Deep-cycle long-life lead-acid storage battery for new energy vehicle as well as preparation method and application of lead-acid storage battery

By adding SnOx, carbon black and graphite to the positive and negative lead paste of lead-acid batteries, and using high-temperature and high-humidity curing technology, the problem of insufficient deep circulation and charging capacity of lead-acid batteries for new energy vehicles has been solved, and a longer time has been achieved service life and higher cycle durability.

CN119069832APending Publication Date: 2024-12-03JUJIANG POWER TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411193838.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Small-capacity lead-acid batteries for new energy vehicles perform poorly in deep circulation and charging, resulting in mudification and sulfation of the active substances on the plate, which fails early and cannot meet the design life requirements.

Method used

Add SnOx to the positive lead paste, carbon black and graphite to the negative lead paste, and adopt high-temperature and high-humidity curing technology to reduce the height of the plate, increase the number of plates and contact area, and enhance the lead paste and the grid through these methods. Combination power improves charging acceptance and cycle durability.

Benefits of technology

It significantly improves the charging acceptance and circulation life of the battery, extends the deep circulation capacity of the battery, and meets the high requirements of new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015795270000031
    Figure BDA0005015795270000031
  • Figure BDA0005015795270000041
    Figure BDA0005015795270000041
  • Figure BDA0005015795270000042
    Figure BDA0005015795270000042
Patent Text Reader

Abstract

The invention belongs to the technical field of manufacturing of lead-acid storage batteries for starting, and particularly relates to a deep-cycle long-life lead-acid storage battery for a new energy vehicle as well as a preparation method and application of the lead-acid storage battery. The preparation method of the lead-acid storage battery comprises the following steps: S1, coating a positive grid with positive lead paste, and coating a negative grid with negative lead paste to obtain a positive unformed plate and a negative unformed plate; s2, curing and drying the positive unformed plate and the negative unformed plate in a curing chamber to obtain a positive plate and a negative plate; and S3, packaging the positive plate, the negative plate and the partition plate, manufacturing a plate group through cast welding, filling the plate group into a battery jar, thermally sealing and assembling a jar cover into a semi-finished battery, and charging the semi-finished battery for formation to obtain a finished battery. Test results show that the deep-cycle long-life lead-acid storage battery for the new energy vehicle has good 20h rate capacity,-18 DEG C low-temperature starting capability, 0 DEG C charging acceptance capability and cycle durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of manufacturing lead-acid batteries for starting, and specifically relates to a deep-cycle long-life lead-acid battery for new energy vehicles, and a preparation method and application thereof. Background Art

[0002] New energy vehicles refer to vehicles that use unconventional vehicle fuels as a power source (or use conventional vehicle fuels and adopt new vehicle power devices), integrate advanced technologies in vehicle power control and drive, and form vehicles with advanced technical principles, new technologies, and new structures. As the degree of electrification of new energy vehicles increases, the power consumption of various operating conditions increases, and higher requirements are placed on the battery's charging acceptance and deep cycle charging and discharging capabilities. At present, new energy vehicles generally select small-capacity (below 50Ah) lead-acid batteries, and lead-acid batteries have premature failures such as plate active material mud and plate sulfation, which are far from the design life. Therefore, it is urgent to develop a lead-acid battery for new energy vehicles to improve the problems of low deep cycle capacity and charging acceptance and short service life of lead-acid batteries. Summary of the invention

[0003] According to a first aspect of the present invention, there is provided a method for preparing a deep cycle long life lead-acid battery for new energy vehicles, comprising the following steps:

[0004] S1. Coating a positive lead paste on the positive electrode grid and a negative lead paste on the negative electrode grid to obtain a positive electrode plate and a negative electrode plate;

[0005] S2, placing the positive electrode plate and the negative electrode plate in a curing chamber for curing and drying to obtain a positive electrode plate and a negative electrode plate;

[0006] S3. After the positive and negative plates and separators are encapsulated, they are made into pole groups by cast welding, and then loaded into battery slots. The slot covers are heat-sealed to assemble into semi-finished batteries, and then the semi-finished batteries are charged and formed to obtain finished batteries.

