Thin film and preparation method thereof, light-emitting device and preparation method thereof, and display device
By preparing and drying the electron transport layer of inorganic nanoparticles below room temperature, the agglomeration problem caused by temperature sensitivity is solved, and the film formation quality and device performance are improved.
Patent Information
- Application Number
- CN202310638006.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
Inorganic nanoparticles are extremely sensitive to temperature during film formation, and are prone to high-speed, directionless agglomeration due to excessive temperature, resulting in poor film formation quality, thereby reducing device efficiency.
The film precursor of the electron transport layer is prepared and dried at a temperature below room temperature, and the solvent is removed by gas blow-drying, the gas flow rate and drying time are controlled to avoid accelerated agglomeration at high temperatures.
Effectively reduce the agglomeration of inorganic nanoparticles, improve film formation quality, and improve device stability and luminous efficiency.
Smart Images

Figure CN119072199A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the display field, and in particular to a thin film and a preparation method thereof, a light-emitting device and a preparation method thereof, and a display device. Background Art
[0002] In recent years, the electron transport layer made by depositing a colloidal solution of inorganic nanoparticles has gradually become the main electron transport layer solution used in quantum dot light-emitting diodes. On the one hand, inorganic nanoparticles have excellent electron transport capabilities. On the other hand, inorganic nanoparticles have a good energy level matching relationship with the cathode and the quantum dot light-emitting layer, which significantly reduces the injection barrier of electrons from the cathode to the quantum dot light-emitting layer, and its deeper valence band energy level can effectively block holes. These characteristics make the electron transport layer made of inorganic nanoparticles the first choice for quantum dot light-emitting diode devices, significantly improving the stability and luminescence efficiency of the device.
[0003] However, while inorganic nanoparticles have excellent properties, they are also extremely sensitive to temperature. During the film-forming process, they are prone to high-speed, non-directional agglomeration due to excessively high temperatures, resulting in poor film quality and, in turn, reduced device efficiency. Summary of the invention
[0004] In view of this, the present application provides a thin film and a method for preparing the same, a light-emitting device and a method for preparing the same, and a display device to improve the film forming quality.
[0005] The present application provides a method for preparing a thin film, which comprises the following steps:
[0006] Providing a substrate, and forming a solution containing inorganic nanoparticles on the substrate at a first preset temperature to obtain a thin film precursor; and
[0007] Drying the film precursor at a second preset temperature to obtain the film;
[0008] Wherein, the first preset temperature and / or the second preset temperature is lower than room temperature.
[0009] Optionally, the first preset temperature and / or the second preset temperature is 0°C-10°C; and / or
[0010] The first preset temperature and the second preset temperature are equal.
[0011] Optionally, the step of drying the film precursor comprises: providing gas to blow dry the film precursor; and / or
[0012] The step of drying the film precursor comprises: providing an inert gas to blow dry the film precursor; and / or
[0013] The flow rate of the gas is 3m / s-14m / s; and / or
[0014] In the step of drying the film precursor, the drying time is more than 1 minute; and / or
[0015] In the step of drying the film precursor, the drying time is 1 min to 30 min; and / or
[0016] The forming of the solution containing inorganic nanoparticles on the substrate and the drying of the thin film precursor are performed under normal pressure.
[0017] Optionally, the solution containing inorganic nanoparticles further comprises a solvent, the mass fraction of the inorganic nanoparticles is 0.1%-20.0%; the mass fraction of the solvent is 80.0%-99.9%; and / or
[0018] The solvent comprises at least one of a saturated hydrocarbon solvent, an unsaturated hydrocarbon solvent, an aromatic hydrocarbon solvent, an alcohol solvent, an ether solvent, a ketone solvent, a nitrile solvent, and an ester solvent; and / or
[0019] The solvent includes at least one of methanol, ethanol, ethylene glycol, propanol, propylene glycol, glycerol, isopropanol, butanol, pentanol, hexanol, cyclohexanol, n-butanol, benzyl alcohol, phenylethyl alcohol, and acetonitrile.
[0020] Optionally, the average particle size of the inorganic nanoparticles is 2 to 20 nm; and / or
[0021] The inorganic nanoparticles are selected from at least one of metal oxides, doped metal oxides, II-VI semiconductor materials, III-V semiconductor materials and I-III-VI semiconductor materials; the metal oxides are selected from ZnO, BaO, TiO 2 SnO 2 At least one of the following; the metal oxide in the doped metal oxide is selected from ZnO, TiO 2 SnO 2 At least one of the doping elements may be selected from at least one of Al, Mg, Li, In, and Ga; the II-VI semiconductor material may be selected from at least one of ZnS, ZnSe, and CdS; the III-V semiconductor material may be selected from at least one of InP and GaP; the I-III-VI semiconductor material may be selected from at least one of CuInS and CuGaS.
[0022] The present application also provides a film, which is prepared by any of the above-mentioned film preparation methods.
[0023] The present application also provides a method for preparing a light-emitting device, which comprises the following steps:
[0024] Providing a light-emitting device preform, wherein the light-emitting device preform comprises a bottom electrode;
[0025] Using the above-mentioned thin film preparation method to prepare a thin film on the light-emitting device preform to obtain an electron transport layer; and
[0026] forming a top electrode on the electron transport layer to obtain a light-emitting device;
[0027] Wherein, the bottom electrode is a cathode, the top electrode is an anode, and before forming the top electrode on the electron transport layer, the method further includes: forming a light-emitting layer on the electron transport layer; or
[0028] The bottom electrode is an anode, the top electrode is a cathode, and the substrate further includes a light-emitting layer formed on the bottom electrode.
[0029] The present application also provides a light-emitting device, which is prepared by the above-mentioned method for preparing a light-emitting device.
