, the molar ratio of the nickel-cobalt-manganese precursor to the lithium element in the lithium source is 1:1.01-1.06.

[0029] Furthermore, the mass of the A-containing dopant accounts for 0.2% to 1.0% of the mass of the nickel-cobalt-manganese precursor.

[0030] Furthermore, the chemical formula of the nickel-cobalt-manganese precursor is Ni a Co b Mn c (OH)2, wherein 0.5≤a≤0.8, 0.05≤b≤0.15, 0.05≤c≤0.4, a+b+c=1.

[0031] Furthermore, the sintering includes four-step sintering, and the four-step sintering specifically includes: first keeping warm at 400-600°C for 2-4h, then keeping warm at 700-800°C for 2-4h, then keeping warm at 850-1000°C for 6-10h, and finally keeping warm at 600-700°C for 3-4h.

[0032] Furthermore, before the mixing of the lithium nickel cobalt manganese oxide, the first coating agent and the second coating agent and calcining, the process further includes crushing the lithium nickel cobalt manganese oxide to a volume median particle size of 3 to 5 μm.

[0033] Furthermore, the mass of the first coating agent accounts for 0.5% to 4.0% of the mass of the lithium nickel cobalt manganese oxide.

[0034] Furthermore, the mass of the second coating agent accounts for 0.4% to 1.5% of the mass of the lithium nickel cobalt manganese oxide.

[0035] Furthermore, the calcination temperature is 600-800° C., and / or the calcination holding time is 4-8 hours.

[0036] The present invention further provides a positive electrode sheet, comprising the low-impedance single-crystal positive electrode material, or the low-impedance single-crystal positive electrode material prepared according to the preparation method of the low-impedance single-crystal positive electrode material.

[0037] The present invention also provides a lithium ion battery, comprising the positive electrode sheet.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) The low-impedance single crystal positive electrode material provided by the present invention has a high first discharge capacity at 4.35V and 4.4V, low impedance at room temperature and low temperature, long cycle life, and low DCR growth.

[0040] (2) The low-impedance single-crystal positive electrode material provided by the present invention has a first coating layer with a spinel structure, which can reduce the Ni content on the surface of the material, improve the surface and interface stability of the material, reduce the interface impedance, and improve the capacity and rate performance. The second coating layer introduces a fast ion conductor for coating, constructs a grid-like nano-coating structure with highly active and inert elements interlaced, and increases the coating uniformity. It can not only improve the ionic and electronic conductivity and reduce the interface impedance, but also reduce the side reactions between the material and the electrolyte during the cycle, improve the interface stability of the material, improve the cycle performance, and inhibit gas production. At the same time, the coating layer can also prevent the release of oxygen to a certain extent, retain lithium and oxygen vacancies, and thus stabilize the original layered structure of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0042] Figure 1 The XRD diagram of the low-impedance single crystal positive electrode material prepared in Example 1 provided by the present invention;

[0043] Figure 2 This is a SEM image of the low-impedance single crystal positive electrode material prepared in Example 1 provided by the present invention;

[0044] Figure 3 This is a SEM image of the low-impedance single crystal positive electrode material prepared in Example 2 provided by the present invention;

[0045] Figure 4 This is a SEM image of the low-impedance single crystal positive electrode material obtained in Example 3 provided by the present invention;

[0046] Figure 5 This is a SEM image of the low-impedance single crystal positive electrode material obtained in Example 4 provided by the present invention;

[0047] Figure 6 This is a SEM image of the low-impedance single crystal positive electrode material obtained in Example 5 provided by the present invention;

[0048] Figure 7 This is a SEM image of the low-impedance single crystal positive electrode material obtained in Example 6 provided by the present invention;

[0049] Figure 8 This is a SEM image of the low-impedance single crystal positive electrode material obtained in Example 7 provided by the present invention;

[0050] Fig. 9 This is a SEM image of the low-impedance single crystal positive electrode material obtained in Example 8 provided by the present invention;

[0051] Fig.10 This is a SEM image of the low-impedance single crystal positive electrode material obtained in Example 9 provided by the present invention;

[0052] Fig.11 This is a SEM image of the low-impedance single crystal positive electrode material obtained in Example 17 provided by the present invention;

[0053] Fig.12 This is a SEM image of the positive electrode material prepared in Comparative Example 1 provided by the present invention;

[0054] Fig.13 This is a comparison chart of δDCR of batteries assembled with the low-impedance single crystal positive electrode materials of Examples 1 to 5 provided by the present invention and batteries assembled with the positive electrode materials of Comparative Example 1 after 50 cycles. DETAILED DESCRIPTION

[0055] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0056] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0057] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0058] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0059] In the first aspect, the present invention provides a high voltage, low impedance single crystal positive electrode material, which includes a base material, and a first coating layer and a second coating layer sequentially coated on the surface of the base material. That is, the present invention adopts double-layer coating. Among them, the first coating layer is an intermediate layer, which is arranged between the base material and the second coating layer. The second coating layer is the outermost layer. A gradient coating effect is formed.

