Composite body and method for producing same
A composite of fine fibrous cellulose with needle-shaped iron (III)-containing particles addresses the inefficiencies of existing adsorbents by enhancing surface area and iron loading, effectively adsorbing and recovering arsenic (V) from water while minimizing waste.
Patent Information
- Application Number
- CN202380036003.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-28
- Publication Date
- 2024-12-03
AI Technical Summary
Existing adsorbents struggle to efficiently adsorb and recover arsenic (V) due to limited surface area and iron loading, leading to ineffective arsenic (V) removal from water, particularly in the presence of similar elements like phosphorus.
A composite comprising fine fibrous cellulose with needle-shaped iron (III)-containing particles, such as iron oxide or hydroxide, supported on its surface, enhancing surface area and iron loading, allowing efficient arsenic (V) adsorption and recovery.
The composite provides a large adsorption surface area, enabling efficient arsenic (V) adsorption and recovery, even in the presence of similar elements, with reduced waste generation and disposal costs.
Smart Images

Figure CN119072353A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a novel composite, a method for producing the same, an arsenic adsorbent including the composite, methods for producing the same, a method for producing purified water using the arsenic adsorbent, and a water purification device including the arsenic adsorbent. Background Art
[0002] Arsenic is widely distributed in the environment, but it is highly harmful. Even trace amounts can cause various diseases and damage health through long-term intake.
[0003] In addition, inorganic arsenic contamination of well water in Southeast Asia and other parts of the world has become a major environmental problem. Therefore, a method for removing arsenic contained in water is needed.
[0004] For example, Patent Document 1 describes that an adsorbent obtained by mixing ferrous hydroxide and a styrene-acrylic acid copolymer binder and granulating the mixture is useful for adsorbing and removing arsenic (III) from strongly acidic water.
[0005] Patent Document 1: Japanese Patent Application Publication No. 2008-207110 Summary of the invention
[0006] Arsenic (V) is adsorbed on the surface of iron, but in the case of the adsorbent, it is difficult to ensure a large adsorption surface for arsenic (V) because the ferrous hydroxide supported on the binder is dissolved in water. In addition, the ferrous hydroxide is bonded to the carboxyl group of the styrene-acrylic acid copolymer binder and supported on the carboxyl group of the styrene-acrylic acid copolymer binder, so it is difficult to increase the iron loading per unit weight, and arsenic (V) cannot be adsorbed efficiently.
[0007] Therefore, an object of the present disclosure is to provide a novel composite having the effect of efficiently adsorbing and recovering arsenic (V) dissolved in water.
[0008] Another object of the present disclosure is to provide a method for manufacturing the composite.
[0009] Another object of the present disclosure is to provide a novel arsenic adsorbent that can efficiently adsorb / recover arsenic (V) dissolved in water.
[0010] Another object of the present disclosure is to provide a method for producing purified water using the arsenic adsorbent.
[0011] Another object of the present disclosure is to provide a water purification device including the arsenic adsorbent.
[0012] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found the following.
[0013] 1. The specific surface area of fine fibrous cellulose is extremely large. If iron (III)-containing particles are supported on the surface of fine fibrous cellulose, aggregation of the iron (III)-containing particles can be suppressed, thereby ensuring a large surface area of the iron (III)-containing particles that is effective for adsorption of arsenic.
[0014] 2. Microfibrous cellulose has three hydroxyl groups to which iron can be bonded in each structural unit, thereby increasing the iron loading per unit weight.
[0015] 3. When the iron (III)-containing particles supported on fine fibrous cellulose are crystallized into needle-like shapes, the surface area effective for adsorption of arsenic can be significantly expanded, and the arsenic adsorption efficiency can be dramatically improved.
[0016] 4. Fine fibrous cellulose has excellent hydrophilicity. When immersed in water, water easily penetrates into the fine fibrous cellulose. Therefore, arsenic dissolved in water is efficiently adsorbed by the iron (III)-containing particles supported on the fine fibrous cellulose.
[0017] The present disclosure has been completed based on these findings.
[0018] That is, the present disclosure provides a composite comprising fine fibrous cellulose and iron (III)-containing particles supported on the fine fibrous cellulose, wherein at least a part of the iron (III)-containing particles has an aspect ratio of 2 or more.
[0019] The present disclosure also provides the composite, wherein the amount of the iron (III)-containing particles supported per 1 g of the fine fibrous cellulose (in terms of iron element) is 1 to 100 mmol.
[0020] The present disclosure also provides the composite, wherein the fine fibrous cellulose is microfibrillated cellulose.