[0030] Optionally, the bottom electrode and the top electrode are independently selected from a doped metal oxide particle electrode, a composite electrode, a graphene electrode, a carbon nanotube electrode, a metal element electrode or an alloy electrode, the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide, and the composite electrode is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO 2 / Ag / TiO 2 、TiO 2 / Al / TiO 2 , ZnS / Ag / ZnS or ZnS / Al / ZnS, wherein the material of the metal electrode is selected from one or more of Ag, Al, Cu, Au, Mo, Pt, Ca and Ba; and / or
[0031] The material of the light-emitting layer is selected from one or more quantum dot light-emitting materials, the quantum dot light-emitting material is selected from one or more single-structure quantum dots, core-shell quantum dots and perovskite semiconductor materials, the material of the single-structure quantum dots, the core material of the core-shell quantum dots and the shell material of the core-shell quantum dots are respectively selected from at least one of the single-structure quantum dots selected from II-VI compounds, IV-VI compounds, III-V compounds and I-III-VI compounds, the II-VI compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, Zn O, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, C At least one of dHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, The IV-VI group compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe; the III-V group compound is selected from at least one of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, At least one of GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, wherein the I-III-VI group compound is selected from CuInS 2 、CuInSe 2 AgInS 2 At least one of the following, the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors, and the inorganic perovskite semiconductor has a general structural formula of AMX 3 , where A is Cs+ ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the organic-inorganic hybrid perovskite semiconductors has a general structural formula of BMX 3 , wherein B is an organic amine cation selected from CH 3 (CH 2 ) n-2 NH 3 + or [NH 3 (CH 2 ) n NH 3 ] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .
[0032] The present application also provides a display device, which includes the light-emitting device as described in any one of the above items.
[0033] According to the thin film and its preparation method, light-emitting device and its preparation method and display device of the embodiments of the present application, the thin film precursor of the electron transport layer is prepared and / or the thin film precursor is dried at a temperature below room temperature, which can reduce the agglomeration of inorganic nanoparticles and thus improve the film quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solution in the present application, the following is a brief introduction to the drawings required for the description of the implementation methods. Obviously, the drawings described below are only some implementation methods of the present application. For those skilled in the art, without paying creative work, they can also
[0035] Figure 1 This is a step diagram of a method for preparing a thin film according to an embodiment of the present application.
[0036] Figure 2 This is a step diagram of a method for preparing a light-emitting device according to an embodiment of the present application.
[0037] Figure 3 This is a schematic diagram of the structure of the light-emitting device of some embodiments of the present application.
[0038] Figure 4 Schematic diagrams of the structures of light-emitting devices according to other embodiments of the present application.
[0039] Figure 5 Schematic diagram of the structure of a display device according to an embodiment of the present application. DETAILED DESCRIPTION
[0040] The technical solution in this application will be described clearly and completely below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.
[0041] In the present application, unless otherwise expressly specified and limited, the first feature "above" or "below" the second feature may include the first and second features directly, or may include the first and second features not being directly connected but being in contact through another feature between them. Moreover, the first feature "above", "above" and "above" the second feature include the first feature being directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. The first feature "below", "below" and "below" the second feature include the first feature being directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features.
[0042] The inventors made the following discoveries during their research on the phenomenon of poor film formation of inorganic nanoparticles:
[0043] A known method for forming an electron transport layer is a spin coating method in a solution method, that is, a solution containing inorganic nanoparticles is dripped onto a substrate rotating at a high speed, and the solution dripped onto the substrate is uniformly coated on the substrate by centrifugal force. Depending on the thickness of the film to be manufactured, the rotation speed of the substrate can be adjusted for different solutions. After spin coating, the substrate coated with inorganic nanoparticles is placed on a heating platform, and the solution is heated to evaporate rapidly to form a film, thereby obtaining an electron transport layer.
[0044] However, inorganic electron transport layer materials, such as zinc oxide, are extremely temperature-sensitive materials, and their daily storage temperature is -18°C. The spin coating temperature is around 25°C, and the zinc oxide solution drips out from the liquid gun. Due to the high ambient temperature, the zinc oxide solution heats up rapidly, and the agglomeration rate increases as the temperature rises. The agglomeration of zinc oxide will directly affect the spin coating film formation effect, for example, causing uneven film formation and agglomeration to form large particles. The uneven interface caused by zinc oxide agglomeration may cause display anomalies such as white spots. Poor film formation will further affect the carrier injection balance of the device, ultimately leading to poor device performance.
[0045] In addition, the method of removing the solvent from the film layer after spin coating is high-temperature baking. This method only considers the rapid volatilization of the solvent and ignores the effect of high temperature on film formation, especially the effect on zinc oxide. High temperature will accelerate the agglomeration of zinc oxide particles. The temperature of high-temperature baking is 50-90°C. Excessively high post-treatment temperature further increases the agglomeration rate of zinc oxide, causing the already agglomerated points to expand rapidly. At the same time, the inventors also found that the solvent forms an interfacial hot air flow during the upward volatilization process. The upward hot air flow will also exert an upward force on the zinc oxide particles, thereby causing the interface of the adjacent film layer to become larger. The increase in the distance between the film layers will cause the conduction band energy level to become larger, resulting in unbalanced carrier injection and thus affecting the device performance.
[0046] In order to solve the above problems, the present application provides a method for preparing a thin film for manufacturing an electron transport layer of a QLED. Figure 1 , the method for preparing the film comprises the following steps:
[0047] S1: providing a substrate, and forming a solution containing inorganic nanoparticles on the substrate at a first preset temperature to obtain a thin film precursor.
[0048] The substrate may be a substrate for electrode preparation known in the art or a light emitting device preform.
[0049] The substrate may be a rigid substrate or a flexible substrate. In some embodiments, the material of the substrate may be selected from but not limited to at least one of glass, silicon wafer, polycarbonate, polymethyl methacrylate, polyethylene terephthalate, polyethylene naphthalate, polyamide and polyether sulfone.
[0050] The light emitting device preform comprises a bottom electrode and a functional layer which are stacked.
[0051] In some embodiments, the bottom electrode is an anode. The functional layer includes a carrier functional layer and at least one of a hole injection layer, a hole transport layer and a light emitting layer. This embodiment can be used to manufacture a vertical QLED device.
[0052] In other embodiments, the bottom electrode is a cathode. The functional layer includes an electron injection layer. This embodiment can be used to manufacture an inverted QLED device.
[0053] The functional layers in the light emitting device preform can be prepared by conventional methods, such as the solution method described below.
[0054] The bottom electrode can be an electrode known in the art for light-emitting devices, for example, it can be selected from but not limited to a doped metal oxide particle electrode, a composite electrode of a metal and a metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode. The material of the doped metal oxide particle electrode can be selected from but not limited to one or more of indium-doped tin oxide (ITO), fluorine-doped tin oxide (FTO), antimony-doped tin oxide (ATO), aluminum-doped zinc oxide (AZO), gallium-doped zinc oxide (GZO), indium-doped zinc oxide (IZO), magnesium-doped zinc oxide (MZO) and aluminum-doped magnesium oxide (AMO). The composite electrode is a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxide particles, such as AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO 2 / Ag / TiO 2 、TiO 2 / Al / TiO 2 , ZnS / Ag / ZnS, ZnS / Al / ZnS, etc. The material of the metal electrode can be selected from but not limited to one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba. Wherein, " / " represents a stacked structure, for example, AZO / Ag / AZO represents a composite electrode including an AZO layer, an Ag layer and an AZO layer stacked in sequence.