[0060] The chemical formula of the matrix material is Li 1+a Ni x Co y Mn z A wO2, wherein 0≤a≤0.1, 0.5≤x≤0.8, 0.05≤y≤0.15, 0.05≤z≤0.4, 0≤w≤0.1, x+y+z+w=1. Wherein, a includes but is not limited to any point value of 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or any range value between two of them. x includes but is not limited to any point value of 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8 or any range value between two of them. y includes but is not limited to any point value of 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15 or any range value between two of them. z includes but is not limited to any point value of 0.05, 0.07, 0.08, 0.1, 0.12, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4 or any range value between two of them. w includes but is not limited to any point value of 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or any range value between two of them. A is a doping element, and doping A can further improve the electrochemical properties of the material. A includes at least one of Zr, Al, Ti, Sr, W, Mg and La elements, and two, three, four, five or more elements can also be selected.

[0061] The above-mentioned base material is layered nickel-cobalt-manganese lithium oxide, which has good safety performance and high energy density. There is a synergistic effect between the base material and the coating layer, which is beneficial to improving the electrochemical performance of the positive electrode material.

[0062] The first coating layer includes a compound having a spinel structure, and the first coating layer includes Co element and / or Mn element.

[0063] The second coating layer includes a fast ion conductor coating layer, and the fast ion conductor coating layer includes at least one of W, Ta, Mo, Al, Zr, Sr, Nb, B, Ca, Mg, La and Ti elements, for example, two, three, four, five or more. That is, the second coating layer includes a fast ion conductor formed by at least one element of W, Ta, Mo, Al, Zr, Sr, Nb, B, Ca, Mg, La and Ti.

[0064] The battery assembled with the low-impedance single crystal positive electrode material provided by the present invention has high first discharge capacity at voltages of 4.35V and 4.4V, low impedance at room temperature and low temperature, long cycle life, and low DCR growth.

[0065] Specifically, the first coating layer including Co and / or Mn elements has a spinel structure, which can reduce the Ni content on the surface of the material, improve the surface and interface stability of the material, reduce the interface impedance, and improve the capacity and rate performance. The second coating layer introduces a fast ion conductor for coating, constructs a grid-like nano-coating structure in which highly active and inert elements are interlaced (the highly active elements and inert elements in the second coating layer are relative), increases the coating uniformity, improves the ion and electronic conductivity, reduces the interface impedance, and reduces the side reactions of the material with the electrolyte during the cycle, improves the interface stability of the material, improves the cycle performance, and inhibits gas production. At the same time, the coating layer can also prevent the release of oxygen to a certain extent, retain lithium and oxygen vacancies, and thus stabilize the original layered structure of the material.

[0066] In some specific embodiments, the compound having a spinel structure includes at least one of lithium cobalt oxide and lithium manganese oxide.

[0067] In some specific embodiments, the battery containing the low-impedance single crystal positive electrode material has an initial discharge capacity of ≥197 mAh / g at a voltage of 2.8 to 4.35 V and 0.1 C, including but not limited to any point value of 197 mAh / g, 198 mAh / g, 199 mAh / g, 200 mAh / g, 201 mAh / g, 202 mAh / g, 203 mAh / g, 204 mAh / g, 205 mAh / g, 210 mAh / g or a range value between any two of them.

[0068] In some specific embodiments, the first coulombic efficiency of a battery containing the low-impedance single crystal positive electrode material at a voltage of 2.8 to 4.35 V and 0.1 C is ≥90%, including but not limited to any point value of 90%, 90.5%, 91%, 91.5%, 92%, 93%, 94%, 95% or a range value between any two of them.

[0069] In some specific embodiments, the battery containing the low-impedance single crystal positive electrode material has an initial discharge capacity of ≥202 mAh / g at a voltage of 2.8 to 4.40 V and 0.1 C, including but not limited to any point value of 202 mAh / g, 203 mAh / g, 204 mAh / g, 205 mAh / g, 206 mAh / g, 207 mAh / g, 208 mAh / g, and 210 mAh / g, or a range value between any two of them.

[0070] In some specific embodiments, the first coulombic efficiency of a battery containing the low-impedance single crystal positive electrode material at a voltage of 2.8 to 4.40 V and 0.1 C is ≥90%, including but not limited to any point value of 90%, 90.5%, 91%, 91.5%, 92%, 93%, 94%, 95% or a range value between any two of them.

[0071] In some specific embodiments, the DC impedance of the battery containing the low-impedance single crystal positive electrode material at 25°C is ≤20Ω at SOC50, including but not limited to any point value of 20Ω, 19Ω, 18Ω, 17Ω, 16Ω, 15Ω, 14Ω, 13Ω, 12Ω, 11Ω, 10Ω or any range value between two of them. Among them, SOC50 means that half of the power of the lithium battery has been used, that is, the remaining power of the lithium battery is 50%.