[0021] The present disclosure also provides the composite, wherein the iron (III)-containing particles contain at least one iron compound selected from the group consisting of iron oxide, iron hydroxide, and iron oxyhydroxide.
[0022] The present disclosure also provides the composite, wherein the iron (III)-containing particles contain: at least one iron compound selected from iron oxide, iron hydroxide and iron oxyhydroxide; and an oxide, hydroxide or oxyhydroxide of at least one metal selected from zirconium and titanium, and the molar ratio [iron / (zirconium and / or titanium)] of the iron compound (iron element conversion value) to the oxide, hydroxide or oxyhydroxide of the metal (metal element conversion value; the total amount when containing two or more kinds) is 1 to 100.
[0023] The present disclosure also provides the composite, wherein the particle diameter of a volume equivalent sphere of the iron (III)-containing particle is less than 1 μm.
[0024] The present disclosure also provides a method for producing a composite, wherein fine fibrous cellulose and an iron compound are mixed in water in the presence of a crystal modifier, the iron compound is adsorbed on the fine fibrous cellulose, and then a heat treatment is performed to produce the composite.
[0025] The present disclosure also provides the method for producing the composite, wherein, in the step of adsorbing the iron compound to the fine fibrous cellulose, the iron compound and at least one metal compound selected from the group consisting of a zirconium compound and a titanium compound are adsorbed together.
[0026] The present disclosure also provides an arsenic adsorbent, which comprises the composite.
[0027] The present disclosure also provides a method for producing purified water, wherein purified water is obtained by treating arsenic-contaminated water with the arsenic adsorbent.
[0028] The present disclosure also provides a water purification device, which includes the arsenic adsorbent.
[0029] The composite disclosed in the present invention has the following structure: needle-shaped iron (III)-containing particles with a large adsorption surface area for arsenic (V) are dispersed on fine fibrous cellulose having an extremely large specific surface area and excellent hydrophilicity. Therefore, if the composite is immersed in water, arsenic (V) dissolved in the water can be efficiently adsorbed and recovered.
[0030] Furthermore, the composite can selectively adsorb and recover arsenic even in the presence of an element such as phosphorus (P) having chemical properties similar to those of arsenic.
[0031] Furthermore, the composite does not generate waste gas even when burned, and the cost required for disposal such as landfill can be greatly reduced by burning the adsorbed arsenic (V) to reduce its volume.
[0032] Therefore, the composite can be preferably used as an arsenic adsorbent for adsorbing and recovering arsenic from water contaminated with arsenic (particularly arsenic (V)). BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a diagram showing a SEM image of the composite (1) obtained in Example 1 (magnification: 5000 times).
[0034] Figure 2 This is a diagram showing a SEM image of the composite (2) obtained in Example 2 (magnification: 5000 times).
[0035] Figure 3These are diagrams showing SEM images of the composites (2), (3), and (4) obtained in Examples 2 to 4. Figure 3 (a) is a 5000-fold field of view, Figure 3 (b) is a 10,000-fold field of view. Figure 3 (c) is a 5000x field of view.
[0036] Figure 4 This is a diagram showing a SEM image of the composite (5) obtained in Example 5 (magnification: 5000 times).
[0037] Figure 5 This is a diagram showing a SEM image of the composite (8) obtained in Reference Example 1 (magnification: 5000 times).
[0038] Figure 6 This is a graph showing the relationship between the As(V) adsorption rate and pH of the composite (2) obtained in the example.
[0039] Figure 7 This is a graph showing the As(V) adsorption rate of the composite (2) obtained in the example in the presence of anions.
[0040] Figure 8 This is a diagram showing that, in one embodiment of the present disclosure, iron oxide particles are bonded to the surface of fine fibrous cellulose (1) under pressure and high temperature in a composite.
[0041] Fig. 9 This is a diagram showing a SEM image of the composite (5) obtained in Example 5 (magnification: 30,000 times).
[0042] Fig.10 This is a diagram showing a SEM image of the composite (7) obtained in Example 7 (magnification: 30,000 times). DETAILED DESCRIPTION
[0043] Hereinafter, one embodiment of the present disclosure will be described in detail. The present disclosure is not limited to the following embodiment, and can be implemented with appropriate modifications within a range that does not hinder the effects of the present disclosure.
[0044] Each configuration and combination thereof in each embodiment is an example, and addition, omission, substitution, and other changes of the configuration may be appropriately made without departing from the gist of the present disclosure. The present disclosure is not limited to the embodiments but only to the claims.
[0045] Each solution disclosed in this specification may also be combined with any other feature disclosed in this specification.