[0055] The material of the hole injection layer can be a material known in the art for the hole injection layer, for example, can be selected from but not limited to 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HAT-CN), PEDOT, PEDOT:PSS, PEDOT:PSS doped with s-MoO 3 Derivatives (PEDOT:PSS:s-MoO 3), 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), tetracyanoquinodimethane (F4-TCQN), copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and at least one of copper oxide.
[0056] The material of the hole transport layer can be a material known in the art for the hole transport layer, for example, it can be selected from but not limited to 4,4'-N,N'-dicarbazolyl-biphenyl (CBP), N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine (α-NPD), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenylene)- yl)-spiro (spiro-TPD), N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine (DNTPD), 4,4',4'-tri(N-carbazolyl)-triphenylamine (TCTA), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))] (TFB), Poly(4-butylphenyl-diphenylamine) (poly-TPD), polyaniline, polypyrrole, poly(p-phenylene vinylene), poly(phenylene vinylene) (PPV), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] (MEH-PPV) and poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene] (MOMO-PPV), copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)- 1,1'-biphenyl compounds, N,N,N',N'-tetraaryl benzidine, PEDOT:PSS and its derivatives, poly(N-vinyl carbazole) (PVK) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine (NPB), spiro NPB, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO 3 , doped or undoped WO 3 , doped or undoped V 2 O 5 , doped or undoped P-type GaN, doped or undoped CrO 3 , doped or undoped CuO.
[0057] The material of the light-emitting layer is selected from one or more quantum dot light-emitting materials, the quantum dot light-emitting materials are selected from one or more of single structure quantum dots, core-shell structure quantum dots and perovskite semiconductor materials, the material of the single structure quantum dots, the core material of the core-shell structure quantum dots and the shell material of the core-shell structure quantum dots are respectively selected from at least one of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds, and the II-VI group compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, Hg Te, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZn At least one of S, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, group IV-VI The compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe, and the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, and GaPA At least one of GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, and the I-III-VI group compound is selected from CuInS 2 、CuInSe 2 AgInS 2 At least one of the perovskite semiconductor materials is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors. The general structural formula of the inorganic perovskite semiconductor is AMX 3 , where A is Cs + ion, M is a divalent metal cation selected from Pb2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following. The general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX 3 , wherein B is an organic amine cation selected from CH 3 (CH 2 ) n-2 NH 3 + or [NH 3 (CH 2 ) n NH 3 ] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .
[0058] The material of the electron injection layer may be selected from, but not limited to, at least one of cesium carbonate, cesium fluoride, cesium azide and lithium fluoride.
[0059] The inorganic nanoparticles may be materials known in the art for use in electron transport layers, for example, may be selected from but not limited to at least one of metal oxides, doped metal oxides, II-VI semiconductor materials, III-V semiconductor materials, and I-III-VI semiconductor materials. Specifically, the metal oxide may be selected from but not limited to ZnO, BaO, TiO 2 SnO 2, at least one of; the metal oxide in the doped metal oxide may be selected from but not limited to ZnO, TiO 2 SnO 2 At least one of the doping elements can be selected from but not limited to at least one of Al, Mg, Li, In, and Ga. For example, the doped metal oxide can be aluminum zinc oxide (AZO), lithium-doped zinc oxide (LZO), and magnesium-doped zinc oxide (MZO). The II-VI semiconductor family materials can be selected from but not limited to at least one of ZnS, ZnSe, and CdS. The III-V semiconductor family materials can be selected from but not limited to at least one of InP and GaP. The I-III-VI semiconductor materials can be selected from but not limited to at least one of CuInS and CuGaS.
[0060] The inorganic nanoparticles may be, depending on their morphology, at least one of inorganic semiconductor nanoparticles, inorganic semiconductor nanosheets, and inorganic semiconductor nanowires, but are not limited thereto.
[0061] In some embodiments, the average particle size of the inorganic semiconductor particles is 2-20 nm, such as 2-8 nm, 5-15 nm, 8-20 nm, 2-10 nm, etc. Within the particle size range, the inorganic semiconductor particles are easy to synthesize and have good uniformity, and can also make the film layer of the electron transport layer uniform and flat.
[0062] The method of forming a thin film precursor by forming a solution containing inorganic nanoparticles on a substrate may be a solution method. The solution method may be a spin coating method, a printing method, an inkjet printing method, a doctor blade method, a printing method, a dip-coating method, a soaking method, a spray coating method, a roll coating method, a casting method, a slit coating method, a strip coating method, and the like.
[0063] The solution containing inorganic nanoparticles also includes a solvent. The solvent includes one or more of saturated hydrocarbons, unsaturated hydrocarbons, aromatic hydrocarbons, alcohol solvents, ether solvents, ketone solvents, nitrile solvents, ester solvents, and derivatives thereof. The solvent is preferably an alcohol solvent, including but not limited to one or more of monohydric alcohols, polyhydric alcohols, and aromatic alcohols, specifically including but not limited to one or more of methanol, ethanol, ethylene glycol, propanol, propylene glycol, glycerol, isopropanol, butanol, amyl alcohol, hexanol, cyclohexanol, n-butanol, benzyl alcohol, and phenylethyl alcohol. Taking the total weight of the solution containing inorganic nanoparticles as 100%, the weight percentage of the inorganic nanoparticles is 0.1-20.0%; the weight percentage of the solvent is 80.0-99.9%.
[0064] The film precursor is called a film precursor because the film layer formed on the substrate with a solution containing inorganic nanoparticles is still in a semi-solid and semi-solution state and needs to be further removed from the solvent.
[0065] Optionally, the first preset temperature is lower than room temperature. Further, the first preset temperature is in the range of 0°C-10°C. Specifically, the first preset temperature may be 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C or 10°C. By forming the thin film precursor at a temperature lower than room temperature, the agglomeration rate of inorganic nanoparticles during the formation of the thin film precursor can be effectively reduced, and the stability of the particle dispersion can be improved, thereby improving the uniformity of film formation. It should be noted that when the temperature is lower than 0°C, the solution spreading film forming rate will be affected, thereby affecting the film forming effect. When the temperature is higher than 10°C, the agglomeration rate of inorganic nanoparticles will increase. Optionally, the first preset temperature is in the range of 3°C-8°C, and the film forming quality is better.
