Wave-absorbing composite material based on graphene oxide and preparation method thereof

By combining graphene oxide with multi-metal alloy nanoparticles, the solution method and lyophilization technology are used to prepare wave absorbing composite materials, which solves the problems of high density, easy corrosion and complex synthesis processes of existing metal wave absorbing materials, and achieves high ratio Highly efficient electromagnetic energy absorption in the surface area and wide frequency domain significantly improves wave absorption performance.

CN119072102APending Publication Date: 2024-12-03NANJING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174260.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing metal absorbent materials have problems such as high density, easy corrosion, high thermal expansion coefficient and complex synthesis process, which limits their application scope in practical applications, especially the reflection loss of FeCoNi/C absorbent materials is weak and effective absorption. Narrow bandwidth.

Method used

Using graphene oxide-based absorbing composite material preparation method, by combining graphene oxide with multi-metal alloy nanoparticles, loose and porous carbon-based precursors are prepared by solution method and lyophilization technology, and pre-carbonization is pre-carbonized under protective atmosphere and Sintering to form an absorbing material with high specific surface area and excellent absorbing properties.

Benefits of technology

Absorbing materials with simple process and large-scale production are achieved, improving the specific surface area and absorption performance of the material, with a maximum reflection loss of -67dB, an effective absorption bandwidth of 5.58GHz, and a reduced material density and enhanced chemical stability. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072102A_ABST
    Figure CN119072102A_ABST
Patent Text Reader

Abstract

The invention discloses a graphene oxide-based wave-absorbing composite material and a preparation method thereof, and the preparation method comprises the following steps: dispersing graphene oxide in deionized water to prepare a dispersion liquid; adding metal acetate, sodium carboxymethyl cellulose (CMC), glucose and polyvinyl alcohol (PVA) into the dispersion liquid, and stirring in a water bath to obtain a mixed solution; quickly freezing the mixed solution, and then freeze-drying to prepare a loose and porous carbon-based precursor; and under a protective atmosphere, pre-carbonizing the precursor and then sintering to prepare the wave-absorbing composite material based on the graphene oxide. According to the method, loading of the alloy nanoparticles on the surface of the graphene oxide is achieved by adopting a simple and convenient technological process, and the method has high generalizability and large-scale performance; the wave-absorbing composite material is prepared through a solution method and freeze-drying, the particle size distribution of metal particles in the material is uniform, the specific surface area of the material is large, the wave-absorbing effect can be enhanced, and the strongest reflection loss can reach-67 dB.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a wave-absorbing material and a preparation method thereof, and in particular to a wave-absorbing composite material based on graphene oxide and a preparation method thereof. Background Art

[0002] With the in-depth expansion of wireless devices in the military and civilian fields, electromagnetic shielding technology has gradually played an increasingly prominent role in military confrontation, maintaining the normal operation of highly integrated electronic equipment, and reducing electromagnetic pollution in the living environment. As a branch of electromagnetic shielding technology, absorbing materials are unique in electromagnetic shielding technology due to their low energy excitation dependence, wide range of applications, and low startup cost.

[0003] For common metal and alloy absorbing materials, their high electrical conductivity or magnetic permeability effectively dissipates the energy from the external electromagnetic field. In addition, their outstanding mechanical strength and easy processing also make metal-based absorbing materials widely used in practical scenarios. Compared with a single metal system, multi-metal alloys not only provide a variety of elemental compositions and resonant frequencies, but also achieve efficient scattering (reflection) of electromagnetic waves by forming complex phase interfaces. Through the reasonable combination of the absorption frequency bands of multi-metal systems, the coverage frequency range of metal absorbing materials can be effectively broadened. However, metal absorbing materials also have problems such as high density, easy corrosion (especially in humid environments), and high thermal expansion coefficient (easy to crack in environments with large temperature gradients), which restricts their scope of application in actual use.