[0072] In some specific embodiments, the DC impedance of the battery containing the low-impedance single crystal positive electrode material at 25°C SOC20 is ≤25Ω, including but not limited to any point value of 23Ω, 21Ω, 20Ω, 19Ω, 18Ω, 17Ω, 16Ω, 15Ω, 14Ω, 13Ω, 12Ω, 11Ω, 10Ω or any range value between two of them. Among them, SOC20 means that 80% of the power of the lithium battery has been used, that is, the remaining power of the lithium battery is 20%.

[0073] In some specific embodiments, the DC impedance of a battery containing the low-impedance single crystal positive electrode material at SOC50 at -10°C is ≤150Ω, including but not limited to any point value of 150Ω, 145Ω, 140Ω, 135Ω, 130Ω, 125Ω, 120Ω, 110Ω, 100Ω or a range value between any two of them.

[0074] In some specific embodiments, the DC impedance of a battery containing the low-impedance single crystal positive electrode material at -10°C SOC20 is ≤270Ω, including but not limited to any point value of 270Ω, 260Ω, 250Ω, 240Ω, 235Ω, 230Ω, 220Ω, 210Ω, 200Ω or a range value between any two of them.

[0075] In some specific embodiments, the capacity retention rate of a battery containing the low-impedance single crystal positive electrode material after 50 cycles at a voltage of 3.0 to 4.50 V is ≥ 94%, including but not limited to any point value of 94%, 94.5%, 95%, 95.5%, 96%, 97%, 98%, 99% or a range value between any two of them.

[0076] In some specific embodiments, the DC impedance growth rate of a battery containing the low-impedance single crystal positive electrode material after 50 cycles at a voltage of 3.0 to 4.50 V is ≤85%, including but not limited to any point value of 85%, 80%, 75%, 70%, 65%, 60%, 55%, 50%, 40%, 30% or a range value between any two of them.

[0077] The lithium ion battery made of the low-impedance single crystal positive electrode material provided by the present invention has high first charge and discharge capacity at high voltage, high first coulomb efficiency, excellent cycle performance, low DC impedance at room temperature and low temperature, and low DC impedance growth rate.

[0078] In some specific embodiments, the first coating layer is lithium cobalt oxide and / or lithium manganese oxide having a spinel structure.

[0079] In some specific embodiments, the mass of the first coating layer accounts for 0.2% to 4.0% of the mass of the base material, including but not limited to any point value of 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4.0% or any range between two values. The mass of the second coating layer accounts for 0.1% to 1.5% of the mass of the base material, including but not limited to any point value of 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.3%, 1.5% or any range between two values.

[0080] In a second aspect, the present invention provides a method for preparing the low-impedance single crystal positive electrode material, which specifically comprises the following steps:

[0081] The mixed material containing the nickel-cobalt-manganese precursor and the lithium source is sintered and cooled to obtain lithium nickel-cobalt-manganese oxide, i.e., the matrix material.

[0082] Optionally, the mixed material further includes a dopant containing element A, wherein A includes at least one of elements Zr, Al, Ti, Sr, W, Mg and La. It is understood that the term "optionally" herein means optional or not, that is, the dopant containing A may be added or not.

[0083] That is, the lithium nickel cobalt manganese oxide contains the doping element A or does not contain the doping element A.

[0084] Furthermore, the lithium nickel cobalt manganese oxide, the first coating agent and the second coating agent are mixed and then calcined, and then cooled to obtain the low-impedance single crystal positive electrode material.

[0085] It can be understood that the adaptation temperatures of the first coating agent and the second coating agent are different, which can ensure that the first coating agent is in the middle layer and the second coating agent is in the outermost layer.

[0086] Wherein, the first coating agent includes a cobalt-containing compound and / or a manganese-containing compound, such as cobalt oxide or manganese oxide. At high temperature, the cobalt-containing compound and / or manganese-containing compound reacts with lithium element to generate lithium cobaltate and / or lithium manganate.

[0087] The second coating agent includes a compound of at least one element of W, Ta, Mo, Al, Zr, Sr, Nb, B, Ca, Mg, La and Ti.

[0088] The method for preparing the low-impedance single crystal positive electrode material provided by the present invention is simple to operate, has a short process, and is suitable for mass production. The positive electrode material prepared by the method has excellent electrochemical properties, and the battery assembled by the method has a high first discharge capacity at 4.35V and 4.4V voltages, low impedance at room temperature and low temperature, long cycle life, and low DCR growth.

[0089] In some specific embodiments, the molar ratio of the nickel-cobalt-manganese precursor to the lithium element in the lithium source is 1:1.01-1.06, including but not limited to any point value of 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06 or a range value between any two of them; in the present application, the molar ratio of the nickel-cobalt-manganese precursor to the lithium element in the lithium source refers to the ratio of the total molar number of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese precursor to the molar number of lithium element in the lithium source.

[0090] In some specific embodiments, the mass of the dopant containing A accounts for 0.2% to 1.0% of the mass of the nickel-cobalt-manganese precursor, including but not limited to any point value of 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0% or any range value between two of them. This is conducive to stabilizing the crystal structure, reducing oxygen release, and improving the capacity and cycle performance of the positive electrode material.

