Phosphorescent OLED device with double-interface exciplex double-quantum well structure
By using MCP and B3PYMPM, CBP and B4PYMPM in green phosphorescence OLED devices to form a dual-interface excitation complex, the introduction of a dual quantum well structure is solved, and the problem of imbalance in hole and electron transmission is achieved with high efficiency green phosphorescence OLED devices .
Patent Information
- Application Number
- CN202411191266.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
In green phosphorescence OLED devices, holes and electron transport are unbalanced, resulting in too narrow composite areas and frequent exciton quenching, affecting device efficiency.
MCP and B3PYMPM, CBP and B4PYMPM are used as co-host materials to form a dual interface excitation composite with TADF effect, and a dual luminescent layer is introduced to form a dual quantum well to achieve carrier transmission balance and improve exciton utilization.
The internal quantum efficiency is achieved 100%, the composite region is widened, the exciton quenching phenomenon is reduced, and the efficiency and brightness of green phosphorescent OLED devices are significantly improved.
Smart Images

Figure CN119072142A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic electroluminescent devices, and in particular to a phosphorescent OLED device with a double-interface exciplex and double quantum well structure. The present invention forms two exciplexes and two quantum wells in the light-emitting layer of the green phosphorescent OLED device, which has an intermolecular TADF effect and broadens the recombination area. The present invention can provide a new idea for preparing a green phosphorescent OLED device with a simple structure and high efficiency. Background Art
[0002] Green phosphorescent OLED devices are organic light-emitting diodes (OLEDs) that use green phosphorescent materials as the light-emitting layer. This type of device mainly uses phosphorescence sensitization technology and the high quantum efficiency characteristics of green phosphorescent materials to achieve high-efficiency and high-brightness green light emission. The core of green phosphorescent OLED devices lies in the application of green phosphorescent materials. Phosphorescent materials can improve the luminous efficiency by capturing triplet excitons during the electroluminescence process. Green phosphorescent OLED devices have great potential in the fields of flat panel displays and solid-state lighting due to their high efficiency, high brightness and long life. With the deepening of research and technological breakthroughs, green phosphorescent OLEDs are expected to achieve further improvements in performance in the future, bringing people a richer and more realistic visual experience.
[0003] In phosphorescent OLEDs, in addition to the light-emitting layer, a suitable host material is also crucial. In OLED devices, hole and electron transport is unbalanced, holes have higher carrier mobility than electron transport materials, and carrier transport is unbalanced; the high exciton concentration under a narrow recombination area causes exciton quenching; since the excitons formed inside the light-emitting layer are composed of 25% singlet excitons and 75% triplet excitons, the triplet excitons in phosphorescent devices cannot be fully utilized, which will reduce device performance and affect device efficiency. Summary of the invention
[0004] The purpose of the present invention is to make up for the defects of the existing technology and provide a phosphorescent OLED device with a double-interface exciton complex and a double quantum well structure. The present invention can meet the charge transfer balance, improve the exciton utilization rate, and effectively reduce the exciton quenching phenomenon to achieve the purpose of high device efficiency. The present invention adds MCP and B3PYMPM; CBP and B4PYMPM as co-host materials to the light-emitting layer of the green phosphorescent OLED device to form a double-interface exciton complex with a TADF effect, introduces a double light-emitting layer to form a double quantum well, achieves 100% internal quantum efficiency, broadens the recombination area, and achieves carrier transmission balance, thereby improving the efficiency of the green phosphorescent OLED device. The present invention provides a new idea for preparing high-efficiency green phosphorescent OLED devices.
[0005] The present invention is achieved through the following technical solutions: A phosphorescent OLED device with a double-interface exciplex double quantum well structure, the phosphorescent OLED device comprises a light-emitting layer, the light-emitting layer comprises a host material and a guest light-emitting material, the host material is a double quantum well structure formed by two exciplex host materials, the two exciplex host materials are MCP and B3PYMPM and CBP and B4PYMPM.
[0006] The two exciplex main materials are 1,3-bis(carbazol-9-yl)benzene (1,3-Bis(carbazol-9-yl)benzene, Synonym: MCP) and B3PYMPM; 4,4-bis(9-carbazolyl)biphenyl (4,4'-Bis(N-carbazolyl)-1,1'-biphenyl, CBP) and B4PYMPM double interface exciplex main body to form a double quantum well structure, and the guest luminescent material is a green phosphorescent material Tris(2-phenylpyridinato-C2,N)iridium(III), Synonym: fac-Ir(ppy) 3 ).
[0007] The film thickness of the host material MCP is 15 nm; the film thickness of the host material CBP and B3PYMPM is 2-4 nm, and the ratio is 1:1 and remains unchanged; the film thickness of B4PYMPM is 40 nm; the light-emitting layer adopts an ultra-thin layer structure, and the guest light-emitting material fac-Ir(ppy) 3 The film thickness is 0.2nm.
