Polyaniline-zinc single flow battery and system
通过在聚苯胺-锌单液流电池中采用单向循环流动的电解液和多层活性物质层结构,解决了锌离子流失和电池极化问题,提高了电池的能量效率和寿命,简化了结构 And reduce costs.
Patent Information
- Application Number
- CN202411209624.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing dual-ion secondary batteries have severe zinc ions lost during charging and discharging, resulting in a decrease in effective capacity and low energy efficiency. The polarization of the battery is not conducive to the increase of energy density.
Design a polyaniline-zinc single-flow battery, adopting a one-way circulating electrolyte, and by setting a multi-layer active material layer and carbon felt between the positive electrode and the negative electrode, combining suitable lithium salt and zinc salt concentrations, electrolysis is achieved. The unidirectional circulating flow of the liquid reduces zinc ion loss and electrolyte flow resistance.
Improves the battery's energy efficiency and life, reduces internal resistance, simplifies the structure, reduces costs, and enhances safety and reliability.
Smart Images

Figure CN119069760A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery preparation, and in particular relates to a polyaniline-zinc single-liquid flow battery and a system. Background Art
[0002] Polyaniline is a conductive polymer prepared by an oxidative polymerization process and has high electrochemical activity. It can be used as an electrode active material for secondary batteries and supercapacitors. The complete redox process of polyaniline can provide a theoretical specific capacity of 290Ah / Kg, making it an electrode material with high specific capacity. Intrinsic polyaniline (polyaniline base) can undergo redox reactions in an aqueous solution of lithium salt. As a negative electrode material, metallic zinc has the advantages of high specific capacity (820Ah / Kg), low redox potential (-0.76V vsSHE), high electrochemical activity in aqueous electrolytes, large reserves, and low price. It is an aqueous secondary battery negative electrode material with great application potential. Using intrinsic polyaniline as the positive electrode and a zinc metal negative electrode can form an aqueous dual-ion secondary battery with an aqueous solution of lithium salt and zinc salt as the electrolyte. This polyaniline-zinc battery has high energy density, good safety, and a relatively low price. See the positive electrode reaction process. Figure 1 , the reaction process of the negative electrode is shown in Figure 2 .
[0003] The concentration of the electrolyte of a dual-ion secondary battery needs to be controlled within a range that is conducive to the occurrence of a reversible reaction. However, the concentrations of lithium ions and zinc ions in such a dual-ion secondary battery will change significantly during the charge and discharge process, resulting in significant battery polarization, which is not conducive to improving the energy efficiency of the battery. In addition, zinc oxide or zinc hydroxide precipitation is produced at the negative electrode during the charge and discharge process, causing zinc ion loss and reducing the effective capacity. Therefore, how to reasonably design the battery structure to improve its energy efficiency and extend its service life is of great significance to dual-ion secondary batteries. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art dual-ion secondary battery, such as zinc ion loss, reduced effective capacity, and poor battery energy density, thereby providing a polyaniline-zinc single-flow battery and system.
[0005] To this end, the present invention provides the following technical solutions.
[0006] The first aspect of the present invention provides a polyaniline-zinc single-flow battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator; the positive electrode comprises a positive electrode film layer, the positive electrode film layer comprises at least one active material layer, the active material of the active material layer comprises intrinsic polyaniline; the negative electrode comprises a zinc sheet;
[0007] The electrolyte circulates unidirectionally in the polyaniline-zinc single-flow battery.
[0008] The electrolyte circulates unidirectionally from the positive electrode to the negative electrode; or,
[0009] The electrolyte circulates unidirectionally from the negative electrode to the positive electrode.
[0010] In the present invention, the unidirectional circulation flow rate of the electrolyte is related to various factors, such as battery power, electrode state, battery size, etc.; for example, based on the total mass of 1g of the active ingredient polyaniline in all active material layers in the positive electrode, the circulation flow rate of the electrolyte is 0.5ml / min to 10ml / min.