[0091] In some specific embodiments, the chemical formula of the nickel-cobalt-manganese precursor is Ni a Co b Mn c(OH)2, wherein 0.5≤a≤0.8, 0.05≤b≤0.15, 0.05≤c≤0.4, a+b+c=1. Wherein, a includes but is not limited to any one of 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8 or any range between them. b includes but is not limited to any one of 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15 or any range between them. c includes but is not limited to any one of 0.05, 0.07, 0.08, 0.1, 0.12, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4 or any range between them.

[0092] In some specific embodiments, the nickel-cobalt-manganese precursor and the lithium source are mixed at high speed, or the nickel-cobalt-manganese precursor, the lithium source and the dopant containing A are mixed at high speed. The speed of the high-speed mixing may be, for example, 800 to 1000 rpm / min, and the time of the high-speed mixing may be, for example, 30 to 50 min, but is not limited thereto.

[0093] In some specific embodiments, the lithium source includes any Li-containing compound commonly used in the art, such as lithium hydroxide, lithium carbonate, lithium acetate, lithium sulfate, etc., but is not limited thereto.

[0094] In some specific embodiments, the sintering includes four-step sintering or four-stage sintering. The four-step sintering specifically includes: first, heat at 400-600°C (including but not limited to any one of 400°C, 450°C, 500°C, 550°C, 600°C or any range between two values) for 2-4h (including but not limited to any one of 2h, 2.5h, 3h, 3.5h, 4h or any range between two values), then heat at 700-800°C (including but not limited to any one of 700°C, 720°C, 750°C, 780°C, 800°C or any range between two values) for 2-4h (including but not limited to any one of 2h, 2.5h, 3h, 3.5h, 4h or any range between two values). The sintering temperature is 400 ° C or 800 ° C, and the sintering temperature is 200 ° C or 200 ° C. The sintering temperature is 400 ° C or 800 ° C. The sintering temperature is 500 ° C or 1000 ° C. The sintering temperature is 500 ° C or 8 ...

[0095] In some specific embodiments, the sintering atmosphere includes air atmosphere and / or oxygen atmosphere.

[0096] In some specific embodiments, before the lithium nickel cobalt manganese oxide, the first coating agent and the second coating agent are mixed and calcined, the lithium nickel cobalt manganese oxide is crushed to a volume median particle size D 50 The step of reducing the particle size to 3-5 μm (e.g., 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm) is advantageous in improving the uniformity of the coating. The pulverizing device may be a jet mill to achieve the purpose of particle dispersion.

[0097] In some specific embodiments, the mass of the first coating agent accounts for 0.5% to 4.0% of the mass of the lithium nickel cobalt manganese oxide, including but not limited to any point value of 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4.0% or any range value between two of them.

[0098] In some specific embodiments, the cobalt-containing compound includes but is not limited to at least one of Co3O4, Co(OH)2, and CoSO4·7H2O.

[0099] In some specific embodiments, the manganese-containing compound includes but is not limited to at least one of MnO, MnO2, Mn(OH)2, and MnSO4.

[0100] In some specific embodiments, the mass of the second coating agent accounts for 0.4% to 1.5% of the mass of the lithium nickel cobalt manganese oxide, including but not limited to any point value of 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.3%, 1.5% or any range value between two of them.

[0101] In some specific embodiments, the first coating agent is a nano-scale material. And / or the second coating agent is a nano-scale material. This can improve the uniformity of coating.

[0102] In some specific embodiments, the calcination temperature is 600-800°C, including but not limited to any point value of 600°C, 630°C, 650°C, 670°C, 700°C, 730°C, 750°C, 780°C, 800°C or a range between any two of them.

[0103] In some specific embodiments, the calcination holding time is 4 to 8 hours, including but not limited to any one of 4 hours, 5 hours, 6 hours, 7 hours, and 8 hours, or a range between any two of them.

[0104] In some specific embodiments, the heating rate of the calcination is 1 to 3°C / min, for example, 1.5°C / min, 2°C / min or 2.5°C / min.

[0105] In some specific embodiments, the calcining atmosphere includes air atmosphere and / or oxygen atmosphere.

[0106] In some specific embodiments, during the mixing of the lithium nickel cobalt manganese oxide, the first coating agent and the second coating agent, high-speed mixing is performed at a rotation speed of 1000 to 1500 rpm / min, and the mixing time may be 20 to 40 minutes, but is not limited thereto.

[0107] In a third aspect, the present invention provides a positive electrode sheet, comprising the low-impedance single-crystal positive electrode material, or the low-impedance single-crystal positive electrode material prepared by the method for preparing the low-impedance single-crystal positive electrode material.

[0108] The battery made of the positive electrode sheet has low impedance, high capacity, high initial efficiency and excellent cycle performance.

[0109] Optionally, the positive electrode sheet further includes a binder and a conductive agent, which is not limited in the present invention.