[0004] The strongest reflection loss of the existing FeCoNi / C absorbing material is relatively weak, usually between -20 and -55 dB, and the effective absorption bandwidth (EAB, RL min <-10dB) is narrow, usually less than 5GHz, and the synthesis process is more complicated. Summary of the invention

[0005] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a graphene oxide-based absorbing composite material with a simple process and scalable production. Another purpose of the present invention is to provide a graphene oxide-based absorbing composite material with a large specific surface area and good absorbing performance.

[0006] Technical solution: The method for preparing a microwave-absorbing composite material based on graphene oxide described in the present invention comprises the following steps:

[0007] Step 1, dispersing graphene oxide in deionized water to prepare a dispersion;

[0008] Step 2, adding metal acetate, sodium carboxymethyl cellulose (CMC), glucose, and polyvinyl alcohol (PVA) to the dispersion, stirring in a water bath to obtain a mixed solution;

[0009] Step 3, the mixed solution is first quickly frozen and then freeze-dried to obtain a loose and porous carbon-based precursor;

[0010] Step 4: Under a protective atmosphere, the precursor is pre-carbonized and then sintered to obtain a graphene oxide-based microwave absorbing composite material.

[0011] CMC mainly plays the role of thickening and stabilizing the system, avoiding the sedimentation of insoluble substances in the dispersion and maintaining the uniformity of the dispersion;

[0012] Glucose is mainly introduced as a carbon source to form a carbon shell on the surface of metal nanoparticles, which can enhance the conductivity of the material on the one hand, and form a microporous structure on the surface of the material on the other hand, thereby enhancing the specific surface area of ​​the material. Both contribute to the improvement of the material's microwave absorption performance.

[0013] The introduction of PVA can maintain the shape and structure of the precursor during the freeze-drying process to avoid collapse or shrinkage

[0014] Furthermore, in step 1, the graphene oxide is in a lamellar shape, and the mass ratio of the graphene oxide to deionized water is 1:100-500.

[0015] Furthermore, in step 1, the dispersion method is stirring for 2 hours, ultrasonic dispersion for 20 minutes, and repeated at least 10 times. Insufficient dispersion time or number of times, and excessive addition of graphene oxide will result in poor dispersion quality of the dispersion.

[0016] Furthermore, in step 2, the metal acetate is one or more of ferric acetate, nickel acetate, and cobalt acetate, and the concentration of the metal acetate in the mixed solution is 0.2-0.8 mol / L. The mass ratio of sodium carboxymethyl cellulose to graphene oxide is 0.5-1.5:1. The mass ratio of metal acetate, sodium carboxymethyl cellulose, glucose, and polyvinyl alcohol is 2.66-2.78:0.2:2.5:1. The temperature of the water bath is 40-70°C, the stirring time is 4-7 hours, and the rotation speed is 400-800 rpm. Too high a concentration of metal acetate will cause the particle size of the metal nanoparticles to be too large, affecting the wave absorbing performance.

[0017] Furthermore, in step three, the rapid freezing is rapid freezing in liquid nitrogen for 8 to 12 hours, and the freeze-drying time is 72 to 96 hours.

[0018] Furthermore, in step 4, the protective atmosphere is argon, the pre-carbonization temperature is 450-550° C., the sintering temperature is 700-850° C., and the heating rate is 5° C. / min.

[0019] The graphene oxide-based microwave absorbing composite material obtained by the preparation method of the graphene oxide-based microwave absorbing composite material has a surface area of ​​65 to 10 m 2 / g, the surface of graphene oxide is evenly loaded with metal nanoparticles with a particle size of 20 to 50 nm.

[0020] Preparation principle: Combine multi-metal alloys with graphene oxide to prepare wave-absorbing composite materials, so that the material body can not only achieve efficient electromagnetic energy absorption in a wide frequency domain (characteristics of multi-metal alloys), but also achieve a reduction in unit mass (carbon materials have the characteristics of low density) and enhanced chemical stability (carbon materials protect metal particles). In addition, by loading alloy nanoparticles on graphene oxide sheets, enhancing the interface polarization of the composite material and introducing internal multiple reflection (scattering), the wave-absorbing performance is synergistically improved.