[0011] The electrolyte comprises a lithium salt and a zinc salt;
[0012] Preferably, the concentration of lithium salt in the electrolyte is 1-5M;
[0013] Preferably, the concentration of lithium salt in the electrolyte is 1.5-2.5M;
[0014] Preferably, the concentration of zinc salt in the electrolyte is 0.5-2.5M;
[0015] Preferably, the concentration of zinc salt in the electrolyte is 0.8-1.2M.
[0016] The anions of the lithium salt and the zinc salt are the same;
[0017] Preferably, the anions in the electrolyte include at least one of sulfate ions, nitrate ions, acetate ions, trifluoromethanesulfonate ions, bistrifluoromethanesulfonyl imide ions, tetrafluoroborate ions, chloride ions and bromide ions;
[0018] Preferably, the anions in the electrolyte include at least one of trifluoromethanesulfonate ions, bistrifluoromethanesulfonyl imide ions and chloride ions.
[0019] The positive electrode film layer also includes at least one layer of carbon felt;
[0020] Preferably, the carbon felt is disposed on both sides of the active material layer;
[0021] Preferably, the carbon felt and the active material layer are arranged alternately.
[0022] The loading amount of the active material layer is 0.1-1 g / cm 2 ;
[0023] Preferably, the loading amount of the active material layer is 0.2-0.3 g / cm 2 .
[0024] The positive electrode film layer includes 2-10 layers of active material layers;
[0025] Preferably, the positive electrode film layer includes 4-6 active material layers.
[0026] The thickness of the carbon felt is 0.1-1 mm;
[0027] Preferably, the carbon felt has a thickness of 0.25-0.5 mm.
[0028] It should be noted that the loading amount of the active material layer in the present invention is a single-layer loading amount, which is the unit mass of all components in the active material layer after drying, that is, the dry weight of the active material slurry in the single-layer active material layer; the thickness of the carbon felt is the thickness of the single-layer carbon felt. The active material layer is arranged between two adjacent layers of carbon felt, that is, the upper and lower surfaces of the outermost side of the positive electrode film layer are both carbon felt.
[0029] The active material layer also includes at least one of a lithium salt and a conductive agent;
[0030] Preferably, the lithium salt in the active material layer is the same as the lithium salt in the electrolyte.
[0031] In the active material layer, the mass ratio of the lithium salt to the intrinsic polyaniline is (5-20):100;
[0032] Preferably, the mass ratio of the conductive agent to the intrinsic polyaniline is (2-10):100.
[0033] When preparing the electrode, the active material slurry is coated on the carbon felt; the mass ratio of the solvent to the polyaniline in the active material slurry is (30-100):100. The solvent can be but is not limited to water. The conductive agent is carbon black, carbon nanotubes, conductive graphite, Ketjen black, etc. The amount of solvent added is the conventional amount in the art, and the slurry is formed, and there is no specific limit on the amount of solvent added.
[0034] The preparation method of active material slurry comprises: grinding and mixing polyaniline, lithium salt and conductive agent, adding solvent to obtain slurry.
[0035] The polyaniline-zinc single flow battery satisfies at least one of (1) to (3):
[0036] (1) The positive electrode further includes a positive electrode current collector, which is laminated to the positive electrode film layer;
[0037] (2) The negative electrode further includes a negative electrode current collector, which is arranged in contact with the zinc sheet;
[0038] (3) The polyaniline-zinc single-flow battery further includes a shell, which is disposed outside the positive electrode and the negative electrode; the shell is also provided with an electrolyte inlet and an electrolyte outlet.
[0039] The polyaniline-zinc single flow battery of the present invention is prepared according to conventional methods in the art.
[0040] The diaphragm of the present invention can be any common diaphragm in the art, such as a ceramic membrane, a filter membrane, etc. The present invention does not require the pore size and thickness of the diaphragm; for example, a hydrophilic filter membrane with a pore size of 0.28-0.8 μm is used as the diaphragm, and the material of the filter membrane can be cellulose, glass fiber, nylon, filter paper, etc.