[0110] In a fourth aspect, the present invention provides a lithium-ion battery, comprising the positive electrode sheet.

[0111] The low-impedance single crystal positive electrode material provided by the present invention can be widely used in various lithium-ion batteries, has a wide application range, and is particularly suitable for high-voltage lithium-ion batteries at voltages of 4.35V and 4.4V.

[0112] The lithium ion battery provided by the present invention has the advantages of low impedance at room temperature and low temperature, good capacity and cycle performance at high voltage, etc.

[0113] Optionally, the lithium-ion battery further includes a negative electrode sheet, a separator and an electrolyte, which is not limited in the present invention.

[0114] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0115] Example 1

[0116] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment comprises the following steps:

[0117] (1) Nickel cobalt manganese hydroxide precursor Ni 0.63 Co 0.05 Mn 0.32 (OH)2, lithium carbonate, dopant ZrO2 and Al2O3 are mixed at high speed and then sintered in four steps, wherein the molar ratio of lithium element in nickel cobalt manganese hydroxide precursor and lithium carbonate is 1:1.06, the mass of ZrO2 is 0.4% of the mass of nickel cobalt manganese hydroxide precursor, and the mass of Al2O3 is 0.2% of the mass of nickel cobalt manganese hydroxide precursor. The four-step sintering method is: in air atmosphere, the first step sintering temperature is 500℃, and the sintering time is 2h; the second step sintering temperature is 700℃, and the sintering time is 2h; the third step sintering temperature is 960℃, and the sintering time is 10h; the fourth step sintering temperature is 700℃, and the sintering time is 3h. After cooling, lithium nickel cobalt manganese oxide Li 1.06 Ni 0.626 Co 0.050 Mn 0.318 Zr 0.003 Al 0.003 O2.

[0118] (2) The lithium nickel cobalt manganese oxide obtained in step (1) is dispersed by a jet mill to obtain a volume median particle size D 50=4 μm powder. (3) The pulverized lithium nickel cobalt manganese oxide powder obtained in step (2) is mixed with the first coating agent nano Co3O4, the second coating agent nano WO3 and nano Al2O3 in a high-speed solid phase, wherein the mass of nano Co3O4 is 0.5% of the mass of the lithium nickel cobalt manganese oxide powder, the mass of nano WO3 is 0.2% of the mass of the lithium nickel cobalt manganese oxide powder, and the mass of nano Al2O3 is 0.3% of the mass of the lithium nickel cobalt manganese oxide powder. The mixed materials are calcined at 750° C. in an air atmosphere for 6 hours, and after cooling, a high voltage, low impedance single crystal positive electrode material is obtained.

[0119] The low-impedance single-crystal positive electrode material prepared in this embodiment includes a base material and a first coating layer and a second coating layer sequentially coated on the surface of the base material. The first coating layer is lithium cobalt oxide with a spinel structure, and the second coating layer is WO3 and Al2O3.

[0120] Example 2

[0121] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass of nano-Co3O4 is 1.0% of the mass of the lithium nickel cobalt manganese oxide powder.

[0122] Example 3

[0123] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass of nano-Co3O4 is 2.0% of the mass of the lithium nickel cobalt manganese oxide powder.

[0124] Example 4

[0125] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass of nano-Co3O4 is 3.0% of the mass of the lithium nickel cobalt manganese oxide powder.

[0126] Example 5

[0127] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass of nano-Co3O4 is 4.0% of the mass of the lithium nickel cobalt manganese oxide powder.

[0128] Example 6

[0129] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 4, except that in step (3), the mass of the nano-WO3 is 0.3% of the mass of the lithium nickel cobalt manganese oxide powder.

[0130] Example 7

[0131] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 4, except that in step (3), the mass of the nano-WO3 is 0.35% of the mass of the lithium nickel cobalt manganese oxide powder.

[0132] Example 8

[0133] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 4, except that in step (3), the mass of nano-WO3 is 0.40% of the mass of the lithium nickel cobalt manganese oxide powder.

[0134] Example 9

[0135] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 4, except that in step (3), the mass of the nano-WO3 is 0.50% of the mass of the lithium nickel cobalt manganese oxide powder.

[0136] Example 10

[0137] The preparation method of the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in embodiment 7, except that in step (3), nano Co3O4 is replaced with an equal mass of nano MnO2. The first coating layer in the low-impedance single crystal positive electrode material prepared in this embodiment is lithium manganate with a spinel structure.

[0138] Embodiment 11

[0139] The preparation method of the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in embodiment 7, except that: in step (3), nano WO3 is replaced by nano MoO3, and nano Al2O3 is replaced by nano ZrO2, wherein the mass of nano MoO3 is 0.4% of the mass of lithium nickel cobalt manganese oxide powder, and the mass of nano ZrO2 is 0.4% of the mass of lithium nickel cobalt manganese oxide powder. The second coating layer in the low-impedance single crystal positive electrode material prepared in this embodiment is MoO3 and ZrO2.