[0046] When a specific description described in one embodiment is also applicable to other embodiments, the description is sometimes omitted in other embodiments. In addition, the lower limit and / or upper limit of the numerical range described in this disclosure are numerical values within the numerical range and can also be replaced by the numerical values shown in the embodiments.
[0047] In the present disclosure, the expression "X to Y" regarding a numerical range means "X or more and Y or less".
[0048] In the present disclosure, the expression "S and / or T" with respect to a component, a substance, etc. means "at least one selected from the group consisting of S and T".
[0049] [Complex]
[0050] The composite disclosed herein comprises fine fibrous cellulose and iron (III)-containing particles, wherein the iron (III)-containing particles are contained in a state of being supported on the fine fibrous cellulose. In addition, at least a portion of the iron (III)-containing particles are particles having an aspect ratio of 2 or more (hereinafter sometimes referred to as "needle-shaped particles"). "Needle-shaped particles" refer to particles having an aspect ratio of 2 or more, and in one embodiment, in particles having an aspect ratio of 2 or more, the shape may be such that the diameter (or width) becomes smaller as it approaches at least one front end, or the shape may be such that at least one front end is sharp.
[0051] The proportion of the needle-shaped particles in the total amount of the iron (III)-containing particles is, for example, 5% by weight or more. From the viewpoint of further expanding the adsorption surface of arsenic and improving the adsorption / recovery efficiency of arsenic, the proportion of the needle-shaped particles in the total amount of the iron (III)-containing particles is preferably 8% by weight or more, and particularly preferably 10% by weight or more. The upper limit of the proportion of the needle-shaped particles in the total amount of the iron (III)-containing particles is 100% by weight, and is 50% by weight, particularly 30% by weight.
[0052] The aspect ratio (particle length / particle diameter) of the needle-shaped particles is greater than 2. From the viewpoint of further expanding the adsorption surface of arsenic and improving the adsorption / recovery efficiency of arsenic, the aspect ratio of the needle-shaped particles is preferably greater than 3, more preferably greater than 5, and particularly preferably greater than 10. Regarding the upper limit of the aspect ratio, for example, it is preferably less than 100, more preferably less than 50, and further preferably less than 30. That is, the aspect ratio of the needle-shaped particles can be any combination of these upper and lower limits, preferably greater than 3 and less than 100, more preferably greater than 5 and less than 50, and further preferably greater than 10 and less than 30.
[0053] By growing the particles under hydrothermal conditions (pressure and high temperature) in the presence of a crystallizing agent during production, the aspect ratio of the needle-shaped particles can easily reach more than 2. By using a crystallizing agent in an amount of, for example, 0.1 to 10 parts by weight relative to 1 part by weight of the iron compound, needle-shaped particle formation can be easily promoted and / or the aspect ratio of the needle-shaped particles can be easily increased.
[0054] The particle diameter of the volume equivalent sphere of the needle-shaped particle (hereinafter sometimes referred to as the "volume equivalent diameter") is, for example, less than 1 μm, preferably less than 800 nm, more preferably less than 600 nm, further preferably less than 500 nm, and further preferably less than 400 nm. When the particle diameter of the volume equivalent sphere of the needle-shaped particle is less than 400 nm, it may be less than 200 nm, or less than 100 nm. Regarding the lower limit of the particle diameter, for example, it is preferably greater than 1 nm, and more preferably greater than 10 nm. That is, the particle diameter of the volume equivalent sphere of the needle-shaped particle can be any combination of these upper and lower limits, for example, greater than 1 nm and less than 1 μm, preferably greater than 1 nm and less than 800 nm, more preferably greater than 10 nm and less than 600 nm, further preferably greater than 10 nm and less than 500 nm, and further preferably greater than 10 nm and less than 400 nm. When the particle diameter of the volume equivalent sphere of the needle-shaped particle is 10 nm to 400 nm, it may be 10 nm to 200 nm, or 10 nm to 100 nm.
[0055] The “particle length” and “particle diameter” of a particle refer to the major axis diameter and minor axis diameter of the particle, respectively.
[0056] The major axis diameter and minor axis diameter of a particle are the diameters of the major axis and minor axis of the particle in a two-dimensional particle image observed by a scanning electron microscope (SEM).