[0041] The electrolyte outlet and electrolyte inlet are determined according to the circulation direction of the electrolyte. Along the flow direction of the electrolyte, the opening where the electrolyte enters the battery is the electrolyte inlet, and the opening where the electrolyte flows out of the battery is the electrolyte outlet.
[0042] The second aspect of the present invention provides a polyaniline-zinc single flow battery system, comprising at least one group of the above-mentioned polyaniline-zinc single flow batteries; and also comprising at least one of (1)-(2):
[0043] (1) a storage tank containing an electrolyte for replenishing the electrolyte for the polyaniline-zinc single-flow battery;
[0044] (2) An electrolyte pump, wherein the electrolyte pump provides power for the unidirectional circulation flow of the electrolyte.
[0045] When the system includes two or more groups of polyaniline-zinc single flow batteries, different batteries can be connected in series and / or in parallel, depending on usage requirements.
[0046] The technical solution of the present invention has the following advantages:
[0047] 1. The polyaniline-zinc single-flow battery provided by the present invention comprises a positive electrode, a negative electrode, an electrolyte and a separator; the positive electrode comprises a positive electrode film layer, the positive electrode film layer comprises at least one active material layer, the active material of the active material layer comprises intrinsic polyaniline; the negative electrode comprises a zinc sheet; the electrolyte circulates unidirectionally in the polyaniline-zinc single-flow battery. The battery of the present invention has the advantages of high energy efficiency and simple structure. Compared with non-flow batteries, the battery of the present invention has a small charge and discharge voltage difference, high energy efficiency, and is convenient for replenishing zinc ions into the system, thereby extending the overall life of the negative electrode and the battery.
[0048] In addition, the battery of the present invention has the advantages of simple structure, good reliability, single pump design, low energy consumption, high system energy efficiency, etc. The battery of the present invention does not require an ion exchange membrane and has low cost.
[0049] 2. The polyaniline-zinc single-liquid flow battery provided by the present invention adopts a neutral electrolyte, which has weak corrosiveness, low toxicity, and good safety, thereby improving the overall safety of the battery.
[0050] 3. The polyaniline-zinc single-liquid flow battery provided by the present invention has a multi-layer design for the positive electrode film layer, which can reduce the flow resistance of the electrolyte, thereby reducing the internal resistance and improving the energy efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0052] Figure 1 It is the chemical reaction formula of the chemical reaction occurring at the positive electrode recorded in the background technology of the present invention;
[0053] Figure 2 is the chemical reaction formula of the chemical reaction occurring at the negative electrode recorded in the background technology of the present invention;
[0054] Figure 3 is a schematic structural diagram of a polyaniline-zinc single flow battery in Example 1 of the present invention;
[0055] Figure 4 is a schematic structural diagram of the positive electrode film layer in Example 1 of the present invention;
[0056] Figure 5 is a schematic structural diagram of a polyaniline-zinc single flow battery system in Example 1 of the present invention;
[0057] Reference numerals:
[0058] 1-positive electrode shell; 2-negative electrode shell; 3-positive electrode current collector; 4-negative electrode current collector; 5-positive electrode film layer; 6-foam zinc; 7-diaphragm; 8-electrolyte; 9-sealing ring; 10-storage tank; 11-electrolyte pump; 12-electrolyte inlet; 13-electrolyte outlet;
[0059] 5-1-active material layer; 5-2-carbon felt. DETAILED DESCRIPTION
[0060] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0061] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0062] Example 1
[0063] This embodiment provides a polyaniline-zinc single flow battery, and its structural schematic diagram is shown in Figure 3 ,include:
[0064] The positive electrode comprises a positive electrode current collector 3 and a positive electrode film layer 5; the positive electrode film layer 5 comprises five active material layers 5-1 and six carbon felt layers 5-2, and the active material layers 5-1 and the carbon felt 5-2 are arranged alternately. The structural schematic diagram is shown in Figure 4 The active material layer includes intrinsic polyaniline, lithium trifluoromethanesulfonate and carbon black in a mass ratio of 10:1.5:0.5; the loading amount of the active material layer on the single-layer carbon felt is 0.2 g / cm 2 The thickness of a single layer of carbon felt is 0.5 mm and the size is 2 cm × 2 cm. The positive electrode current collector 3 is a stainless steel current collector. The preparation method of the positive electrode film layer 5 includes: mixing intrinsic polyaniline, lithium trifluoromethanesulfonate and carbon black in a mass ratio of 10:1.5:0.5 and grinding them, adding deionized water after they are fully mixed and continuing to grind for 2 hours until a uniform viscous slurry is formed, and evenly scraping it on the carbon felt, and controlling the active material layer loading on the carbon felt to be about 0.2 g / cm 2 , five layers of carbon felt coated with active material layers are placed according to Figure 4 They are stacked one by one, and then the carbon felt without active material layer is covered on the exposed active material layer. The drying temperature is set at 90° C. and after drying, a positive electrode film layer containing 5 active material layers and 6 carbon felt layers is obtained.