[0140] Example 12

[0141] The preparation method of the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in embodiment 7, except that: in step (3), nano WO3 is replaced by nano SrO, and nano Al2O3 is replaced by nano CaO, wherein the mass of nano SrO is 0.5% of the mass of lithium nickel cobalt manganese oxide powder, and the mass of nano CaO is 0.5% of the mass of lithium nickel cobalt manganese oxide powder. The second coating layer in the low-impedance single crystal positive electrode material prepared in this embodiment is SrO and CaO.

[0142] Embodiment 13

[0143] The preparation method of the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in embodiment 7, except that: in step (3), nano WO3 and nano Al2O3 are replaced by nano Ta2O5, nano B2O3, nano Nb2O5 and nano TiO2, wherein the mass of nano Ta2O5 is 0.1% of the mass of lithium nickel cobalt manganese oxide powder, the mass of nano B2O3 is 0.2% of the mass of lithium nickel cobalt manganese oxide powder, the mass of nano Nb2O5 is 0.5% of the mass of lithium nickel cobalt manganese oxide powder, and the mass of nano TiO2 is 0.3% of the mass of lithium nickel cobalt manganese oxide powder. The second coating layer in the low-impedance single crystal positive electrode material prepared in this embodiment is Ta2O5, B2O3, Nb2O5 and TiO2.

[0144] Embodiment 14

[0145] The preparation method of the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in embodiment 7, except that in step (1), ZrO2 is replaced by an equal mass of SrO, and Al2O3 is replaced by an equal mass of La2O3. After cooling, lithium nickel cobalt manganese oxide Li 1.06 Ni 0.626 Co 0.050 Mn 0.318 Sr 0.003 La 0.003 O2.

[0146] Embodiment 15

[0147] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in embodiment 7, except that: in step (1), Ni 0.63 Co 0.05 Mn 0.32 (OH)2 replaced by Ni 0.70 Co 0.15 Mn 0.15 (OH)2. After cooling, lithium nickel cobalt manganese oxide Li 1.06 Ni 0.695 Co 0.149 Mn 0.149 Zr 0.004 Al 0.003 O2.

[0148] Example 16

[0149] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment comprises the following steps:

[0150] (1) Nickel cobalt manganese hydroxide precursor Ni 0.63 Co 0.05 Mn 0.32(OH)2 and lithium carbonate are mixed at high speed and then sintered in four steps, wherein the molar ratio of the nickel cobalt manganese hydroxide precursor to the lithium element in the lithium carbonate is 1:1.02, and the four-step sintering method is as follows: in an oxygen atmosphere, the first step is sintered at a temperature of 400°C and a sintering time of 4 hours; the second step is sintered at a temperature of 800°C and a sintering time of 3 hours; the third step is sintered at a temperature of 850°C and a sintering time of 8 hours; the fourth step is sintered at a temperature of 600°C and a sintering time of 4 hours. After cooling, lithium nickel cobalt manganese oxide Li 1.02 Ni 0.63 Co 0.05 Mn 0.32 O2.

[0151] (2) The lithium nickel cobalt manganese oxide obtained in step (1) is dispersed by a jet mill to obtain a volume median particle size D 50 =5μm powder.

[0152] (3) The crushed lithium nickel cobalt manganese oxide powder obtained in step (2) is mixed with the first coating agent nano Co3O4, the second coating agent nano WO3 and nano Al2O3 in a high-speed solid phase, wherein the mass of nano Co3O4 is 0.5% of the mass of the lithium nickel cobalt manganese oxide powder, the mass of nano WO3 is 0.2% of the mass of the lithium nickel cobalt manganese oxide powder, and the mass of nano Al2O3 is 0.3% of the mass of the lithium nickel cobalt manganese oxide powder. The mixed materials are calcined at 650° C. in an air atmosphere for 8 h, and cooled to obtain a high voltage, low impedance single crystal positive electrode material.

[0153] Embodiment 17

[0154] The method for preparing the low-impedance single crystal positive electrode material provided in this embodiment is basically the same as that in Embodiment 6, except that in step (3), no nano WO3 is added, that is, the mass of the second coating agent accounts for 0.3% of the mass of lithium nickel cobalt manganese oxide.

[0155] Comparative Example 1

[0156] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of Example 4, except that in step (3), no nano-Co3O4 is added.

[0157] Comparative Example 2

[0158] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of Example 4, except that in step (3), no nano WO3 and nano Al2O3 are added.