[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant features:

[0022] 1. A relatively simple process was used to realize the loading of alloy nanoparticles on the surface of graphene oxide, and the method has strong scalability and applicability;

[0023] 2. The microwave-absorbing composite material is prepared by solution method and freeze-drying. The particle size distribution of metal particles in the material is uniform and the specific surface area of ​​the material is large, which is conducive to enhancing the microwave-absorbing effect;

[0024] 3. Combining small-particle magnetic metal alloys with graphene materials synergistically enhances the material's wave absorption performance, with the highest reflection loss (RL min ) can reach -67dB, effective absorption bandwidth (EAB, RL min <-10dB) up to 5.58GHz. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a reflection loss performance diagram of the Fe-Ni alloy / graphene oxide absorbing composite material of the present invention;

[0026] Figure 2 This is a scanning electron microscope image of the Fe-Ni alloy / graphene oxide absorbing composite material of the present invention;

[0027] Figure 3 It is a reflection loss performance diagram of the Fe-Co alloy / graphene oxide absorbing composite material of the present invention;

[0028] Figure 4 This is a scanning electron microscope image of the Fe-Co alloy / graphene oxide absorbing composite material of the present invention;

[0029] Figure 5 This is a reflection loss performance diagram of the Ni-Co alloy / graphene oxide absorbing composite material of the present invention;

[0030] Figure 6This is a scanning electron microscope image of the Ni-Co alloy / graphene oxide absorbing composite material of the present invention;

[0031] Figure 7 It is a reflection loss performance diagram of the Fe-Ni-Co alloy / graphene oxide absorbing composite material of the present invention;

[0032] Figure 8 It is a scanning electron microscope image of the Fe-Ni-Co alloy / graphene oxide absorbing composite material of the present invention. DETAILED DESCRIPTION

[0033] Unless otherwise specified, the materials, reagents, instruments, etc. used in the following examples can be obtained from commercial sources. Experimental methods without specific conditions in the examples are usually carried out under conventional conditions or under conditions recommended by the manufacturer. Graphene oxide is in the form of flakes.

[0034] Example 1

[0035] A method for preparing a Fe-Ni alloy / graphene oxide wave absorbing composite material comprises the following steps:

[0036] (1) 200 mg of graphene oxide was dispersed in 30 ml of deionized water, stirred for 2 hours, and ultrasonically dispersed for 20 minutes, and repeated 12 times to prepare a dispersion.

[0037] (2) Add 7.5 mmol of ferric acetate (1.45 g), 7.5 mmol of nickel acetate (1.33 g), 200 mg of sodium carboxymethyl cellulose (CMC), 2.5 g of glucose, and 1 g of polyvinyl alcohol to the dispersion, heat to 60° C. in a water bath, and apply mechanical stirring at 500 rpm for 5 hours at the same temperature to obtain a mixed solution. The concentration of the metal acetate in the mixed solution is 0.5 mol / L.

[0038] (3) The mixed solution was rapidly frozen in liquid nitrogen for 8 hours and then freeze-dried for 96 hours to obtain a loose and porous carbon-based precursor.

[0039] (4) Under the protection of high-purity argon, the precursor was pre-carbonized at 500°C for 2 hours at a heating rate of 5°C / min, and then sintered at 750°C for 3 hours to obtain a Fe-Ni alloy / graphene oxide absorbing composite material.

[0040] The Fe-Ni alloy / graphene oxide absorbing composite material obtained in this example has a specific surface area of ​​71 m 2 / g, using the coaxial line method to test the wave absorption performance Figure 1 As shown, the appearance is Figure 2 As shown. Figures 1-2 It can be seen that in terms of performance, the strongest reflection loss of the material can reach -28dB, and the effective absorption bandwidth (EAB, RLmin <-10dB) can reach 5.04GHz; in terms of morphology, alloy nanoparticles (particle size of about 50nm) are uniformly loaded on the graphene nanosheet layer.