[0066] In addition, it should be noted that the instruments used in the solution method, such as the spin coater, do not have a temperature control function. The instrument can be improved to have a temperature control function or the ambient temperature can be kept at a low temperature through a pipeline connection.
[0067] In some embodiments of the present application, the first preset temperature may also be room temperature. Specifically, the first preset temperature may be 25°C.
[0068] S2: Drying the film precursor at a second preset temperature to obtain a film.
[0069] Optionally, the second preset temperature is lower than room temperature. Further, the second preset temperature is in the range of 0°C-10°C. The second preset temperature can be 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C or 10°C. By lowering the drying temperature of the thin film precursor, the agglomeration of inorganic nanoparticles in the thin film precursor can be reduced, and the interfacial hot air flow formed during the upward volatilization of the solvent can also be alleviated, causing the interface of adjacent film layers to become larger, and the distance between the film layers will increase, which will cause the conduction band energy level to become larger, resulting in unbalanced carrier injection and thus affecting the performance of the device. It should be noted that when the temperature is lower than 0°C, it will affect the volatilization rate of the solvent. When the temperature is higher than 10°C, the agglomeration rate of inorganic nanoparticles will increase. Optionally, the second preset temperature is in the range of 3°C-8°C, and the film quality is better.
[0070] In the method for preparing the thin film of the present application, one of the first preset temperature and the second preset temperature may be within the range of 0° C. to 10° C. Optionally, both the first preset temperature and the second preset temperature are within the range of 0° C. to 10° C.
[0071] Optionally, the first preset temperature and the second preset temperature are equal.
[0072] Optionally, the step of drying the film precursor includes: providing gas to blow dry the film precursor. Under the premise of ensuring a relatively low ambient temperature, the film layer solvent is removed by blowing with gas, firstly, annealing is not required, and the agglomeration rate of inorganic nanoparticles accelerated by annealing is reduced, and the agglomeration of inorganic nanoparticles accelerated by high temperature can be avoided; secondly, the influence of high temperature on the film layer can be avoided; thirdly, the water and oxygen on the surface of the residual film layer can be further removed.
[0073] Optionally, the gas is an inert gas. The inert gas may be nitrogen or argon. Since the inorganic nanoparticles are sensitive to water and oxygen, using an inert gas for drying can prevent them from being affected by water and oxygen and causing performance degradation.
[0074] Optionally, the gas flow rate is 3m / s-14m / s. When the gas flow rate is controlled within this range, it can help the solvent evaporate to form a film, and will not damage the film layer due to excessively high flow rate.
[0075] Optionally, in the step of drying the film precursor, the drying time is 1 min or longer. A dry film can be obtained with a minimum drying time of 1 min. It is understood that the processing time can also be extended. Specifically, the drying time is 1 min or longer and 30 min or shorter.
[0076] Optionally, the above steps are all performed under a standard atmospheric pressure. Of course, they can also be performed in an atmosphere higher or lower than a standard atmospheric pressure as required.
[0077] The present application also provides a film, which is prepared by the above-mentioned film preparation method.
[0078] Please refer to Figure 2 The present application also provides a method for preparing a light-emitting device, which comprises the following steps:
[0079] S11: providing a light-emitting device preform, wherein the light-emitting device preform comprises a bottom electrode, and forming a solution containing inorganic nanoparticles on the light-emitting device preform at a first preset temperature to obtain a thin film precursor.
[0080] The light emitting device preform, bottom electrode, first preset temperature, inorganic nanoparticles, thin film precursor and the formation method thereof in step S11 can all refer to step S1, and the description thereof is omitted here.
[0081] S12: Drying the thin film precursor at a second preset temperature to obtain an electron transport layer.
[0082] The second preset temperature in step S11 and the drying method of the thin film precursor may refer to step S2 , and the description thereof is omitted here.
[0083] S13: forming a top electrode on the light-emitting layer to obtain a light-emitting device.
[0084] When the bottom electrode in step S11 is a cathode, the top electrode in step S13 is an anode, and before step S13, it also includes: forming a light-emitting layer on the electron transport layer, or when the bottom electrode in step S11 is an anode, the top electrode in step S13 is a cathode, and the substrate also includes a light-emitting layer formed on the bottom electrode. The material selection of the light-emitting layer can refer to step S1, and the material of the top electrode can refer to the material of the bottom electrode in step S1, and can be selected according to needs.
[0085] In the method for preparing the thin film light emitting device of the present application, one of the first preset temperature and the second preset temperature can be within the range of 0°C-10°C. Optionally, both the first preset temperature and the second preset temperature are within the range of 0°C-10°C.
[0086] Optionally, the step of drying the film precursor includes: drying the film precursor with gas. The solvent can be quickly removed by air flow at low temperature, and annealing is not required to avoid annealing to accelerate the agglomeration rate of zinc oxide.
[0087] Optionally, the gas is an inert gas. The inert gas may be nitrogen or argon. Since the inorganic nanoparticles are sensitive to water and oxygen, using an inert gas for drying can prevent them from being affected by water and oxygen and causing performance degradation.
[0088] Optionally, the gas flow rate is 3m / s-14m / s. When the gas flow rate is controlled within this range, it can help the solvent evaporate to form a film, and will not damage the film layer due to excessively high flow rate.
[0089] Optionally, in the step of drying the film precursor, the drying time is 1 min or longer. A dry film can be obtained with a minimum drying time of 1 min. It is understood that the processing time can also be extended. Specifically, the drying time is 1 min or longer and 30 min or shorter.
[0090] Optionally, after step S14, the following steps may also be included:
[0091] A layer of packaging glue is covered on the top electrode to isolate the device from corrosion by water and oxygen. The packaging glue is a resin glue, such as acrylic resin or epoxy resin.
[0092] The present application also provides a light-emitting device, which is prepared by the above-mentioned method for preparing the light-emitting device.
[0093] See also Figure 3 In some embodiments, the light emitting device 100 includes a bottom electrode 10, a hole injection layer 20, a hole transport layer 30, a light emitting layer 40, an electron transport layer 50, an electron injection layer 60 and a top electrode 70 which are sequentially stacked. The bottom electrode 10 is an anode and the top electrode 70 is a cathode.