[0065] The negative electrode comprises a negative electrode current collector 4 and a zinc foam 6; the negative electrode current collector 4 is a stainless steel current collector.
[0066] The electrolyte 8 includes an aqueous solution of 2.5 M lithium trifluoromethanesulfonate and 1 M zinc trifluoromethanesulfonate. The circulation flow rate of the electrolyte is 5 ml / min.
[0067] The diaphragm 7 is a hydrophilic nylon filter membrane with a pore size of 0.45 μm.
[0068] The shell includes a positive electrode shell 1 and a negative electrode shell 2. The positive electrode shell 1 is used to cover the positive electrode, and the negative electrode shell 2 is used to cover the negative electrode. The positive electrode shell 1 and the negative electrode shell 2 are connected by a sealing ring 9 and bolts. The shell is also provided with an electrolyte inlet 12 and an electrolyte outlet 13.
[0069] This embodiment provides a polyaniline-zinc single flow battery system, and its structural schematic diagram is shown in Figure 5 , including the above-mentioned polyaniline-zinc single-flow battery, further comprising:
[0070] A storage tank 10 is used to store electrolyte and is connected to the polyaniline-zinc single flow battery to replenish the electrolyte;
[0071] The electrolyte pump 11 provides power for the unidirectional circulation of the electrolyte.
[0072] The assembly method of the polyaniline-zinc single flow battery system comprises:
[0073] The positive electrode shell, positive electrode current collector, positive electrode film, diaphragm, zinc foam, negative electrode current collector and negative electrode shell are assembled in this order, and the positive electrode shell and negative electrode shell are sealed and connected using sealing rings and bolts; the positive electrode shell is provided with an electrolyte inlet, and the negative electrode shell is provided with an electrolyte outlet. The storage tank and the battery are connected through the electrolyte inlet and electrolyte outlet to form a loop, so that the electrolyte can circulate unidirectionally from the positive electrode to the negative electrode, and the circulation flow rate of the electrolyte is 5ml / min.
[0074] The polyaniline-zinc single flow battery system was charged and discharged with a charge cut-off voltage of 1.8 V and a discharge cut-off voltage of 0.4 V at 40 mA / cm 2 The battery is charged for 4 hours with a current of 160 mAh / cm 2 , the battery coulombic efficiency is 96.1% and the energy efficiency is 80.7%.