[0057] In one embodiment, in at least one SEM two-dimensional particle image, the major axis diameters of ten randomly selected particles and the minor axis diameter of the same particle are measured, wherein the aspect ratio of at least one of the particles is greater than 2. In the case where the aspect ratio is greater than 2, the aspect ratio may be greater than 4, for example, 4. Moreover, the major axis diameters of ten particles and the minor axis diameter of the same particle are measured, and it is further preferred that, relative to the total weight of the composite, more preferably more than 5% by weight, more preferably more than 7% by weight, and further preferably more than 9% by weight of the particles have an aspect ratio of greater than 2. In the case where the particle diameter of the volume equivalent sphere of the needle-shaped particles is greater than 9% by weight, it may be greater than 10% by weight, may be greater than 11% by weight, may be greater than 12% by weight, or may be greater than 13% by weight.
[0058] The particle diameter of the volume equivalent sphere can be obtained by SEM observation and image analysis. The particle diameter of the volume equivalent sphere is the average value of the value of the volume equivalent sphere particle diameter (D) calculated by multiplying the three sides of ten randomly selected particles in at least one SEM two-dimensional particle image, and calculating the volume (V) by the following formula.
[0059] D=(6 / πV) (1 / 3)
[0060] In the particles containing iron (III), in addition to needle-shaped particles, particles of other shapes may also be included. As other shapes, for example, spherical (true spherical, roughly true spherical, ellipsoidal, etc.), polyhedral, flat, flaky, irregular shapes, etc. can be listed. In other words, particles having an aspect ratio of less than 2 may be included in the particles containing iron (III), and as particles having an aspect ratio of less than 2, the above-mentioned spherical (true spherical, roughly true spherical, ellipsoidal, etc.), polyhedral, flat, flaky, irregular shapes, etc. can be listed.
[0061] As iron (III)-containing particles, it is preferred that they contain at least one iron compound (for example, a water-insoluble trivalent iron compound) selected from iron oxide (Fe2O3), iron hydroxide (Fe(OH)3) and iron oxide (FeOOH), and more preferably at least one selected from the group consisting of iron oxide (Fe2O3) and iron oxide (FeOOH).
[0062] The iron (III)-containing particles may contain other components in addition to the water-insoluble trivalent iron compound, for example, an oxide, hydroxide or oxyhydroxide of at least one metal selected from zirconium and titanium such as zirconium oxide, zirconium hydroxide, zirconium oxyhydroxide, titanium oxide, titanium hydroxide, titanium oxyhydroxide, or a combination of two or more of the oxides, hydroxides and oxyhydroxides selected from the metals. The iron (III)-containing particles may contain iron (III) in the form of a mixed oxide with at least one of the other metals.
[0063] The oxide, hydroxide or oxyhydroxide of the metal has excellent affinity for arsenic (e.g., pentavalent arsenic). Therefore, if the iron component and the metal oxide are carried together on the surface of the microfibrous cellulose, or if a mixed oxide of the iron component and the metal is carried, the arsenic adsorption capacity can be further improved. In the case where the iron (III)-containing particles contain other components in addition to the water-insoluble trivalent iron compound, it is more preferred to contain at least one selected from the group consisting of oxides and oxyhydroxides of at least one metal selected from zirconium and titanium. In the case where the iron (III)-containing particles contain a mixed oxide of iron (III) and at least one of the other metals, it is preferred to contain a mixed oxide (Fe 2+) with zirconium and / or titanium.x Zr y O z , Fe x Ti y O z At least one of the above.
[0064] The iron (III)-containing particles may contain, in any combination, at least two or more selected from trivalent iron compounds, at least one of the oxides, hydroxides or oxyhydroxides of zirconium and / or titanium, and a mixed oxide of iron (III) and at least one of the metals, or may contain all of an iron compound, a zirconium and / or titanium compound, and a mixed oxide of iron with zirconium and / or titanium.
[0065] When the iron (III)-containing particles contain both a water-insoluble trivalent iron compound and an oxide, hydroxide or oxyhydroxide of the metal, the molar ratio of the iron compound (in terms of iron element conversion) to the oxyhydroxide or oxyhydroxide of the metal (in terms of metal element conversion; the total amount when two or more are contained) [iron / (zirconium + titanium)] is, for example, 1 to 100. When the iron (III)-containing particles contain a mixed oxide of iron (III) and the other metal, the molar ratio of the iron (III) (in terms of iron element conversion) to the other metal (in terms of metal element conversion; the total amount when two or more are contained) [iron / (zirconium + titanium)] is, for example, 1 to 100.
[0066] The upper limit of the molar ratio is preferably 50, more preferably 30, further preferably 20, and particularly preferably 15. The lower limit of the molar ratio is preferably 3, particularly preferably 5, and most preferably 7. That is, the molar ratio [iron / (zirconium + titanium)] may be any combination of these upper and lower limits, and is preferably 3 to 50, more preferably 3 to 30, further preferably 5 to 20, and further preferably 7 to 15.