[0094] See also Figure 4 In some embodiments, the light emitting device 200 includes a bottom electrode 210, an electron injection layer 260, an electron transport layer 250, a light emitting layer 240, a hole transport layer 230, a hole injection layer 220, and a top electrode 270, which are sequentially stacked. The bottom electrode 210 is a cathode, and the top electrode 270 is an anode.
[0095] The materials of the various film layers of the light emitting device 100 / 200 are as described above and will not be described in detail here.
[0096] Some film layers in the light emitting device 100 / 200 are omitted as required and will not be described in detail here.
[0097] Please refer to Figure 5 The present application also provides a display device 1 , which includes a light-emitting device 100 .
[0098] The display device 1 can be any electronic product with a display function, including but not limited to smart phones, tablet computers, laptops, digital cameras, digital video cameras, smart wearable devices, smart weighing electronic scales, car displays, televisions or e-book readers, among which the smart wearable devices can be, for example, smart bracelets, smart watches, virtual reality (VR) helmets, etc.
[0099] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.
[0100] Example 1
[0101] In the manufacturing process of the light emitting device, zinc oxide is spin-coated at low temperature and the solvent is removed by nitrogen at room temperature. Other functional layers are spin-coated at room temperature and the solvent is removed at room temperature. Other functional layers refer to functional layers other than the bottom electrode and the top electrode.
[0102] The specific steps are as follows:
[0103] S1: Spin coat a PEDOT:PSS hole injection layer on the ITO substrate at a rotation speed of 3000 r / min, a solution concentration of 15 mg / ml, a duration of 40 s, a thickness of 40 nm, and a processing temperature of 25 °C.
[0104] S2: placing the intermediate device with the hole injection layer formed thereon on a desolvation station for desolvation treatment by introducing nitrogen gas at a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 25°C.
[0105] S3: A layer of TFB is prepared on the hole injection layer as a hole transport layer, with a rotation speed of 3000 r / min, a solution concentration of 8 mg / ml, a duration of 40 s, a thickness of 35 nm, and a processing temperature of 25°C.
[0106] S4: placing the intermediate device with the hole transport layer formed thereon on a desolvation station for desolvation treatment, wherein the inlet gas is nitrogen gas, the gas flow rate is 7 m / s, the treatment time is 1 min, and the treatment temperature is 25°C.
[0107] S5: Spin-coat a layer of CdSe@ZnS on the hole transport layer as a quantum dot light-emitting layer, with a rotation speed of 2000 r / min, a solution concentration of 12.5 mg / ml, a duration of 40 s, a thickness of 30 nm, and a processing temperature of 25°C.
[0108] S6: placing the intermediate device with the quantum dot light-emitting layer formed thereon on a desolvation table for desolvation treatment. The treatment method is to introduce nitrogen gas, with a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 25°C.
[0109] S7: Spin coat a layer of ZnO as an electron transport layer on the quantum dot light-emitting layer, the rotation speed is 2000r / min, the solution concentration is 12.5mg / ml, the solvent is n-butanol, the time is 40s, the thickness is 50nm, and the spin coating temperature is 0℃.
[0110] S8: placing the intermediate device with the electron transport layer formed thereon on a desolvation station for desolvation treatment by introducing nitrogen gas at a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 25°C.
[0111] S9: evaporating an Al electrode on the electron transport layer.
[0112] S10: A layer of encapsulation glue is covered on the Al electrode to obtain an inverted structure QLED device.
[0113] Example 2
[0114] In the manufacturing process of the light emitting device of Example 2, zinc oxide is spin-coated at low temperature, and the solvent is removed by nitrogen at low temperature. Other functional layers are spin-coated at room temperature and the solvent is removed at room temperature.
[0115] S1: Spin coat a PEDOT:PSS hole injection layer on the ITO substrate at a rotation speed of 3000 r / min, a solution concentration of 15 mg / ml, a duration of 40 s, a thickness of 40 nm, and a processing temperature of 25 °C.
[0116] S2: placing the intermediate device with the hole injection layer formed thereon on a desolvation station for desolvation treatment by introducing nitrogen gas at a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 25°C.
[0117] S3: A layer of TFB is prepared on the hole injection layer as a hole transport layer, with a rotation speed of 3000 r / min, a solution concentration of 8 mg / ml, a duration of 40 s, a thickness of 35 nm, and a processing temperature of 25°C.
[0118] S4: placing the intermediate device with the hole transport layer formed thereon on a desolvation station for desolvation treatment, wherein the inlet gas is nitrogen gas, the gas flow rate is 7 m / s, the treatment time is 1 min, and the treatment temperature is 25°C.
[0119] S5: Spin-coat a layer of CdSe@ZnS on the hole transport layer as a quantum dot light-emitting layer, with a rotation speed of 2000 r / min, a solution concentration of 12.5 mg / ml, a duration of 40 s, a thickness of 30 nm, and a processing temperature of 25°C.
[0120] S6: placing the intermediate device with the quantum dot light-emitting layer formed thereon on a desolvation table for desolvation treatment. The treatment method is to introduce nitrogen gas, with a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 25°C.
[0121] S7: Spin coat a layer of ZnO as an electron transport layer on the quantum dot light-emitting layer, the rotation speed is 2000r / min, the solution concentration is 12.5mg / ml, the solvent is n-butanol, the time is 40s, the thickness is 50nm, and the spin coating temperature is 0℃.
[0122] S8: placing the intermediate device with the electron transport layer formed thereon on a desolvation station for desolvation treatment by introducing nitrogen gas at a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 0°C.
[0123] S9: evaporating an Al electrode on the electron transport layer.
[0124] S10: A layer of encapsulation glue is covered on the Al electrode to obtain an inverted structure QLED device.
[0125] Example 3
[0126] In the manufacturing process of the light emitting device of Example 3, zinc oxide is spin-coated at low temperature, and the solvent is removed by nitrogen at low temperature. Other functional layers are spin-coated at room temperature and the solvent is removed at high temperature.
[0127] The specific steps are as follows:
[0128] S1: Spin coat a PEDOT:PSS hole injection layer on the ITO substrate at a rotation speed of 3000 r / min, a solution concentration of 15 mg / ml, a duration of 40 s, a thickness of 40 nm, and a processing temperature of 25 °C.