[0075] Example 2
[0076] This embodiment provides a polyaniline-zinc single flow battery, comprising:
[0077] The positive electrode comprises a positive electrode current collector 3 and a positive electrode film layer 5; the positive electrode film layer 5 comprises 5 active material layers and 6 carbon felt layers, and the active material layers and the carbon felt are arranged alternately; the active material layer comprises intrinsic polyaniline, lithium bis(trifluoromethanesulfonylimide) and carbon black in a mass ratio of 10:1.5:0.5; the loading amount of the active material layer on the single-layer carbon felt is 0.2 g / cm 2 ; The thickness of a single layer of carbon felt is 0.5 mm and the size is 2 cm×2 cm. The positive electrode current collector 3 is a stainless steel current collector. Among them, the preparation method of the positive electrode film layer 5 includes: mixing intrinsic polyaniline, lithium bis(trifluoromethanesulfonyl)imide, and carbon black in a mass ratio of 10:1.5:0.5 and grinding them, adding deionized water after they are fully mixed and continuing to grind for 2 hours until a uniform and viscous slurry is formed, and evenly scraping it on the carbon felt, and controlling the active material layer loading on the carbon felt to be about 0.2 g / cm 2 , five layers of carbon felt coated with active material layers are placed according to Figure 4They are stacked one by one, and then the carbon felt without active material layer is covered on the exposed active material layer. The drying temperature is set at 90° C. and after drying, a positive electrode film layer containing 5 active material layers and 6 carbon felt layers is obtained.
[0078] The negative electrode comprises a negative electrode current collector 4 and a zinc foam 6; the negative electrode current collector 4 is a stainless steel current collector.
[0079] The electrolyte 8 includes an aqueous solution of 2.5M lithium bis(trifluoromethanesulfonyl)imide and 1M zinc bis(trifluoromethanesulfonyl)imide. The circulation flow rate of the electrolyte is 5 ml / min.
[0080] The diaphragm 7 is a hydrophilic nylon filter membrane with a pore size of 0.45 μm.
[0081] The shell includes a positive electrode shell 1 and a negative electrode shell 2. The positive electrode shell 1 is used to cover the positive electrode, and the negative electrode shell 2 is used to cover the negative electrode. The positive electrode shell 1 and the negative electrode shell 2 are connected by a sealing ring 9 and bolts. The shell is also provided with an electrolyte inlet 12 and an electrolyte outlet 13.
[0082] This embodiment provides a polyaniline-zinc single flow battery system, comprising the above-mentioned polyaniline-zinc single flow battery, and further comprising:
[0083] A storage tank 10 is used to store electrolyte and is connected to the polyaniline-zinc single flow battery to replenish the electrolyte;
[0084] The electrolyte pump 11 provides power for the unidirectional circulation of the electrolyte.
[0085] The assembly method of the polyaniline-zinc single flow battery system comprises:
[0086] The positive electrode shell, positive electrode current collector, positive electrode film, diaphragm, zinc foam, negative electrode current collector and negative electrode shell are assembled in this order, and the positive electrode shell and negative electrode shell are sealed and connected using sealing rings and bolts; the positive electrode shell is provided with an electrolyte inlet, and the negative electrode shell is provided with an electrolyte outlet. The storage tank and the battery are connected through the electrolyte inlet and electrolyte outlet to form a loop, so that the electrolyte can circulate unidirectionally from the positive electrode to the negative electrode, and the circulation flow rate of the electrolyte is 5ml / min.
[0087] The polyaniline-zinc single flow battery system was charged and discharged with a charge cut-off voltage of 1.8 V and a discharge cut-off voltage of 0.4 V at 40 mA / cm 2 The battery is charged for 4 hours with a current of 160 mAh / cm 2 , the battery coulombic efficiency is 95.8% and the energy efficiency is 81.6%.
[0088] Example 3
[0089] This embodiment provides a polyaniline-zinc single flow battery, comprising:
[0090] The positive electrode comprises a positive electrode current collector 3 and a positive electrode film layer; the positive electrode film layer 5 comprises 5 active material layers and 6 carbon felt layers, and the active material layers and the carbon felt are arranged alternately; the active material layer comprises intrinsic polyaniline, lithium chloride and carbon black in a mass ratio of 10:1.5:0.5; the loading amount of the active material layer on the single-layer carbon felt is 0.2 g / cm 2 The thickness of a single layer of carbon felt is 0.5 mm and the size is 2 cm × 2 cm. The positive electrode current collector 3 is a stainless steel current collector. The preparation method of the positive electrode film layer 5 includes: mixing intrinsic polyaniline, lithium chloride and carbon black in a mass ratio of 10:1.5:0.5 and grinding them, adding deionized water after they are fully mixed and continuing to grind for 2 hours until a uniform viscous slurry is formed, and evenly scraping it on the carbon felt, and controlling the active material layer loading on the carbon felt to be about 0.2 g / cm 2 , five layers of carbon felt coated with active material layers are placed according to Figure 4 They are stacked one by one, and then the carbon felt without active material layer is covered on the exposed active material layer. The drying temperature is set at 90° C. and after drying, a positive electrode film layer containing 5 active material layers and 6 carbon felt layers is obtained.