[0067] Here, "zirconium + titanium" means "zirconium and / or titanium". That is, [iron / (zirconium + titanium)] means "iron / (zirconium and / or titanium)".
[0068] In one embodiment, the molar ratio [iron / (zirconium+titanium)] is preferably a molar ratio of "iron / zirconium" or "iron / titanium".
[0069] The content of the iron (III)-containing particles in 1 g of the composite (or the total of the fine fibrous cellulose and the iron (III)-containing particles contained in the composite) (converted value of the iron element) is, for example, 10 to 5000 μmol. The upper limit of the content of the iron (III)-containing particles (converted value of the iron element) is preferably 4000 μmol, particularly preferably 3500 μmol, and most preferably 3000 μmol. The lower limit of the content of the iron (III)-containing particles (converted value of the iron element) is preferably 100 μmol, more preferably 500 μmol, particularly preferably 1000 μmol, most preferably 1500 μmol, and may also be 2000 μmol. That is, the content of the iron (III)-containing particles (converted value of the iron element) can be any combination of these upper and lower limits, and is preferably greater than 100 μmol and less than 4000 μmol, more preferably greater than 500 μmol and less than 4000 μmol, further preferably greater than 1000 μmol and less than 3500 μmol, further preferably greater than 1500 μmol and less than 3500 μmol, further preferably greater than 1500 μmol and less than 3000 μmol, and may also be greater than 2000 μmol and less than 3000 μmol.
[0070] The total loading amount of iron (III)-containing particles in the complex can be evaluated by adding 6 mol / L hydrochloric acid to the complex to dissolve the trivalent iron in the form of iron (III) ions, measuring the concentration of iron (III) ions in the eluate using an instrument such as an ICP emission spectrometer, and using the method described in the examples to evaluate the total loading amount of iron (III) particles in the complex.
[0071] In the composite, the content of the iron (III)-containing particles per 1 g of fine fibrous cellulose (in terms of iron element) is, for example, 1 to 100 mmol, preferably 1 to 50 mmol, more preferably 1 to 10 mmol, particularly preferably 1 to 5 mmol, and most preferably 1 to 3 mmol.
[0072] The content of the iron (III)-containing particles relative to the fine fibrous cellulose can be calculated or measured by the same method as the content of the iron (III)-containing particles in the composite.
[0073] The weight of the fine fibrous cellulose contained in the composite can be evaluated by subtracting the weight of the zero-valent iron and trivalent iron particles calculated based on the total amount of zero-valent iron and trivalent iron supported in the composite (iron element conversion value) from the weight of the composite. The amount of zero-valent iron and trivalent iron supported relative to 1 g of fine fibrous cellulose can be calculated based on the total amount of zero-valent iron and trivalent iron supported in the composite and the weight of the fine fibrous cellulose contained in the composite.
[0074] The microfibrous cellulose is, for example, a cellulose fiber that has been torn in the longitudinal direction and has been micronized, and is preferably microfibrillated cellulose. The cellulose fiber being torn in the longitudinal direction means that the cellulose fiber is torn in the fiber direction.
[0075] The average fiber length of the fine fibrous cellulose is, for example, 0.5 to 1.5 mm, preferably 0.5 to 1.2 mm, and particularly preferably 0.6 to 0.8 mm. The average fiber diameter of the fine fibrous cellulose is, for example, 0.5 to 50 μm.
[0076] The aspect ratio (average fiber length / average fiber diameter) of the fine fibrous cellulose is preferably 5 to 10,000, more preferably 7 to 5,000, and even more preferably 10 to 3,000.
[0077] In the case of fine fibrous cellulose, the fiber length and fiber diameter are the length of the major axis and the diameter of the minor axis of the fiber in a two-dimensional particle image observed by SEM.
[0078] In one embodiment, the aspect ratio of the microfibrous cellulose is a value calculated by measuring the length of the major axis of ten or more cellulose fibers and the minor axis diameter of the same cellulose in a two-dimensional SEM cellulose image, and calculating the average value of the major axis length and the average value of the minor axis diameter by using the average fiber length / average fiber diameter. Alternatively, the aspect ratio of the microfibrous cellulose may be a value calculated by using the average fiber length / average fiber diameter by using the average fiber length and the average fiber diameter (or reference fiber diameter) described in the product information disclosed by the manufacturer.