[0041] Example 2

[0042] A method for preparing a Fe-Co alloy / graphene oxide wave absorbing composite material comprises the following steps:

[0043] (1) 200 mg of graphene oxide was dispersed in 30 ml of deionized water, stirred for 2 hours, and ultrasonically dispersed for 20 minutes, and repeated 12 times to prepare a dispersion.

[0044] (2) Add 7.5 mmol of ferric acetate (1.45 g), 7.5 mmol of cobalt acetate (1.33 g), 200 mg of sodium carboxymethyl cellulose (CMC), 2.5 g of glucose, and 1 g of polyvinyl alcohol to the dispersion, heat to 60° C. in a water bath, and apply mechanical stirring at 500 rpm for 5 hours at the same temperature to obtain a mixed solution. The concentration of the metal acetate in the mixed solution is 0.5 mol / L.

[0045] (3) The mixed solution was rapidly frozen in liquid nitrogen for 8 hours and then freeze-dried for 96 hours to obtain a loose and porous carbon-based precursor.

[0046] (4) Under the protection of high-purity argon, the precursor was pre-carbonized at 500°C for 2 hours at a heating rate of 5°C / min, and then sintered at 750°C for 3 hours to obtain a Fe-Co alloy / graphene oxide absorbing composite material.

[0047] The Fe-Co alloy / graphene oxide absorbing composite material obtained in this example has a specific surface area of ​​65m 2 / g, the wave absorption performance is as follows Figure 3 As shown, the appearance is Figure 4 As shown. Figures 3-4 It can be seen that in terms of performance, the strongest reflection loss of the material can reach -24dB, and the effective absorption bandwidth (EAB, RL min <-10dB) can reach 5.22; in terms of morphology, the alloy nanoparticles (particle size of about 40nm) are uniformly loaded on the graphene nanosheets.

[0048] Example 3

[0049] A method for preparing a Ni-Co alloy / graphene oxide wave absorbing composite material comprises the following steps:

[0050] (1) 200 mg of graphene oxide was dispersed in 30 ml of deionized water, stirred for 2 hours, and ultrasonically dispersed for 20 minutes, and repeated 12 times to prepare a dispersion.

[0051] (2) Add 7.5 mmol nickel acetate (1.33 g), 7.5 mmol cobalt acetate (1.33 g), 200 mg sodium carboxymethyl cellulose (CMC), 2.5 g glucose, and 1 g polyvinyl alcohol to the dispersion, heat to 60° C. in a water bath, and apply mechanical stirring at 500 rpm for 5 hours at the same temperature to obtain a mixed solution. The concentration of the metal acetate in the mixed solution is 0.5 mol / L.

[0052] (3) The mixed solution was rapidly frozen in liquid nitrogen for 8 hours and then freeze-dried for 96 hours to obtain a loose and porous carbon-based precursor.

[0053] (4) Under the protection of high-purity argon, the precursor was pre-carbonized at 500°C for 2 hours at a heating rate of 5°C / min, and then sintered at 750°C for 3 hours to obtain a Ni-Co alloy / graphene oxide absorbing composite material.

[0054] The Ni-Co alloy / graphene oxide absorbing composite material obtained in this example has a specific surface area of ​​106m 2 / g, wave absorption performance Figure 5 As shown, the appearance is Figure 6 As shown. Figures 5-6 It can be seen that in terms of performance, the strongest reflection loss of the material can reach -67dB, and the effective absorption bandwidth (EAB, RL min <-10dB) can reach 5.58; in terms of morphology, the alloy nanoparticles (particle size is about 20nm) are uniformly loaded on the graphene nanosheets.

[0055] Example 4

[0056] A method for preparing a Fe-Ni-Co alloy / graphene oxide wave absorbing composite material comprises the following steps:

[0057] (1) 200 mg of graphene oxide was dispersed in 30 ml of deionized water, stirred for 2 hours, and ultrasonically dispersed for 20 minutes, and repeated 12 times to prepare a dispersion.