[0091] The negative electrode comprises a negative electrode current collector 4 and a zinc foam 6; the negative electrode current collector 4 is a stainless steel current collector.
[0092] The electrolyte 8 includes an aqueous solution of 2.5M lithium chloride and 1M zinc chloride. The circulation flow rate of the electrolyte is 5 ml / min.
[0093] The diaphragm 7 is a hydrophilic nylon filter membrane with a pore size of 0.45 μm.
[0094] The shell includes a positive electrode shell 1 and a negative electrode shell 2. The positive electrode shell 1 is used to cover the positive electrode, and the negative electrode shell 2 is used to cover the negative electrode. The positive electrode shell 1 and the negative electrode shell 2 are connected by a sealing ring 9 and bolts. The shell is also provided with an electrolyte inlet 12 and an electrolyte outlet 13.
[0095] This embodiment provides a polyaniline-zinc single flow battery system, comprising the above-mentioned polyaniline-zinc single flow battery, and further comprising:
[0096] A storage tank 10 is used to store electrolyte and is connected to the polyaniline-zinc single flow battery to replenish the electrolyte;
[0097] The electrolyte pump 11 provides power for the unidirectional circulation of the electrolyte.
[0098] The assembly method of the polyaniline-zinc single flow battery system comprises:
[0099] The positive electrode shell, positive electrode current collector, positive electrode film, diaphragm, zinc foam, negative electrode current collector and negative electrode shell are assembled in this order, and the positive electrode shell and negative electrode shell are sealed and connected using sealing rings and bolts; the positive electrode shell is provided with an electrolyte inlet, and the negative electrode shell is provided with an electrolyte outlet. The storage tank and the battery are connected through the electrolyte inlet and electrolyte outlet to form a loop, so that the electrolyte can circulate unidirectionally from the positive electrode to the negative electrode, and the circulation flow rate of the electrolyte is 5ml / min.
[0100] The polyaniline-zinc single flow battery system was charged and discharged with a charge cut-off voltage of 1.8 V and a discharge cut-off voltage of 0.4 V at 40 mA / cm 2 The battery is charged for 4 hours with a current of 160 mAh / cm 2 , the battery coulombic efficiency is 93.8% and the energy efficiency is 78.3%.
[0101] Example 4
[0102] This embodiment provides a polyaniline-zinc single flow battery, comprising:
[0103] The positive electrode comprises a positive electrode current collector 3 and a positive electrode film layer; the positive electrode film layer 5 comprises 8 active material layers and 9 carbon felt layers, and the active material layers and the carbon felt are arranged alternately; the active material layer comprises intrinsic polyaniline, lithium tetrafluoroborate and carbon nanotubes in a mass ratio of 10:0.5:0.2; the loading amount of the active material layer on the single-layer carbon felt is 0.5 g / cm 2 ; The thickness of a single layer of carbon felt is 0.3 mm and the size is 2 cm × 2 cm. The positive electrode current collector 3 is a stainless steel current collector. The preparation method of the positive electrode film layer 5 includes: mixing intrinsic polyaniline, lithium tetrafluoroborate, and carbon nanotubes in a mass ratio of 10:0.5:0.2 and grinding them, adding 5 mL of deionized water after they are fully mixed and continuing to grind for 2 hours until a uniform and viscous slurry is formed, and evenly scraping it on the carbon felt, and controlling the active material layer loading on the carbon felt to be about 0.5 g / cm 2 , stack 8 layers of carbon felt coated with active material layers in sequence, then cover the exposed active material layer with carbon felt not coated with active material layers, set the drying temperature to 90°C, and after drying, obtain a positive electrode film layer containing 8 active material layers and 9 carbon felt layers.