[0079] The composite may further contain other components, but the total content of fine fibrous cellulose and iron (III)-containing particles is, for example, 50% by weight or more, preferably 60% by weight or more, particularly preferably 70% by weight or more, most preferably 80% by weight or more, and particularly preferably 90% by weight or more of the total amount of the composite. If the content of fine fibrous cellulose and iron (III)-containing particles is below the above range, there is a tendency that it is difficult to efficiently and selectively adsorb arsenic.
[0080] The shape of the complex is not particularly limited as long as the effects of the present disclosure are not impaired, but is preferably in a gel, powder, or granular form from the viewpoint of facilitating recovery of arsenic from the aqueous solution after adsorbing the arsenic.
[0081] There are no particular limitations on the method for adsorbing arsenic dissolved in an aqueous solution onto the complex, and examples thereof include: a method in which the complex is filled into a chromatographic column or the like and an aqueous solution containing arsenic is flowed therein; a method in which the complex is added to an aqueous solution containing arsenic and the mixture is stirred; and the like.
[0082] The state where metal particles (particles (2) containing iron (III)) grow on fine fibrous cellulose (1) is shown in FIG. Figure 8 By bonding a plurality of particles smaller than the fiber diameter to the surface of the fine fibrous cellulose fibers, more iron can be carried than when the iron compound is adsorbed only on the surface of the fiber. In addition, by making the aspect ratio greater than 2, arsenic can be adsorbed on more surfaces in the particles.
[0083] Arsenic (V) exists in the form of arsenate ions in aqueous solution. In the case of the complex, in water, at least one iron compound selected from iron oxide, iron hydroxide, and iron oxyhydroxide is complexed via the hydroxyl group of arsenic (particularly arsenate ions), thereby adsorbing and fixing arsenic (particularly arsenate ions) ( Figure 8 )(See below).
[0084] [Chemical formula 1]
[0085]
[0086] [Chemical formula 2]
[0087]
[0088] In [Chemical Formula 1], "Fe" connected to cellulose by a dotted line refers to iron of an iron compound contained in the iron (III)-containing particles adsorbed to cellulose, and indicates that iron adsorbs and fixes arsenic as described above.
[0089] [Chemical Formula 2] represents the state in which the metals (Fe, Zr, Ti) contained in the iron (III)-containing particles (2) adsorb and fix arsenic.
[0090] The adsorption capacity of arsenic of the complex is, for example, 300 μmol / g or more, preferably 500 μmol / g or more, more preferably 900 μmol / g or more, and further preferably 1300 μmol / g or more. The upper limit of the adsorption capacity of arsenic is, for example, 5000 μmol / g. That is, the adsorption capacity of arsenic of the complex can be any combination of these upper and lower limits, for example, 300 μmol / g or more and 5000 μmol / g or less, preferably 500 μmol / g or more and 5000 μmol / g or less, more preferably 900 μmol / g or more and 5000 μmol / g or less, and further preferably 1300 μmol / g or more and 5000 μmol / g or less.
[0091] The adsorption capacity of arsenic per 1 mol of iron (III)-containing particles (converted value of the iron element) contained in the composite is, for example, 0.2 mol or more, preferably 0.3 mol or more, and particularly preferably 0.5 mol or more. The upper limit value of the adsorption capacity of arsenic is, for example, 10 mol, and particularly 5 mol. That is, the adsorption capacity of arsenic per 1 mol of iron (III)-containing particles (converted value of the iron element) contained in the composite can be any combination of these upper and lower limits, for example, 0.2 mol or more and 10 mol or less, preferably 0.3 mol or more and 10 mol or less, more preferably 0.5 mol or more and 10 mol or less, and further preferably 0.5 mol or more and 5 mol or less.
[0092] At least one iron compound selected from iron oxide, iron hydroxide and iron oxyhydroxide has a high affinity for arsenic ions, but has a low affinity for other anions such as phosphorus-containing dihydrogen phosphate ions, halide ions, and sulfate ions, which have chemical properties similar to arsenic. The complex contains an iron compound having the above characteristics, so that even in the presence of other anions, the arsenic adsorption capacity is not reduced and arsenic can be selectively adsorbed.
[0093] It should be noted that the adsorption capacity of the arsenic adsorbent for arsenic is the adsorption amount when 0.01 g of the composite is immersed in 10 mL of a 1000 mg / L arsenic (V) aqueous solution at 25°C and shaken with an oscillator for 30 minutes, and is calculated according to the formula described in the examples.
[0094] By using the composite disclosed herein, arsenic (particularly arsenic (V)) dissolved in water can be recovered.
[0095] Furthermore, after the composite of the present disclosure is allowed to adsorb arsenic, it is possible to significantly reduce the volume by burning it, thereby reducing the cost required for treatment.