[0007] In some embodiments, the raw material composition of the positive electrode lead paste includes, by mass, 900-1100 parts of lead powder, 130-150 parts of water, 90-110 parts of sulfuric acid, 0.8-1.1 parts of short fibers, 3.0-6.0 parts of 4BS seeds (i.e., tetrabasic lead sulfate), 2-3 parts of sodium perborate, SnO x 1.1 to 1.5 parts, of which SnO x The value of x is any value between 1 and 2, and the density of sulfuric acid is 1.38 to 1.42 g / cm 3 .

[0008] The present invention adds SnO to the positive electrode lead paste xThe purpose is to use the Sn in the grid alloy and the Sn in the lead paste to form a stable interface through the curing process, enhance the bonding force between the lead paste and the grid, reduce the internal resistance, and improve the charging acceptance capacity.

[0009] In some embodiments, the raw material composition of the negative electrode lead paste includes, by mass, 900-1100 parts of lead powder, 80-150 parts of water, 68-90 parts of sulfuric acid, 0.3-0.5 parts of short fibers, 8-15 parts of composite additives, 0.3-0.6 parts of carbon black, and 0.3-0.6 parts of graphite, wherein the density of sulfuric acid is 1.38-1.42 g / cm 3 .

[0010] The present invention adds carbon black and graphite to the negative electrode lead paste, the purposes of which are: first, utilizing the characteristics of high capacitance and high conductivity to form a conductive network and improve the conductivity of the negative electrode plate; second, reducing the reaction overpotential of lead generation and promoting the lead deposition process; third, forming a second phase to avoid the generation of coarse lead sulfate particles, making the lead sulfate easy to dissolve and avoiding irreversible sulfation; and fourth, improving the low-temperature discharge performance of the battery.

[0011] In some embodiments, the composite additive consists of 0.3-0.7 wt% of barium sulfate based on the mass of the lead powder and 1.0-2.0 wt% of lignin based on the mass of the lead powder.

[0012] The present invention adds a composite additive into the negative electrode lead paste, which can improve the plate porosity, prevent the lead surface from shrinking, improve the charge and discharge performance of the plate, and increase the cycle life of the battery.

[0013] In some embodiments, when the green plate is cured, the temperature and humidity of the curing chamber are set according to the following procedure:

[0014] In the first stage, the temperature is 75℃, the humidity is 98%, and the air volume is 25m 3 / min, time 0.5h;

[0015] The second stage, temperature 75℃, humidity 90%, wind volume 25m 3 / min, time 12h;

[0016] The third stage, temperature 54℃, humidity 85%, wind volume 25m 3 / min, time 0.5h;

[0017] Stage 4: Temperature 54°C, humidity 80%, wind volume 30m 3 / min, time 8h;

[0018] The fifth stage, temperature 54℃, humidity 50%, wind volume 50m 3 / min, time 4h;

[0019] When the green plates are drying, set the temperature and humidity of the curing chamber according to the following procedure:

[0020] In the first stage, the temperature is 55℃, the humidity is 40%, and the air volume is 60m 3 / min, time 6h;

[0021] The second stage, temperature 65℃, humidity 20%, air volume 75m 3 / min, time 4h;

[0022] The third stage, temperature 75℃, humidity 15%, wind volume 90m 3 / min, time 3h;

[0023] Stage 4: Temperature 80°C, humidity 3%, air volume 95m 3 / min, time 22h;

[0024] The fifth stage, temperature 45℃, humidity 3%, wind volume 50m 3 / min, time 1h.

[0025] The present invention adopts a high temperature and high humidity curing process with a maximum curing temperature of 75° C., thereby enhancing the bonding force between the lead paste and the grid, reducing the internal resistance, and improving the charging acceptance and service life of the battery.

[0026] The present invention adopts a method of gradually reducing the temperature and humidity from a high temperature of 75° C. and a high humidity of 98% during the green plate curing stage, which is beneficial to further oxidation of Pb and can form tribasic lead sulfate (3BS) and tetrabasic lead sulfate (4BS) of specific composition, thereby improving the service life and initial performance of the battery.