[0159] Experimental example

[0160] The low-impedance single crystal positive electrode material prepared in each embodiment and the positive electrode material prepared in each comparative example are respectively used as active materials, acetylene black is a conductive agent, and PVDF is a binder, and the mixture is mixed at a mass ratio of 90:5:5, and a solvent NMP is added thereto, and the mixture is uniformly mixed to form a slurry, and the slurry is coated on an aluminum foil, and dried in a vacuum drying oven at 70°C for 18 hours. After drying, it is cut into positive electrode sheets with a diameter of 12 mm by a slicer, and button batteries are assembled in a glove box. The electrolyte is 1 mol / L LiPF6 dissolved in EC+DEC (mass ratio is 1:1). After the battery is assembled, it is left to stand for 12 hours, and the battery is charged and discharged for the first time at room temperature 25°C, and the impedance at room temperature 25°C and low temperature -10°C, the cycle performance (45°C) and the DCR growth are tested using a blue electric test system, and the results are shown in Tables 1 and 2. Wherein, DCR is the DC impedance; δDCR is the DC impedance growth rate. Discharge DCR: (I1, t1) = |V0-V1| / I1, where V0 is the sampling voltage at the end of static discharge, V1 is the voltage at the end of discharge, t1 is the discharge duration of 10s, I1 is the discharge current value, I1 = 1~2C. SOC50 and SOC20 are two ways to express the state of charge of lithium batteries, representing the state of 50% and 20% of the battery power remaining, respectively.

[0161] Table 1 First charge and discharge capacity and first coulombic efficiency at different voltages

[0162]

[0163]

[0164] Table 2 DCR, δDCR and capacity retention rate at different temperatures

[0165]

[0166] As can be seen from Tables 1 and 2, the high voltage, low impedance single crystal positive electrode materials prepared in Examples 1 to 5 have significantly improved capacity, room temperature impedance, low temperature impedance, cycle retention rate and DCR growth rate at voltages of 4.35V and 4.40V compared to the positive electrode materials prepared in Comparative Example 1, and are all better than Comparative Example 1. In Examples 1 to 5, as the Co coating amount increases, the surface Ni content decreases, the Co content increases, the surface stability improves, the capacity first increases and then decreases, and the room temperature, low temperature impedance and cycle performance gradually improve, wherein when the Co3O4 coating amount is 3%, the comprehensive performance is better.

[0167] Similarly, the high voltage, low impedance single crystal positive electrode materials prepared in Examples 1 to 5 have significantly improved capacity, room temperature impedance, low temperature impedance, cycle retention rate and DCR growth rate at 4.35V and 4.40V compared to the positive electrode materials prepared in Comparative Example 2. When the WO3 coating amount is 0.35% to 0.4%, the overall performance is better.

[0168] This shows that the first coating layer and the second coating layer in the low-impedance single crystal positive electrode material provided in this embodiment have a synergistic effect. Setting the first coating layer and the second coating layer at the same time can significantly improve the capacity and coulombic efficiency at high voltage, reduce the impedance at room temperature and low temperature, reduce the DCR growth rate, and improve the cycle retention rate. Double-layer coating is indispensable.

[0169] Furthermore, by comparing Example 6 and Example 17, it can be seen that the second coating layer contains only one fast ion conductor and the second coating agent has a low quality, which will lead to a decrease in the overall electrochemical performance, especially a significant increase in δDCR.

[0170] In addition, the XRD pattern of the low impedance single crystal positive electrode material prepared in Example 1 is shown in Figure 1 The SEM image of the low impedance single crystal positive electrode material prepared in Example 1 is shown in Figure 2 The SEM image of the low impedance single crystal positive electrode material prepared in Example 2 is shown in Figure 3 The SEM image of the low impedance single crystal positive electrode material prepared in Example 3 is shown in Figure 4 The SEM image of the low impedance single crystal positive electrode material prepared in Example 4 is shown in Figure 5 The SEM image of the low impedance single crystal positive electrode material prepared in Example 5 is shown in Figure 6 The SEM image of the low impedance single crystal positive electrode material prepared in Example 6 is shown in Figure 7 The SEM image of the low impedance single crystal positive electrode material prepared in Example 7 is shown in Figure 8 The SEM image of the low impedance single crystal positive electrode material prepared in Example 8 is shown in Fig. 9 The SEM image of the low impedance single crystal positive electrode material prepared in Example 9 is shown in Fig.10 The SEM image of the low impedance single crystal positive electrode material prepared in Example 17 is shown in Fig.11 The SEM image of the positive electrode material prepared in Comparative Example 1 is shown in Fig.12 shown.

[0171] The comparison of the δDCR of the battery made of the low impedance single crystal positive electrode material of Examples 1 to 5 after 50 cycles and the δDCR of the battery made of the positive electrode material of Comparative Example 1 after 50 cycles is shown in Fig.13 shown.

[0172] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A low-impedance single crystal positive electrode material, characterized in that: It comprises a base material, and a first coating layer and a second coating layer sequentially coated on the surface of the base material; The chemical formula of the matrix material is Li1+aNi x Co y Mn z A w O2, wherein 0≤a≤0.1, 0.5≤x≤0.8, 0.05≤y≤0.15, 0.05≤z≤0.4, 0≤w≤0.1, x+y+z+w=1, and A includes at least one of Zr, Al, Ti, Sr, W, Mg and La; The first coating layer includes a compound having a spinel structure, and the first coating layer includes Co element and / or Mn element; The second coating layer includes a fast ion conductor coating layer, and the fast ion conductor coating layer includes at least one of W, Ta, Mo, Al, Zr, Sr, Nb, B, Ca, Mg, La and Ti elements.