[0129] S2: placing the intermediate device with the hole injection layer formed thereon on a desolventizing station for desolventizing treatment. The treatment method is high temperature drying, and the treatment temperature is 90°C.
[0130] S3: A layer of TFB is prepared on the hole injection layer as a hole transport layer, with a rotation speed of 3000 r / min, a solution concentration of 8 mg / ml, a duration of 40 s, a thickness of 35 nm, and a processing temperature of 25°C.
[0131] S4: placing the intermediate device with the hole transport layer formed thereon on a desolvation station for desolvation treatment, wherein the treatment method is to introduce nitrogen gas, the gas flow rate is 7 m / s, the treatment time is 1 min, and the treatment temperature is 90°C.
[0132] S5: Spin-coat a layer of CdSe@ZnS on the hole transport layer as a quantum dot light-emitting layer, with a rotation speed of 2000 r / min, a solution concentration of 12.5 mg / ml, a duration of 40 s, a thickness of 30 nm, and a processing temperature of 25°C.
[0133] S6: placing the intermediate device with the quantum dot light-emitting layer formed thereon on a desolvation table for desolvation treatment. The treatment method is to introduce nitrogen gas, with a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 90°C.
[0134] S7: Spin coat a layer of ZnO as an electron transport layer on the quantum dot light-emitting layer, the rotation speed is 2000r / min, the solution concentration is 12.5mg / ml, the solvent is n-butanol, the time is 40s, the thickness is 50nm, and the spin coating temperature is 0℃.
[0135] S8: placing the intermediate device with the electron transport layer formed thereon on a desolvation station for desolvation treatment by introducing nitrogen gas at a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 0°C.
[0136] S9: evaporating an Al electrode on the electron transport layer.
[0137] S10: A layer of encapsulation glue is covered on the Al electrode to obtain an inverted structure QLED device.
[0138] Example 4
[0139] In the manufacturing process of the light emitting device of Example 4, zinc oxide is spin-coated at room temperature, and the solvent is removed by nitrogen at low temperature. Other functional layers are spin-coated at room temperature and the solvent is removed by nitrogen at high temperature.
[0140] The specific steps are as follows:
[0141] S1: Spin coat a PEDOT:PSS hole injection layer on the ITO substrate at a rotation speed of 3000 r / min, a solution concentration of 15 mg / ml, a duration of 40 s, a thickness of 40 nm, and a processing temperature of 25 °C.
[0142] S2: placing the intermediate device with the hole injection layer formed thereon on a desolventizing station for desolventizing treatment. The treatment method is high temperature drying, and the treatment temperature is 90°C.
[0143] S3: A layer of TFB is prepared on the hole injection layer as a hole transport layer, with a rotation speed of 3000 r / min, a solution concentration of 8 mg / ml, a duration of 40 s, a thickness of 35 nm, and a processing temperature of 25°C.
[0144] S4: placing the intermediate device with the hole transport layer formed thereon on a desolvation station for desolvation treatment, wherein the treatment method is to introduce nitrogen gas, the gas flow rate is 7 m / s, the treatment time is 1 min, and the treatment temperature is 90°C.
[0145] S5: Spin-coat a layer of CdSe@ZnS on the hole transport layer as a quantum dot light-emitting layer, with a rotation speed of 2000 r / min, a solution concentration of 12.5 mg / ml, a duration of 40 s, a thickness of 30 nm, and a processing temperature of 25°C.
[0146] S6: placing the intermediate device with the quantum dot light-emitting layer formed thereon on a desolvation table for desolvation treatment. The treatment method is to introduce nitrogen gas, with a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 90°C.
[0147] S7: Spin coat a layer of ZnO as an electron transport layer on the quantum dot light-emitting layer, the rotation speed is 2000r / min, the solution concentration is 12.5mg / ml, the solvent is n-butanol, the time is 40s, the thickness is 50nm, and the spin coating temperature is 25℃.
[0148] S8: placing the intermediate device with the electron transport layer formed thereon on a desolvation station for desolvation treatment by introducing nitrogen gas at a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 0°C.
[0149] S9: evaporating an Al electrode on the electron transport layer.
[0150] S10: A layer of encapsulation glue is covered on the Al electrode to obtain an inverted structure QLED device.
[0151] Example 5
[0152] In the manufacturing process of the light emitting device of Example 5, zinc oxide is spin-coated at low temperature, and the solvent is removed by nitrogen at high temperature. Other functional layers are spin-coated at room temperature and the solvent is removed at high temperature.
[0153] The specific steps are as follows:
[0154] S1: Spin coat a PEDOT:PSS hole injection layer on the ITO substrate at a rotation speed of 3000 r / min, a solution concentration of 15 mg / ml, a duration of 40 s, a thickness of 40 nm, and a processing temperature of 25 °C.
[0155] S2: placing the intermediate device with the hole injection layer formed thereon on a desolventizing station for desolventizing treatment. The treatment method is high temperature drying, and the treatment temperature is 90°C.
[0156] S3: A layer of TFB is prepared on the hole injection layer as a hole transport layer, with a rotation speed of 3000 r / min, a solution concentration of 8 mg / ml, a duration of 40 s, a thickness of 35 nm, and a processing temperature of 25°C.
[0157] S4: placing the intermediate device with the hole transport layer formed thereon on a desolvation station for desolvation treatment, wherein the treatment method is to introduce nitrogen gas, the gas flow rate is 7 m / s, the treatment time is 1 min, and the treatment temperature is 90°C.
[0158] S5: Spin-coat a layer of CdSe@ZnS on the hole transport layer as a quantum dot light-emitting layer, with a rotation speed of 2000 r / min, a solution concentration of 12.5 mg / ml, a duration of 40 s, a thickness of 30 nm, and a processing temperature of 25°C.
[0159] S6: placing the intermediate device with the quantum dot light-emitting layer formed thereon on a desolvation table for desolvation treatment. The treatment method is to introduce nitrogen gas, with a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 90°C.
[0160] S7: Spin coat a layer of ZnO as an electron transport layer on the quantum dot light-emitting layer, the rotation speed is 2000r / min, the solution concentration is 12.5mg / ml, the solvent is n-butanol, the time is 40s, the thickness is 50nm, and the spin coating temperature is 0℃.
[0161] S8: placing the intermediate device with the electron transport layer formed thereon on a desolventizing station for desolventizing treatment. The treatment method is high temperature drying, and the treatment temperature is 90°C.