[0008] The film thickness of the host material MCP is 15 nm; the film thickness of the host material CBP and B3PYMPM is 3 nm, and the ratio is 1:1 and remains unchanged; the film thickness of B4PYMPM is 40 nm; the guest material fac-Ir(ppy) 3 The film thickness is 0.2nm.
[0009] The guest luminescent material fac-Ir(ppy) of the phosphorescent OLED device 3 The light-emitting layer is formed on the ITO glass substrate by full evaporation; the main materials of the light-emitting layer CBP and B3PYMPM are co-evaporated at a constant rate.
[0010] In order to prepare a high-efficiency green phosphorescent OLED device, devices A and B were prepared for testing, where B was a control group. The preparation method of devices A and B includes the following steps: Device A: (ITO / MoO3(10nm) / TAPC(30nm) / MCP(15nm) / fac-Ir(ppy)3(0.2nm) / CBP:B3PYMPM, 1:1(3nm) / fac-Ir(ppy)3 (0.2 nm) / B4PYMPM(40 nm) / LiF(1 nm) / Al(100 nm)); The steps for device preparation are as follows: (1) Place the ITO glass substrate into an ultrasonic cleaner for ultrasonic cleaning; (2) Use a nitrogen gun to blow dry the cleaned ITO glass substrate, and then dry it on a hot table; (3) Treat the ITO glass substrate with UV ozone; (4) Place the ITO glass substrate after UV-ozone treatment on a customized substrate rack, then place it into the coating machine, and evacuate the interior of the coating machine chamber; (5) MoO was evaporated on the ITO-based glass substrate. 3 ,TAPC,MCP,fac-Ir(ppy) 3 , B3PYMPM: CBP, fac-Ir(ppy)3, B4PYMPM, LiF, Al, the ratio of the two main materials CBP and B3PYMPM in the light-emitting layer is 1:1, the film thickness is 3 nm, and the guest material is fac-Ir(ppy) 3 The film thickness is 0.2 nm, and then the coating machine is opened to take out the prepared device after the coating machine drops to a suitable temperature; (6) Packaging the prepared device; (7) Conduct performance tests on the prepared devices; Device B (Control): (ITO / MoO 3 (10 nm) / TAPC(30 nm) / MCP(15 nm) / fac-Ir(ppy) 3 (0.2 nm) / B4PYMPM(40 nm) / LiF(1 nm) / Al(100 nm)); The steps for device preparation are as follows: (1) Repeat steps (1), (2), (3), and (4) of device A; (2) MoO was deposited on the ITO glass substrate. 3 ,TAPC,MCP,fac-Ir(ppy)3,B4PYMPM,LiF,Al,light-emitting layer guest material fac-Ir(ppy) 3 The film thickness is 0.2 nm, and then the coating machine is turned on to take out the prepared device after the chamber temperature of the coating machine reaches the appropriate temperature; (3) Packaging the prepared device; (4) Conduct performance tests on the prepared devices; The principle of the present invention is: Two exciplex materials, MBP and B3PYMPM, are used simultaneously in the green phosphorescent device; CBP and B4PYMPM are used as the main body to form an interface exciplex, and a double light-emitting layer is introduced to form a double quantum well, which has the intermolecular TADF property, so that the triplet excitons can be converted into singlet states through reverse intersystem crossing, and the triplet excitons are effectively utilized to achieve 100% internal quantum efficiency. The double light-emitting layer double quantum well structure is used to broaden the recombination area of the light-emitting layer and reduce the exciton quenching phenomenon caused by exciton accumulation; the transmission balance of the light-emitting layer carriers is guaranteed. By comparing the efficiency of the green phosphorescent OLED device with a single interface exciplex as the main body, the efficiency of the double quantum well green phosphorescent OLED device with the addition of the double interface exciplex is greatly improved.
[0011] The advantages of the present invention are: The present invention adds MCP and B3PYMPM; CBP and B4PYMPM as co-host materials into the light-emitting layer of a green phosphorescent OLED device to form a double-interface exciplex with a TADF effect, introduces a double light-emitting layer to form a double quantum well, broadens the recombination area, achieves carrier transmission balance, and thus improves the efficiency of the green phosphorescent OLED device.