[0104] The negative electrode comprises a negative electrode current collector 4 and a zinc foam 6; the negative electrode current collector 4 is a stainless steel current collector.
[0105] The electrolyte 8 includes an aqueous solution of 1.5 M lithium tetrafluoroborate and 1.5 M zinc tetrafluoroborate. The circulation rate of the electrolyte is 5 ml / min.
[0106] The diaphragm 7 is a hydrophilic nylon filter membrane with a pore size of 0.45 μm.
[0107] The shell includes a positive electrode shell 1 and a negative electrode shell 2. The positive electrode shell 1 is used to cover the positive electrode, and the negative electrode shell 2 is used to cover the negative electrode. The positive electrode shell 1 and the negative electrode shell 2 are connected by a sealing ring 9 and bolts. The shell is also provided with an electrolyte inlet 12 and an electrolyte outlet 13.
[0108] This embodiment provides a polyaniline-zinc single flow battery system, comprising the above-mentioned polyaniline-zinc single flow battery, and further comprising:
[0109] A storage tank 10 is used to store electrolyte and is connected to the polyaniline-zinc single flow battery to replenish the electrolyte;
[0110] The electrolyte pump 11 provides power for the unidirectional circulation of the electrolyte.
[0111] The assembly method of the polyaniline-zinc single flow battery system comprises:
[0112] The positive electrode shell, positive electrode current collector, positive electrode film, diaphragm, zinc foam, negative electrode current collector and negative electrode shell are assembled in this order, and the positive electrode shell and negative electrode shell are sealed and connected using sealing rings and bolts; the positive electrode shell is provided with an electrolyte inlet, and the negative electrode shell is provided with an electrolyte outlet. The storage tank and the battery are connected through the electrolyte inlet and electrolyte outlet to form a loop, so that the electrolyte can circulate unidirectionally from the positive electrode to the negative electrode, and the circulation flow rate of the electrolyte is 5ml / min.
[0113] The polyaniline-zinc single flow battery system was charged and discharged with a charge cut-off voltage of 1.8 V and a discharge cut-off voltage of 0.4 V at 40 mA / cm 2 The battery is charged for 4 hours with a current of 160 mAh / cm 2 , the battery coulombic efficiency is 93.4% and the energy efficiency is 80.2%.
[0114] Example 5
[0115] This embodiment provides a polyaniline-zinc single-flow battery system, which is different from the embodiment 1 in that: the positive electrode structure is different. The positive electrode of this embodiment includes a positive electrode current collector and an active material layer, and the active material layer is attached to the positive electrode current collector; the composition of the active material layer is the same as that of the embodiment 1, and the loading amount of the active material layer is 1g / cm 2 .
[0116] The polyaniline-zinc single flow battery system was charged and discharged with a charge cut-off voltage of 1.8 V and a discharge cut-off voltage of 0.4 V at 40 mA / cm 2 The battery is charged for 4 hours with a current of 160 mAh / cm 2 , the battery coulombic efficiency is 91.8% and the energy efficiency is 73.5%.
[0117] Comparative Example 1
[0118] This comparative example provides a polyaniline-zinc single-flow battery, which is different from Example 1 in that the electrolyte is not circulated.
[0119] The battery provided in this comparative example has a running time of about 3.15 hours and cannot be fully charged in 4 hours. When the area capacity reaches 126 mAh / cm 2 When the cut-off voltage reaches 1.8V, the coulombic efficiency is 90.1% and the energy efficiency is 63.8%. In this comparative example, the resistance increases due to concentration polarization, and the overpotential is large, so the charging process reaches the cut-off potential. This further illustrates that the present invention can effectively eliminate electrode polarization and improve the energy efficiency of the battery by designing the battery as a single liquid flow battery.