[0096] Since the composite has the above characteristics, it is useful as an adsorbent for adsorbing and recovering arsenic (particularly arsenic (V)) from arsenic-contaminated water.
[0097] [Method for producing a composite body]
[0098] The composite can be produced, for example, by mixing fine fibrous cellulose and an iron compound in water in the presence of a crystal modifier, allowing the iron compound to adsorb to the fine fibrous cellulose (adsorption step), and then subjecting the mixture to a heat treatment (hydrothermal treatment step).
[0099] (Adsorption process)
[0100] This step is a step of mixing fine fibrous cellulose and an iron compound in water in the presence of a crystallizing agent to adsorb the iron compound to the fine fibrous cellulose.
[0101] As the iron compound, for example, a trivalent iron compound such as FeCl 3 can be used.
[0102] The amount of the iron compound used is, for example, 1 to 100 mmol, or preferably 1 to 50 mmol, relative to 1 g of the fine fibrous cellulose.
[0103] The amount of the iron compound used is, for example, 1 to 10 g per 1 g of the fine fibrous cellulose. From the viewpoint of obtaining a composite having particularly excellent arsenic adsorption capacity, the amount of the iron compound used is preferably 2 to 8 g, particularly preferably 3 to 6 g per 1 g of the fine fibrous cellulose.
[0104] As the crystal mediator, it is preferable to select and use a compound that promotes needle-shaped crystallization of the iron (III)-containing particles, for example, sodium sulfate can be used.
[0105] The amount of the crystal mediator used is, for example, 0.1 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and particularly preferably 0.1 to 2 parts by weight relative to 1 part by weight of the iron compound. By using the crystal mediator within the above range, the needle-shaped crystallization of the iron compound can be promoted, the needle-shaped particles of the iron (III)-containing particles can be promoted, and / or the aspect ratio of the needle-shaped particles can be increased, which can further expand the adsorption surface of arsenic.
[0106] In the method of the present disclosure, a metal compound having a good affinity for arsenic may also be used to improve the arsenic adsorption capacity.
[0107] Examples of the metal compound include zirconium compounds such as zirconium oxide (ZrO2), zirconium hydroxide, zirconium oxyhydroxide, zirconium oxychloride (ZrCl2O), and zirconium chloride (ZrCl4); titanium compounds such as titanium oxide, titanium chloride, titanium hydroxide, and titanium oxyhydroxide, etc. These compounds may be used alone or in combination of two or more.
[0108] As the metal compound, from the viewpoint of excellent affinity with arsenic and particularly excellent effect of increasing the adsorption amount of arsenic, it is preferably at least one selected from the oxides, hydroxides and oxyhydroxides of the metal, more preferably at least one selected from the group consisting of the oxides and oxyhydroxides of the metal, and further preferably a zirconium compound such as zirconium oxychloride (ZrCl2O).
[0109] The amount of the metal compound used (the total amount when two or more kinds are used) is, for example, 0.01 to 10 parts by weight, or preferably 0.01 to 2 parts by weight, relative to 1 part by weight of the iron compound.
[0110] The usage ratio (molar ratio) [Fe / (Zr+Ti)] of the iron compound (in terms of iron element conversion) and the zirconium compound and / or titanium compound (in terms of metal element conversion; when two or more kinds are contained, the total amount thereof) is, for example, 1 to 100. The upper limit of the molar ratio is preferably 50, and particularly preferably 10. The lower limit of the molar ratio is preferably 3, particularly preferably 5, and most preferably 8. That is, the usage ratio (molar ratio) [Fe / (Zr+Ti)] may be any combination of these upper and lower limits, and is preferably 3 or more and 50 or less, more preferably 5 or more and 50 or less, and further preferably 8 or more and 10 or less.
[0111] Here, "Zr+Ti" means "Zr (zirconium compound) and / or Ti (titanium compound)". That is, [Fe / (Zr+Ti)] means "iron / (zirconium compound and / or titanium compound)".
[0112] In one embodiment, the molar ratio [Fe / (Zr+Ti)] is preferably the molar ratio of "iron / zirconium compound" or "iron / titanium compound".
[0113] When the metal compound is used, the iron compound and the metal compound are added together to water and stirred to allow the metal compound to be adsorbed to the fine fibrous cellulose.
[0114] Microfibrous cellulose is, for example, a substance in which cellulose fibers are longitudinally torn and micronized, i.e., microfibrillated cellulose. Microfibrous cellulose can be produced, for example, by subjecting cellulose fibers having a specific fiber length to a beating treatment and / or a mechanical shearing treatment (e.g., a homogenization treatment) to tear the cellulose fibers along the fiber direction.