[0012] The present invention improves device performance by forming a quantum well structure through an interface exciton complex. The addition of a quantum well structure in the light-emitting layer of an OLED device makes the exciton recombination area wider. The quantum well structure can achieve a more balanced carrier transport. The ultra-thin interface exciton complex structure newly introduces an efficient reverse intersystem crossing process to improve the exciton utilization rate, thereby improving the luminous efficiency and brightness of the device to meet the needs of multiple fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is the energy level diagram of device A; Figure 2 is the energy level diagram of device B; Figure 3 is the structure diagram of device A; Figure 4 is the structural diagram of device B; Figure 5 The structure diagram of the light-emitting layer material of the device; Figure 6 Energy diagram of the device. DETAILED DESCRIPTION
[0014] like Figure 1 and 2As shown, a phosphorescent OLED device with a double-interface exciplex double quantum well structure includes a light-emitting layer with an interface exciplex as the main body, and the light-emitting layer is composed of a main material and a guest light-emitting material. Two exciplex main materials (MCP and B3PYMPM, CBP and B4PYMPM) are added to the light-emitting layer of the green phosphorescent OLED device to form a double quantum well structure.
[0015] like Figure 5 As shown, the light-emitting layer of the phosphorescent OLED device is selected from 1,3-bis(carbazol-9-yl)benzene (1,3-Bis(carbazol-9-yl)benzene, Synonym: MCP) and B3PYMPM; 4,4-bis(9-carbazolyl)biphenyl (4,4'-Bis(N-carbazolyl)-1,1'-biphenyl, CBP) and B4PYMPM double interface exciplex main body to form a double quantum well, and the green phosphorescent material is tris(2-phenylpyridinato-C2,N)iridium(III), Synonym: fac-Ir(ppy) 3 ) as the guest luminescent material.
[0016] The film thickness of the host material MCP is 15 nm; the film thickness of the host material CBP and B3PYMPM is 2-4 nm, and the ratio is 1:1 and remains unchanged; the film thickness of B4PYMPM is 40 nm; the light-emitting layer adopts an ultra-thin layer structure, and the guest material fac-Ir(ppy) 3 The film thickness is 0.2nm.
[0017] The film thickness of the host material MCP is 15 nm; the film thickness of the host materials CBP and B3PYMPM is preferably 3 nm, and the ratio is 1:1 and remains unchanged; the film thickness of B4PYMPM is 40 nm; the guest material fac-Ir(ppy) 3 The film thickness is 0.2nm.
[0018] Other functional layers and guest luminescent materials of phosphorescent OLED devices fac-Ir(ppy) 3 The light-emitting layers are formed on the ITO glass substrate by full evaporation; the light-emitting layers adopt an ultra-thin layer structure, and the main materials of the light-emitting layer CBP and B3PYMPM are co-evaporated at a constant rate to accurately control the doping concentration.
[0019] The following is a detailed description of the embodiments of the present invention. Based on the technical solution of the present invention, this embodiment provides a detailed implementation method and a specific operation process. The protection scope of the present invention includes but is not limited to the following embodiments.
[0020] To prepare device A: For a device with the structure of (ITO / MoO3(10nm) / TAPC(30nm) / MCP(15nm) / fac-Ir(ppy)3(0.2nm) / CBP:B3PYMPM, 1:1(3nm) / fac-Ir(ppy)3 (0.2 nm) / B4PYMPM(40 nm) / LiF(1 nm) / Al(100 nm)), the following steps are performed: (1) Cleaning of ITO glass substrate: The ITO glass substrate was placed in a beaker with ITO washing solution added and diluted with pure water. The beaker was then placed in an ultrasonic cleaner for 30 min of ultrasonic treatment, and then the pure water was replaced for 10 min of ultrasonic treatment.
[0021] (2) Drying of ITO glass substrate: The cleaned ITO glass substrate was blown dry with a high-purity nitrogen gun, and then placed in a constant temperature drying oven at 120°C for 900 seconds, and the substrate was placed in a mold for later use; (3) UV-ozone treatment of ITO glass substrate: The dried ITO glass substrate was taken out from the drying oven and placed in a UV ozone machine for 20 min to further remove organic matter adhering to the ITO glass substrate and improve the work function of the ITO surface; (4) Device preparation process: After the treatment in steps (1), (2), and (3), the ITO glass substrate treated with UV ozone was placed on a custom substrate rack and then placed in the evaporation chamber of the EvoVac ultrahigh vacuum coating machine. The valve of the chamber was closed and the evaporation chamber was evacuated. When the vacuum degree of the chamber was increased to 6.5×10 -6 Torr can start evaporation. Then evaporate the functional layers of the device in turn: MoO3, TAPC, MCP, [fac-Ir(ppy)3]2, B4PYMPM, LiF, Al, and the thickness of each film layer is 10 nm, 30nm, 15 nm, 0.2nm, 40 nm, 1nm, 100nm respectively. The rates of each layer are 0.5 Å / s, 1.2 Å / s, 1.0 Å / s, 0.02Å / s, 1.2 Å / s, 0.2 Å / s, 1.2Å / s; and the main materials of the light-emitting layer CBP and B3PYMPM, the evaporation rates are 0.2 Å / s and 0.06 Å / s, the ratio of CBP and B3PYMPM is 1:1, and the film thickness is 3nm. After the coating is completed, wait for the coating machine chamber to drop to the appropriate temperature, then open the coating machine and take out the prepared device. The energy transfer diagram of the device is shown in Figure 6 shown.