[0058] (2) Add 5 mmol nickel acetate (0.88 g), 5 mmol cobalt acetate (0.89 g), 5 mmol iron acetate (0.97 g), 200 mg sodium carboxymethyl cellulose (CMC), 2.5 g glucose, and 1 g polyvinyl alcohol to the dispersion, heat to 60° C. in a water bath, and apply mechanical stirring at 500 rpm for 5 hours at the same temperature to obtain a mixed solution. The concentration of the metal acetate in the mixed solution is 0.5 mol / L.

[0059] (3) The mixed solution was rapidly frozen in liquid nitrogen for 8 hours and then freeze-dried for 96 hours to obtain a loose and porous carbon-based precursor.

[0060] (4) Under the protection of high-purity argon, the precursor was pre-carbonized at 500°C for 2 hours at a heating rate of 5°C / min, and then sintered at 750°C for 3 hours to obtain a Fe-Ni-Co alloy / graphene oxide absorbing composite material.

[0061] The Fe-Ni-Co alloy / graphene oxide absorbing composite material obtained in this example has a specific surface area of ​​72 m 2 / g, wave absorption performance Figure 7 As shown, the appearance is Figure 8 As shown. Figures 7-8 It can be seen that in terms of performance, the strongest reflection loss of the material can reach -25dB, and the effective absorption bandwidth (EAB, RL min <-10dB) can reach 5.04; in terms of morphology, the alloy nanoparticles (particle size of about 30nm) are uniformly loaded on the graphene nanosheets.

[0062] Example 5

[0063] A method for preparing a Fe-Ni-Co alloy / graphene oxide wave absorbing composite material comprises the following steps:

[0064] (1) 200 mg of graphene oxide was dispersed in 30 ml of deionized water, stirred for 2 hours, and ultrasonically dispersed for 20 minutes, and repeated 12 times to prepare a dispersion.

[0065] (2) Add 2.5 mmol nickel acetate (0.44 g), 2.5 mmol cobalt acetate (0.45 g), 2.5 mmol iron acetate (0.49 g), 100 mg sodium carboxymethyl cellulose (CMC), 1.25 g glucose, and 0.5 g polyvinyl alcohol to the dispersion, heat to 40° C. in a water bath, and apply mechanical stirring at 400 rpm for 7 hours at the same temperature to obtain a mixed solution. The concentration of the metal acetate in the mixed solution is 0.25 mol / L.

[0066] (3) The mixed solution was rapidly frozen in liquid nitrogen for 12 hours and then freeze-dried for 72 hours to obtain a loose and porous carbon-based precursor.

[0067] (4) Under the protection of high-purity argon, the precursor was pre-carbonized at 450°C for 2 hours at a heating rate of 5°C / min, and then sintered at 700°C for 3 hours to obtain a Fe-Ni-Co alloy / graphene oxide absorbing composite material.

[0068] Example 6

[0069] A method for preparing a microwave-absorbing composite material based on graphene oxide comprises the following steps:

[0070] (1) 200 mg of graphene oxide was dispersed in 30 ml of deionized water, stirred for 2 hours, and ultrasonically dispersed for 20 minutes, and repeated 12 times to prepare a dispersion.

[0071] (2) Add 7.5 mmol nickel acetate (1.32 g), 7.5 mmol cobalt acetate (1.35 g), 7.5 mmol iron acetate (1.47 g), 300 mg sodium carboxymethyl cellulose (CMC), 3.75 g glucose, and 1.5 g polyvinyl alcohol to the dispersion, heat to 70° C. in a water bath, and apply mechanical stirring at 800 rpm for 4 hours at the same temperature to obtain a mixed solution. The concentration of the metal acetate in the mixed solution is 0.75 mol / L.

[0072] (3) The mixed solution was rapidly frozen in liquid nitrogen for 8 hours and then freeze-dried for 84 hours to obtain a loose and porous carbon-based precursor.