[0120] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A polyaniline-zinc single flow battery, characterized in that: It comprises a positive electrode, a negative electrode, an electrolyte and a separator; the positive electrode comprises a positive electrode film layer, the positive electrode film layer comprises at least one active material layer, and the active material of the active material layer comprises intrinsic polyaniline; the negative electrode comprises a zinc sheet; The electrolyte circulates unidirectionally in the polyaniline-zinc single-flow battery.
2. The polyaniline-zinc single flow battery according to claim 1, characterized in that: The electrolyte circulates unidirectionally from the positive electrode to the negative electrode; or, The electrolyte circulates unidirectionally from the negative electrode to the positive electrode.
3. The polyaniline-zinc single flow battery according to claim 1, characterized in that: The electrolyte comprises a lithium salt and a zinc salt; Preferably, the concentration of lithium salt in the electrolyte is 1-5M; Preferably, the concentration of lithium salt in the electrolyte is 1.5-2.5M; Preferably, the concentration of zinc salt in the electrolyte is 0.5-2.5M; Preferably, the concentration of zinc salt in the electrolyte is 0.8-1.2M.
4. The polyaniline-zinc single flow battery according to claim 3, characterized in that: The anions of the lithium salt and the zinc salt are the same; Preferably, the anions in the electrolyte include at least one of sulfate ions, nitrate ions, acetate ions, trifluoromethanesulfonate ions, bistrifluoromethanesulfonyl imide ions, tetrafluoroborate ions, chloride ions and bromide ions; Preferably, the anions in the electrolyte include at least one of trifluoromethanesulfonate ions, bistrifluoromethanesulfonyl imide ions and chloride ions.
5. The polyaniline-zinc single flow battery according to claim 1, characterized in that: The positive electrode film layer also includes at least one layer of carbon felt; Preferably, the carbon felt is disposed on both sides of the active material layer; Preferably, the carbon felt and the active material layer are arranged alternately.
6. The polyaniline-zinc single flow battery according to claim 5, characterized in that: The loading amount of the active material layer is 0.1-1 g / cm 2 ; Preferably, the loading amount of the active material layer is 0.2-0.3 g / cm 2 .
7. The polyaniline-zinc single flow battery according to claim 1 or 5, characterized in that: The positive electrode film layer includes 2-10 layers of active material layers; Preferably, the positive electrode film layer includes 4-6 active material layers.
8. The polyaniline-zinc single flow battery according to claim 5, characterized in that: The thickness of the carbon felt is 0.1-1 mm; Preferably, the carbon felt has a thickness of 0.25-0.5 mm.
9. The polyaniline-zinc single flow battery according to claim 3 or 4, characterized in that: The active material layer also includes at least one of a lithium salt and a conductive agent; Preferably, the lithium salt in the active material layer is the same as the lithium salt in the electrolyte.
10. The polyaniline-zinc single flow battery according to claim 9, characterized in that: The mass ratio of the lithium salt to the intrinsic polyaniline is (5-20):100; Preferably, the mass ratio of the conductive agent to the intrinsic polyaniline is (2-10):
100.
11. The polyaniline-zinc single flow battery according to claim 1, characterized in that: Satisfy at least one of (1)-(3): (1) The positive electrode further includes a positive electrode current collector, which is laminated to the positive electrode film layer; (2) The negative electrode further includes a negative electrode current collector, which is bonded to the zinc sheet; (3) The polyaniline-zinc single-flow battery further includes a shell, which is disposed outside the positive electrode and the negative electrode; the shell is also provided with an electrolyte inlet and an electrolyte outlet.
12. A polyaniline-zinc single flow battery system, characterized in that: The invention comprises at least one group of polyaniline-zinc single flow batteries as described in any one of claims 1 to 11; and further comprises at least one of (1) to (2): (1) a storage tank containing an electrolyte for replenishing the electrolyte for the polyaniline-zinc single-flow battery; (2) An electrolyte pump, wherein the electrolyte pump provides power for the unidirectional circulation flow of the electrolyte.