[0027] The present invention adopts five stages of different temperatures and humidity when drying the green plates, with the purpose of slowly drying the plates on the basis of gradually reducing the humidity, so as to avoid the rapid water loss of the plates causing cracking of the lead paste and affecting the battery performance.

[0028] In some embodiments, the plate parameters of the pole group are: the height of the positive plate is 110-120 mm, the number of positive plates is 4-7 pcs, the height of the negative plate is 110-120 mm, the number of negative plates is 4-7 pcs, and the contact area between the positive and negative plates is 60000-90000 mm 2 .

[0029] The present invention reduces the internal resistance and improves the charging acceptance capacity of the battery by reducing the height of the electrode plate, increasing the number of electrode plates, and increasing the contact area between the positive and negative electrode plates.

[0030] In some embodiments, the semi-finished battery is charged and formed according to the following method:

[0031] The first stage of charging: charging current 0.6C, charging time 2h;

[0032] The second stage is to let it stand for 30 minutes;

[0033] The third stage of charging: charging current 0.4C, charging time 8h;

[0034] The fourth stage of charging: charging current 0.2C, charging time 5h.

[0035] According to a second aspect of the present invention, a deep-cycle and long-life lead-acid battery for new energy vehicles prepared by the above-mentioned preparation method is provided.

[0036] According to a third aspect of the present invention, there is provided a use of the above-mentioned deep-cycle and long-life lead-acid battery for new energy vehicles in the preparation of new energy vehicles.

[0037] The beneficial effects of the present invention include:

[0038] (1) The present invention adds SnO to the positive electrode lead paste x By adding carbon black and graphite to the negative electrode lead paste, adopting a high temperature and high humidity curing process, reducing the plate height, increasing the number of plates, and increasing the contact area between the positive and negative plates, the internal resistance of the battery is reduced, which helps to improve the battery's charging acceptance capacity.

[0039] (2) The present invention adds SnO to the positive electrode lead paste x , using high temperature and high humidity curing process, which enhances the bonding strength between the lead paste and the grid, improves the 4BS crystal form, enhances the cycle durability of the battery, and extends the cycle service life of the battery. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with specific examples. It is worth noting that the following examples are only for better explanation of the content of the present invention and do not limit the scope of protection of the present invention. The process steps not disclosed in the examples are prior art.

[0041] Example 1

[0042] The deep cycle long life lead-acid battery for new energy vehicles of this embodiment includes a positive electrode grid, a positive electrode lead paste coated on the positive electrode grid, a negative electrode grid, and a negative electrode lead paste coated on the negative electrode grid, wherein the formula of the positive electrode lead paste is shown in Table 1:

[0043] Table 1 Positive electrode lead paste formula of Example 1

[0044]

[0045]

[0046] The formula of negative electrode lead paste is shown in Table 2:

[0047] Table 2 Negative electrode lead paste formula of Example 1

[0048] composition Mass / kg Lead powder 1000 Pure water 100 <![CDATA[Sulfuric acid (1.42 g / cm 3 )]]> 68 Short Fiber 0.5 Compound Additives 14.1 Carbon Black 0.5 graphite 0.5

[0049] Note: The composite additive in Table 2 consists of 3.5 kg barium sulfate and 10.6 kg lignin.

[0050] The preparation method thereof comprises the following steps:

[0051] (1) Preparation of positive electrode lead paste: Weigh lead powder, short fibers, 4BS seeds, sodium perborate, and SnO2 by mass, pour into a positive electrode paste machine, mix well, add pure water, stir well, then add sulfuric acid under stirring conditions, continue stirring, and control the paste temperature below 68°C. The apparent density of the lead paste before producing the paste is 4.54 g / cm 3 When the apparent density of the lead paste reaches the standard and the temperature is lower than 50°C, the paste is produced to obtain the positive electrode lead paste.