2. The low-impedance single crystal positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) The battery containing the low-impedance single crystal positive electrode material has an initial discharge capacity of ≥197 mAh / g at 0.1C at a voltage of 2.8 to 4.35 V; (2) The battery containing the low-impedance single crystal positive electrode material has a first coulombic efficiency of ≥90% at a voltage of 2.8 to 4.35 V and a temperature of 0.1 C; (3) The battery containing the low-impedance single crystal positive electrode material has an initial discharge capacity of ≥202 mAh / g at 0.1C at a voltage of 2.8 to 4.40 V; (4) The battery containing the low-impedance single crystal positive electrode material has a first coulombic efficiency of ≥90% at a voltage of 2.8 to 4.40 V and a temperature of 0.1 C; (5) The DC impedance of the battery containing the low-impedance single crystal positive electrode material at SOC50 is ≤20Ω at 25°C; (6) The DC impedance of the battery containing the low-impedance single crystal positive electrode material at SOC20 is ≤25Ω at 25°C; (7) The DC impedance of the battery containing the low-impedance single crystal positive electrode material at SOC50 is ≤150Ω at -10°C; (8) The DC impedance of a battery containing the low-impedance single crystal positive electrode material at SOC20 is ≤270Ω at -10°C; (9) The capacity retention rate of a battery containing the low-impedance single crystal positive electrode material after 50 cycles at a voltage of 3.0 to 4.50 V is ≥ 94%; (10) The DC impedance growth rate of a battery containing the low-impedance single crystal positive electrode material is ≤85% when cycled for 50 cycles at a voltage of 3.0 to 4.50 V; (11) The first coating layer includes lithium cobalt oxide and / or lithium manganese oxide.

3. The method for preparing a low-impedance single crystal positive electrode material according to claim 1 or 2, characterized in that: The steps include: Sintering a mixed material containing a nickel-cobalt-manganese precursor and a lithium source to obtain lithium nickel-cobalt-manganese oxide; optionally, the mixed material further includes a dopant containing A, wherein A includes at least one of Zr, Al, Ti, Sr, W, Mg and La; The lithium nickel cobalt manganese oxide, the first coating agent and the second coating agent are mixed and calcined to obtain the low-impedance single crystal positive electrode material; wherein the first coating agent includes a cobalt-containing compound and / or a manganese-containing compound; and the second coating agent includes a compound of at least one element selected from the group consisting of W, Ta, Mo, Al, Zr, Sr, Nb, B, Ca, Mg, La and Ti.

4. The method for preparing a low-impedance single crystal positive electrode material according to claim 3, characterized in that: At least one of the following conditions is met: (1) The molar ratio of the nickel-cobalt-manganese precursor to the lithium element in the lithium source is 1:1.01-1.06; (2) The mass of the A-containing dopant accounts for 0.2% to 1.0% of the mass of the nickel-cobalt-manganese precursor; (3) The chemical formula of the nickel-cobalt-manganese precursor is Ni a Co b Mn c (OH)2, wherein 0.5≤a≤0.8, 0.05≤b≤0.15, 0.05≤c≤0.4, a+b+c=1.

5. The method for preparing a low-impedance single crystal positive electrode material according to claim 3, characterized in that: The sintering comprises four-step sintering, which specifically comprises: firstly keeping the temperature at 400-600°C for 2-4h, then keeping the temperature at 700-800°C for 2-4h, then keeping the temperature at 850-1000°C for 6-10h, and finally keeping the temperature at 600-700°C for 3-4h.

6. The method for preparing a low-impedance single crystal positive electrode material according to claim 3, characterized in that: The step of mixing the lithium nickel cobalt manganese oxide, the first coating agent and the second coating agent and then calcining the mixture further includes the step of crushing the lithium nickel cobalt manganese oxide to a volume median particle size of 3 to 5 μm.

7. The method for preparing a low-impedance single crystal positive electrode material according to claim 3, characterized in that: At least one of the following conditions is met: (1) The mass of the first coating agent accounts for 0.5% to 4.0% of the mass of the lithium nickel cobalt manganese oxide; (2) The mass of the second coating agent accounts for 0.4% to 1.5% of the mass of the lithium nickel cobalt manganese oxide.

8. The method for preparing a low-impedance single crystal positive electrode material according to claim 3, characterized in that: The calcination temperature is 600-800° C., and / or the calcination holding time is 4-8 hours.

9. A positive electrode sheet, characterized in that: It comprises the low-impedance single-crystal positive electrode material as claimed in any one of claims 1 to 2, or the low-impedance single-crystal positive electrode material prepared by the preparation method of the low-impedance single-crystal positive electrode material as claimed in any one of claims 3 to 8.

10. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 9.

Citation Information

Cited By

  • Lithium cobalt oxide positive electrode material and preparation method and application thereof

    CN121149207A