[0073] (4) Under the protection of high-purity argon, the precursor was pre-carbonized at 550°C for 2 hours at a heating rate of 5°C / min, and then sintered at 850°C for 3 hours to obtain a Fe-Ni-Co alloy / graphene oxide absorbing composite material.

[0074] Comparative Example 1

[0075] The remaining steps of this comparative example are the same as those of Example 3, except that PVA is not added. The results show that the specific surface area of ​​the material decreases, and the corresponding wave absorbing performance decreases.

[0076] Comparative Example 2

[0077] The remaining steps of this comparative example are the same as those of Example 3, except that glucose is not added. The results show that the tap density of the material increases, the specific surface area decreases, and the wave absorbing performance decreases.

[0078] Comparative Example 3

[0079] The remaining steps of this comparative example are the same as those of Example 3, except that freeze drying is replaced by drying. The results show that the material tap density increases, the particle size of the graphene nanosheet increases (and agglomerates), the specific surface area of ​​the material decreases, and the wave absorbing performance decreases significantly.

[0080] Among the above embodiments, the best embodiment is embodiment 3.

Claims

1. A method for preparing a microwave absorbing composite material based on graphene oxide, It is characterized in that The following steps are involved: Step 1, dispersing graphene oxide in deionized water to prepare a dispersion; Step 2, adding metal acetate, sodium carboxymethyl cellulose, glucose and polyvinyl alcohol to the dispersion, stirring in a water bath to obtain a mixed solution; Step 3, the mixed solution is first quickly frozen and then freeze-dried to obtain a loose and porous carbon-based precursor; Step 4: Under a protective atmosphere, the precursor is pre-carbonized and then sintered to obtain a graphene oxide-based microwave absorbing composite material.

2. The method for preparing the microwave absorbing composite material based on graphene oxide according to claim 1, Features: In the step 1, the graphene oxide is in the form of a sheet.

3. The method for preparing the microwave absorbing composite material based on graphene oxide according to claim 1, Features: In the step 1, the mass ratio of graphene oxide to deionized water is 1:100-500.

4. The method for preparing the microwave absorbing composite material based on graphene oxide according to claim 1, Features: In the step 2, the metal acetate is one or more of ferric acetate, nickel acetate, and cobalt acetate, and the concentration of the metal acetate in the mixed solution is 0.2-0.8 mol / L.

5. The method for preparing the microwave absorbing composite material based on graphene oxide according to claim 1, Features: In the step 2, the mass ratio of sodium carboxymethyl cellulose to graphene oxide is 0.5 to 1.5:

1.

6. The method for preparing the microwave absorbing composite material based on graphene oxide according to claim 1, Features: In the step 2, the mass ratio of metal acetate, sodium carboxymethyl cellulose, glucose and polyvinyl alcohol is 2.66-2.78:0.2:2.5:

1.

7. The method for preparing the microwave absorbing composite material based on graphene oxide according to claim 1, Features: In the step 2, the temperature of the water bath is 40-70° C., the stirring time is 4-7 hours, and the rotation speed is 400-800 rpm.

8. The method for preparing the microwave absorbing composite material based on graphene oxide according to claim 1, Features: In the step three, the rapid freezing is carried out in liquid nitrogen for 8 to 12 hours, and the freeze-drying time is 72 to 96 hours.

9. The method for preparing the microwave absorbing composite material based on graphene oxide according to claim 1, Features: In the step 4, the protective atmosphere is argon, the pre-carbonization temperature is 450-550°C, and the sintering temperature is 700-850°C.

10. A microwave absorbing composite material based on graphene oxide obtained by the method for preparing the microwave absorbing composite material based on graphene oxide according to any one of claims 1 to 9, Features: Its surface area is 65 to 10 m 2 / g, and the surface of the graphene oxide is uniformly loaded with metal nanoparticles with a particle size of 20 to 50 nm.