[0052] (2) Preparation of negative electrode lead paste: Weigh lead powder, short fibers, composite additives, carbon black, and graphite by mass, pour into a negative electrode paste machine, mix well, add pure water, stir well, then add sulfuric acid under stirring conditions, continue stirring, and control the paste temperature below 68°C. The apparent density of the lead paste before producing the paste is 4.55 g / cm 3 When the apparent density of the lead paste reaches the standard and the temperature is lower than 50°C, the paste is produced to obtain the negative electrode lead paste.

[0053] (3) Plate coating: Coat the positive electrode grid with positive lead paste and coat the negative electrode grid with negative lead paste to obtain positive and negative electrode plates.

[0054] (4) Curing and drying of green plates: The positive green plates and negative green plates are placed in a curing chamber for curing and drying. The temperature and humidity of the curing chamber are set according to the procedure shown in Table 3 to obtain positive and negative plates.

[0055] Table 3 Green plate curing and drying procedures

[0056]

[0057]

[0058] (5) Battery assembly: After the positive and negative plates and separators are encapsulated, they are made into electrode groups by COS casting welding (the electrode plate parameters of the electrode group are shown in Table 4), then installed in the battery slot, and the slot cover is heat-sealed to assemble into a semi-finished battery.

[0059] Table 4 Plate parameters of pole group

[0060]

[0061] (6) Battery formation: Add dilute sulfuric acid (1.2 g / cm 3 ), after standing for 50 minutes, it is electrified and the charging process is as follows:

[0062] The first stage of charging: charging current 0.6C, charging time 2h;

[0063] The second stage is to let it stand for 30 minutes;

[0064] The third stage of charging: charging current 0.4C, charging time 8h;

[0065] The fourth stage of charging: charging current 0.2C, charging time 5h;

[0066] After the formation charge is completed, the battery is replaced with acid (the acid density of the battery when it leaves the factory is 1.28g / cm 3 ), liquid level adjustment, small cover heat sealing, cleaning and drying, to obtain the finished battery.

[0067] Below, based on the 6-QW-32 starting lead-acid battery standard, the deep cycle and long life lead-acid battery for new energy vehicles prepared in Example 1 (3 batteries, marked as 1#, 2#, and 3#, respectively) was tested according to the GB / T5008-2013 standard and the JB / T12666 standard, and an ordinary 32Ah lead-acid battery was used as a comparative example. The test results are shown in Table 5.

[0068] Table 5 Battery test results

[0069]

[0070]

[0071] As can be seen from Table 5, the 20h rate capacity, -18℃ low temperature starting capability, 0℃ charge acceptance and cycle endurance of 1#, 2# and 3# lead-acid batteries all meet the technical requirements, among which the 0℃ charge acceptance and cycle endurance are more than 40% higher than the technical requirements, which shows that the deep-cycle and long-life lead-acid battery for new energy vehicles of the present invention has excellent 20h rate capacity, -18℃ low temperature starting capability, 0℃ charge acceptance and cycle endurance, and meets the requirements for deep-cycle and long-life for new energy vehicles; while the 20h rate capacity and -18℃ low temperature starting capability of the ordinary 32Ah lead-acid battery in the comparative example just meet the technical requirements, and the 0℃ charge acceptance and cycle endurance do not meet the requirements for deep-cycle and long-life for new energy vehicles.

[0072] The present invention adds SnO into the positive electrode lead paste. xBy adding carbon black and graphite to the negative electrode lead paste, adopting a high temperature and high humidity curing process, reducing the plate height, increasing the number of plates, and increasing the contact area between the positive and negative plates, the internal resistance of the battery is reduced, which helps to improve the battery's charging acceptance capacity.

[0073] The present invention adds SnO into the positive electrode lead paste. x , using high temperature and high humidity curing process, which enhances the bonding strength between the lead paste and the grid, improves the 4BS crystal form, enhances the cycle durability of the battery, and extends the cycle service life of the battery.