[0162] S9: evaporating an Al electrode on the electron transport layer.
[0163] S10: A layer of encapsulation glue is covered on the Al electrode to obtain an inverted structure QLED device.
[0164] Example 6
[0165] The difference between Example 6 and Example 3 is that the temperature for spin coating zinc oxide is 10°C, and the temperature for removing the solvent with nitrogen is also 10°C.
[0166] In the manufacturing process of light-emitting devices, zinc oxide is spin-coated at low temperature and the solvent is removed by nitrogen at low temperature. Other functional layers are spin-coated at room temperature and the solvent is removed at high temperature.
[0167] Example 7
[0168] The difference between Example 7 and Example 3 is that the temperature for spin coating zinc oxide is 3°C, and the temperature for removing the solvent with nitrogen is also 3°C.
[0169] In the manufacturing process of light-emitting devices, zinc oxide is spin-coated at low temperature and the solvent is removed by nitrogen at low temperature. Other functional layers are spin-coated at room temperature and the solvent is removed at high temperature.
[0170] Example 8
[0171] The difference between Example 8 and Example 3 is that the temperature for spin coating zinc oxide is 8°C, and the temperature for removing the solvent with nitrogen is also 8°C.
[0172] In the manufacturing process of light-emitting devices, zinc oxide is spin-coated at low temperature and the solvent is removed by nitrogen at low temperature. Other functional layers are spin-coated at room temperature and the solvent is removed at high temperature.
[0173] Comparative Example
[0174] Each functional layer is spin-coated at room temperature and the solvent is removed at high temperature.
[0175] The specific steps are as follows:
[0176] S1: Spin coat a PEDOT:PSS hole injection layer on the ITO substrate at a rotation speed of 3000 r / min, a solution concentration of 15 mg / ml, a duration of 40 s, a thickness of 40 nm, and a processing temperature of 25 °C.
[0177] S2: placing the intermediate device with the hole injection layer formed thereon on a desolventizing station for desolventizing treatment. The treatment method is high temperature drying, and the treatment temperature is 90°C.
[0178] S3: A layer of TFB is prepared on the hole injection layer as a hole transport layer, with a rotation speed of 3000 r / min, a solution concentration of 8 mg / ml, a duration of 40 s, a thickness of 35 nm, and a processing temperature of 25°C.
[0179] S4: placing the intermediate device with the hole transport layer formed thereon on a desolvation station for desolvation treatment, wherein the treatment method is to introduce nitrogen gas, the gas flow rate is 7 m / s, the treatment time is 1 min, and the treatment temperature is 90°C.
[0180] S5: Spin-coat a layer of CdSe@ZnS on the hole transport layer as a quantum dot light-emitting layer, with a rotation speed of 2000 r / min, a solution concentration of 12.5 mg / ml, a duration of 40 s, a thickness of 30 nm, and a processing temperature of 25°C.
[0181] S6: placing the intermediate device with the quantum dot light-emitting layer formed thereon on a desolvation table for desolvation treatment. The treatment method is to introduce nitrogen gas, with a gas flow rate of 7 m / s, a treatment time of 1 min, and a treatment temperature of 90°C.
[0182] S7: Spin coat a layer of ZnO as an electron transport layer on the quantum dot light-emitting layer, the rotation speed is 2000r / min, the solution concentration is 12.5mg / ml, the solvent is n-butanol, the time is 40s, the thickness is 50nm, and the spin coating temperature is 25℃.
[0183] S8: placing the intermediate device with the electron transport layer formed thereon on a desolventizing station for desolventizing treatment. The treatment method is high temperature drying, and the treatment temperature is 90°C.
[0184] S9: evaporating an Al electrode on the electron transport layer.
[0185] S10: A layer of encapsulation glue is covered on the Al electrode to obtain an inverted structure QLED device.
[0186] The performance tests were carried out for Examples 1-5 and the comparative example, and the test method was as follows:
[0187] The test method of luminous efficiency EQE is as follows: using FPD optical characteristic measurement equipment, controlling QE PRO spectrometer, Keithley 2400, Keithley 6485 through LabView, measuring parameters such as voltage, current, brightness, luminous spectrum, and recording the minimum voltage V min and maximum value V max And the device luminous efficiency EQE is obtained by calculation.
[0188] A 128-channel life test system customized by Guangzhou New Vision Company was used to test the maximum brightness L, life T95 and life T95@1000nit of the light-emitting devices in Examples 1 to 14 and the comparative example. The system architecture is that a 2mA constant current source drives the light-emitting device to test the change in voltage or current. The photodiode detector and the test system test the change in brightness (photocurrent) of the light-emitting device. The brightness meter tests and calibrates the brightness (photocurrent) of the electroluminescent device to obtain the maximum brightness L, life T95, and the time it takes for the initial brightness of the light-emitting device to decay to 95%. The time it takes for the initial brightness of the light-emitting device to decay to 95% is converted to the aging time at 1000nit to obtain the life T95@1000nit.
[0189] The test results are shown in Table 1:
[0190]
[0191] The following are the experimental conditions of Examples 1-5 and Comparative Examples:
[0192] Example 1: low temperature spin coating of zinc oxide solution, room temperature nitrogen desolventizing, room temperature spin coating of other functional layers, room temperature nitrogen desolventizing;
[0193] Example 2: Low temperature spin coating of zinc oxide solution, low temperature nitrogen removal of solvent, other functional layers are spin coated at room temperature, and room temperature nitrogen removal of solvent;
[0194] Example 3: Low temperature spin coating of zinc oxide solution, low temperature nitrogen removal of solvent, other functional layers spin coating at room temperature, high temperature removal of solvent;
[0195] Example 4: Spin coating zinc oxide solution at room temperature, removing solvent with low temperature nitrogen, and spin coating other functional layers at room temperature and removing solvent with high temperature;
[0196] Example 5: Spin coating zinc oxide solution at low temperature and removing the solvent at high temperature, and spin coating other functional layers at room temperature and removing the solvent at high temperature;
[0197] Comparative example: Each functional layer is spin-coated at room temperature and the solvent is removed at high temperature (conventional preparation method).
[0198] From the comparison between Example 1 and Example 2, it can be seen that in the process of preparing the electron transport layer, the effect of removing the solvent at low temperature is better than that of removing the solvent at room temperature.