[0022] (5) Device packaging process: The device after evaporation was taken out, and the glass cover coated with UV curing adhesive was adhered to the device substrate using a prepared fixture in a glove box with a water and oxygen content of less than 1 ppm. The organic layer was shielded and irradiated under UV light for 3 min for curing.
[0023] (6) Perform performance test on the packaged device: To prepare control device B: (ITO / MoO 3 (10 nm) / TAPC(30 nm) / MCP(15 nm) / fac-Ir(ppy) 3 A device with a structure of (0.2 nm) / B4PYMPM(40 nm) / LiF(1 nm) / Al(100 nm)) is provided, wherein the steps of the present invention are as follows: (1) Repeat steps (1), (2), and (3) of preparing device A.
[0024] (2) Device preparation process: After the treatment in steps (1), (2), and (3), the ITO glass substrate treated with UV ozone was placed on a custom substrate rack and then placed in the evaporation chamber of the EvoVac ultrahigh vacuum coating machine. The valve of the chamber was closed and the evaporation chamber was evacuated. When the vacuum degree of the chamber was increased to 6.5×10 -6 Torr can start evaporation. Then evaporate the functional layers of the device in turn: MoO3, TAPC, MCP, fac-Ir(ppy)3, B4PYMPM, LiF, Al, the thickness of each film layer is 10 nm, 30 nm, 15 nm, 0.2nm, 40 nm, 1nm, 100nm. The rate of each layer is 0.5 Å / s, 1.2 Å / s, 1.0 Å / s, 0.02Å / s, 1.2Å / s, 0.2 Å / s, 1.2Å / s. After the coating is completed, wait for the coating machine chamber to drop to the appropriate temperature and then open the coating machine to take out the prepared device.
[0025] (3) Device packaging process: The device after evaporation was taken out, and the glass cover coated with UV curing adhesive was adhered to the device substrate using a prepared fixture in a glove box with a water and oxygen content of less than 1 ppm. The organic layer was shielded and irradiated under UV light for 3 min for curing.
[0026] (4) Perform performance test on the packaged device: The structures of device A and device B are as follows Figure 3 , 4As shown, device A has higher luminescence efficiency than device B with a single interface exciplex as the main body. Introducing a double quantum well structure with a double interface exciplex into a green phosphorescent OLED device helps to improve efficiency.
Claims
1. A phosphorescent OLED device with a double-interface exciplex double quantum well structure, the phosphorescent OLED device comprising a light-emitting layer, the light-emitting layer comprising a host material and a guest light-emitting material, characterized in that: The main body material is a double quantum well structure formed by two exciplex main body materials, wherein the two exciplex main body materials are MCP and B3PYMPM and CBP and B4PYMPM.
2. The phosphorescent OLED device with a double-interface exciplex double quantum well structure according to claim 1, characterized in that: The two exciplex main materials are 1,3-bis(carbazol-9-yl)benzene (1,3-Bis(carbazol-9-yl)benzene, Synonym: MCP) and B3PYMPM; 4,4-bis(9-carbazolyl)biphenyl (4,4'-Bis(N-carbazolyl)-1,1'-biphenyl, CBP) and B4PYMPM double interface exciplex main body forms a double quantum well structure, and the guest luminescent material is a green phosphorescent material Tris(2-phenylpyridinato-C2,N)iridium(III), Synonym: fac-Ir(ppy)3).
3. The phosphorescent OLED device with a double-interface exciplex double quantum well structure according to claim 1, characterized in that: The film thickness of the host material MCP is 15 nm; the film thickness of the host material CBP and B3PYMPM is 2-4 nm, and the ratio is 1:1 and remains unchanged; the film thickness of B4PYMPM is 40 nm; the light-emitting layer adopts an ultra-thin layer structure, and the film thickness of the guest light-emitting material fac-Ir(ppy)3 is 0.2 nm.
4. The phosphorescent OLED device with a double-interface exciplex double quantum well structure according to claim 3, characterized in that: The film thickness of the host material MCP is 15 nm; the film thickness of the host materials CBP and B3PYMPM is 3 nm, and the ratio is 1:1 and remains unchanged; the film thickness of B4PYMPM is 40 nm; and the film thickness of the guest material fac-Ir(ppy)3 is 0.2 nm.
5. The phosphorescent OLED device with a double-interface exciplex double quantum well structure according to claim 1, characterized in that: The guest luminescent material fac-Ir(ppy)3 luminescent layer of the phosphorescent OLED device is formed on an ITO glass substrate by full evaporation; the main materials of the luminescent layer CBP and B3PYMPM are co-evaporated at a constant rate.