[0074] The above are only some specific embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a deep-cycle long-life lead-acid battery for new energy vehicles, It is characterized in that The steps include: S1. Coating a positive lead paste on the positive electrode grid and a negative lead paste on the negative electrode grid to obtain a positive electrode plate and a negative electrode plate; S2, placing the positive electrode plate and the negative electrode plate in a curing chamber for curing and drying to obtain a positive electrode plate and a negative electrode plate; S3. After the positive and negative plates and separators are encapsulated, they are made into pole groups by cast welding, and then loaded into battery slots. The slot covers are heat-sealed to assemble into semi-finished batteries, and then the semi-finished batteries are charged and formed to obtain finished batteries.

2. The preparation method according to claim 1, It is characterized in that The raw material composition of the positive lead paste includes, by weight: 900-1100 parts of lead powder, 130-150 parts of water, 90-110 parts of sulfuric acid, 0.8-1.1 parts of short fibers, 3.0-6.0 parts of 4BS seeds, 2-3 parts of sodium perborate, SnO x 1.1 to 1.5 parts, the SnO x The value of x is any value between 1 and 2, and the density of sulfuric acid is 1.38 to 1.42 g / cm 3 .

3. The preparation method according to claim 1 or 2, It is characterized in that The raw material composition of the negative electrode lead paste includes, by mass, 900-1100 parts of lead powder, 80-150 parts of water, 68-90 parts of sulfuric acid, 0.3-0.5 parts of short fibers, 8-15 parts of composite additives, 0.3-0.6 parts of carbon black, and 0.3-0.6 parts of graphite. The density of the sulfuric acid is 1.38-1.42 g / cm 3 .

4. The preparation method according to claim 3, It is characterized in that The composite additive consists of 0.3-0.7wt% of barium sulfate by weight of the lead powder and 1.0-2.0wt% of lignin by weight of the lead powder.

5. The preparation method according to claim 1 or 2, It is characterized in that When curing green plates, set the temperature and humidity of the curing chamber according to the following procedure: In the first stage, the temperature is 75℃, the humidity is 98%, and the air volume is 25m 3 / min, time 0.5h; The second stage, temperature 75℃, humidity 90%, wind volume 25m 3 / min, time 12h; The third stage, temperature 54℃, humidity 85%, wind volume 25m 3 / min, time 0.5h; Stage 4: Temperature 54°C, humidity 80%, wind volume 30m 3 / min, time 8h; Stage 5: Temperature 54°C, humidity 50%, wind volume 50m 3 / min, time 4h; When the green plates are drying, set the temperature and humidity of the curing chamber according to the following procedure: In the first stage, the temperature is 55℃, the humidity is 40%, and the air volume is 60m 3 / min, time 6h; The second stage, temperature 65℃, humidity 20%, air volume 75m 3 / min, time 4h; The third stage, temperature 75℃, humidity 15%, wind volume 90m 3 / min, time 3h; Stage 4: Temperature 80°C, humidity 3%, air volume 95m 3 / min, time 22h; The fifth stage, temperature 45℃, humidity 3%, wind volume 50m 3 / min, time 1h.

6. The preparation method according to claim 1 or 2, It is characterized in that The plate parameters of the pole group are as follows: the height of the positive plate is 110-120 mm, the number of positive plates is 4-7 pcs, the height of the negative plate is 110-120 mm, the number of negative plates is 4-7 pcs, and the contact area between the positive and negative plates is 60000-90000 mm 2 .

7. The preparation method according to claim 1 or 2, It is characterized in that The semi-finished battery is charged and formed as follows: The first stage of charging: charging current 0.6C, charging time 2h; The second stage is to let it stand for 30 minutes; The third stage of charging: charging current 0.4C, charging time 8h; The fourth stage of charging: charging current 0.2C, charging time 5h.

8. A deep-cycle and long-life lead-acid battery for new energy vehicles prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the deep-cycle long-life lead-acid battery for new energy vehicles as claimed in claim 8 in the preparation of new energy vehicles.

Citation Information

Patent Citations

  • Deep-cycle long-life lead-acid storage battery lead paste for parking, battery thereof and manufacturing process method of battery

    CN113675397A

  • Energy storage battery

    CN116417760A

  • Additive for anti-softening long-life storage battery positive electrode lead paste

    CN118352523A