[0199] From the comparison between Example 2 and Example 3, it can be seen that in the process of preparing other functional layers, the effect of removing solvent at high temperature is better than that of removing solvent at room temperature. The possible reason is that other functional layers need high temperature heating to better remove solvent, but the ideal effect cannot be achieved by nitrogen at room temperature, so the electrical performance is worse.
[0200] From the comparison between Example 3 and Example 4, it can be seen that in the process of preparing the electron transport layer, the effect of low-temperature spin coating of the zinc oxide solution is better than that of normal-temperature spin coating of the zinc oxide solution.
[0201] From the comparison between Example 3 and Example 5, it can be seen that in the process of preparing the electron transport layer, the effect of removing the solvent at low temperature is better than that of removing the solvent at room temperature.
[0202] From the comparison between Example 3 and Examples 6-8, it can be seen that in the process of preparing the electron transport layer, the zinc oxide spin coating and low-temperature drying at 3-8°C have better effects than those at 0°C and 10°C.
[0203] From the comparison between Examples 1-8 and the comparative example, when the other functional layers are spin-coated at room temperature and the solvent is removed at high temperature, the effects of Examples 3-5 in which zinc oxide solution is spin-coated at low temperature and / or nitrogen is used to remove the solvent are better than those of the comparative example. However, if nitrogen is used to remove the solvent at room temperature for other functional layers, the performance of the obtained QLED device is reduced regardless of whether the electron transport layer is prepared at low temperature.
[0204] The above provides a detailed introduction to the implementation methods of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The above description of the implementation methods is only used to help understand the present application. At the same time, for those skilled in the art, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present application.
Claims
1. A method for preparing a thin film, characterized in that: The following steps are involved: Providing a substrate, and forming a solution containing inorganic nanoparticles on the substrate at a first preset temperature to obtain a thin film precursor; and Drying the film precursor at a second preset temperature to obtain the film; Wherein, the first preset temperature and / or the second preset temperature is lower than room temperature.
2. The method for preparing a thin film according to claim 1, characterized in that: The first preset temperature and / or the second preset temperature is 0°C-10°C; and / or The first preset temperature and the second preset temperature are equal.
3. The method for preparing a thin film according to claim 1, characterized in that: The step of drying the film precursor comprises: providing gas to blow dry the film precursor; and / or The step of drying the film precursor comprises: providing an inert gas to blow dry the film precursor; and / or The flow rate of the gas is 3m / s-14m / s; and / or In the step of drying the film precursor, the drying time is more than 1 minute; and / or In the step of drying the film precursor, the drying time is 1 min to 30 min; and / or The forming of the solution containing inorganic nanoparticles on the substrate and the drying of the thin film precursor are performed under normal pressure.
4. The method for preparing a thin film according to claim 1, characterized in that: The solution containing inorganic nanoparticles further comprises a solvent, wherein the mass fraction of the inorganic nanoparticles is 0.1%-20.0%; the mass fraction of the solvent is 80.0%-99.9%; and / or The solvent comprises at least one of a saturated hydrocarbon solvent, an unsaturated hydrocarbon solvent, an aromatic hydrocarbon solvent, an alcohol solvent, an ether solvent, a ketone solvent, a nitrile solvent, and an ester solvent; and / or The solvent includes at least one of methanol, ethanol, ethylene glycol, propanol, propylene glycol, glycerol, isopropanol, butanol, pentanol, hexanol, cyclohexanol, n-butanol, benzyl alcohol, phenylethyl alcohol, and acetonitrile.
5. The method for preparing a thin film according to claim 1, characterized in that: The average particle size of the inorganic nanoparticles is 2 to 20 nm; and / or The inorganic nanoparticles are selected from at least one of metal oxides, doped metal oxides, II-VI semiconductor materials, III-V semiconductor materials and I-III-VI semiconductor materials; the metal oxide is selected from at least one of ZnO, BaO, TiO2, and SnO2; the metal oxide in the doped metal oxide is selected from at least one of ZnO, TiO2, and SnO2, and the doping element can be selected from at least one of Al, Mg, Li, In, and Ga; the II-VI semiconductor material is selected from at least one of ZnS, ZnSe, and CdS; the III-V semiconductor material is selected from at least one of InP and GaP; the I-III-VI semiconductor material is selected from at least one of CuInS and CuGaS.
6. A film, characterized in that: The film is prepared by the method for preparing the film according to any one of claims 1 to 5.
7. A method for preparing a light emitting device, characterized in that: The following steps are involved: Providing a light-emitting device preform, wherein the light-emitting device preform comprises a bottom electrode; A thin film is prepared on the light-emitting device preform by the thin film preparation method according to any one of claims 1 to 5 to obtain an electron transport layer; as well as forming a top electrode on the electron transport layer to obtain a light-emitting device; Wherein, the bottom electrode is a cathode, the top electrode is an anode, and before forming the top electrode on the electron transport layer, the method further includes: forming a light-emitting layer on the electron transport layer; or The bottom electrode is an anode, the top electrode is a cathode, and the substrate further includes a light-emitting layer formed on the bottom electrode.
8. A light emitting device, characterized in that: The light emitting device is prepared by the method for preparing the light emitting device according to claim 7.
9. The light emitting device according to claim 8, characterized in that: The bottom electrode and the top electrode are independently selected from a doped metal oxide particle electrode, a composite electrode, a graphene electrode, a carbon nanotube electrode, a metal element electrode or an alloy electrode, the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide, the composite electrode is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS or ZnS / Al / ZnS, and the material of the metal electrode is selected from one or more of Ag, Al, Cu, Au, Mo, Pt, Ca and Ba; and / or The material of the light-emitting layer is selected from one or more quantum dot light-emitting materials, and the quantum dot light-emitting material is selected from one or more single-structure quantum dots, core-shell quantum dots and perovskite semiconductor materials. The material of the single-structure quantum dots, the core material of the core-shell quantum dots and the shell material of the core-shell quantum dots are respectively selected from at least one of the single-structure quantum dots selected from II-VI compounds, IV-VI compounds, III-V compounds and I-III-VI compounds. The II-VI compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdS At least one of CdS, SnSe, SnTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, wherein the Group IV-VI compound is selected from SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, Sn At least one of SeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe, and the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaA At least one of GaInNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2, the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors, the inorganic perovskite semiconductor has a general structural formula of AMX3, wherein A is Cs + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the organic-inorganic hybrid perovskite semiconductors, the general structural formula of which is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .
10. A display device, characterized in that: Comprising the light emitting device as claimed in claim 8 or 9.