[0115] As the cellulose fiber, for example, cellulose fibers derived from wood pulp (conifer pulp, broadleaf pulp) and cotton linter pulp can be preferably used. They can be used alone or in combination of two or more. It should be noted that the pulp can also contain different components such as hemicellulose.
[0116] Furthermore, the cellulose fibers may be fibers having functional groups such as hydrophilic groups imparted on the surface thereof.
[0117] The average fiber length of the microfibrous cellulose is, for example, 0.5 to 1.5 mm, preferably 0.5 to 1.2 mm, and particularly preferably 0.6 to 0.8 mm. The average fiber diameter of the microfibrous cellulose is, for example, 0.5 to 50 μm.
[0118] Examples of the aspect ratio of fine fibrous cellulose are preferably those described in the section "complex".
[0119] As the fine fibrous cellulose, for example, commercially available products such as "Celish", "Filter Master", "PC110S", and "PC110T" (all manufactured by Daicel Miraizu Corporation) can be used.
[0120] Through this step, the iron compound and the metal compound (or a mixed oxide of iron and the metal) as required can be adsorbed on the microfibrous cellulose. There are no particular restrictions on the manner in which the iron compound (when the iron compound and the metal compound are used together, the iron compound and the metal compound, or a mixed oxide of iron and the metal) is adsorbed on the microfibrous cellulose. For example, the iron compound can be adsorbed on the microfibrous cellulose in the form of ions.
[0121] (Hydrothermal treatment process)
[0122] This step is a step of heating the fine fibrous cellulose having adsorbed the iron compound in water.
[0123] The heat treatment temperature is, for example, 100 to 150° C. The heat treatment pressure is, for example, normal pressure to 5 atm, preferably normal pressure to 3 atm. The heat treatment time is, for example, 0.5 to 10 hours. The heat treatment can be performed using a known conventional heating method (for example, a heating block type heating decomposition system).
[0124] The heat treatment time is, for example, 0.5 to 10 hours, preferably 1 to 7 hours, and particularly preferably 3 to 7 hours. If the heat treatment time is extended within the above range, crystallization tends to be promoted.
[0125] By subjecting the fine fibrous cellulose having adsorbed an iron compound to a heat treatment in water, iron (III)-containing particles at least part of which are needle-shaped can be precipitated on the surface of the fine fibrous cellulose.
[0126] When an iron compound and a zirconium compound and / or a titanium compound are used together, after heat treatment, iron (III)-containing particles containing at least one iron compound selected from iron oxide, iron hydroxide and iron oxide (= water-insoluble trivalent iron compound) and an oxide, hydroxide or hydroxide of at least one metal selected from zirconium and titanium, at least a portion of which is in the shape of needles, can be precipitated on the surface of the microfibrous cellulose, or iron (III)-containing particles containing a mixed oxide of iron (III) and zirconium and / or titanium, at least a portion of which is in the shape of needles, can be precipitated on the surface of the microfibrous cellulose.
[0127] Through this step, a composite having a structure in which iron (III)-containing particles at least partly in the form of needles are supported on fine fibrous cellulose is obtained.
[0128] [Arsenic adsorbent]
[0129] The arsenic adsorbent disclosed in the present invention includes the composite. The arsenic adsorbent may also include other components other than the composite, and the proportion of the composite in the total amount of the arsenic adsorbent (or the total amount of non-volatile components contained in the arsenic adsorbent) is, for example, 50% by weight or more, preferably 60% by weight or more, more preferably 70% by weight or more, particularly preferably 80% by weight or more, most preferably 90% by weight or more, and particularly preferably 95% by weight or more. It should be noted that the arsenic adsorbent may also be composed only of the composite.
[0130] It should be noted that in the present disclosure, "non-volatile components" refers to the total weight of components other than solvents (including water or organic solvents), for example, components remaining after heating 1 g of arsenic adsorbent at 100° C. for 1 hour under normal pressure.
[0131] The shape of the arsenic adsorbent is not particularly limited as long as the effects of the present disclosure are not impaired, but is preferably in a gel, powder, or granular form from the viewpoint of facilitating recovery of arsenic from the aqueous solution after adsorbing the arsenic.
[0132] Since the arsenic adsorbent of the present disclosure includes the composite, it can be preferably used for adsorbing and removing arsenic (V) dissolved in water.
[0133] The arsenic adsorbent can be prepared by producing a composite using the composite production method, adding other components as needed, and performing molding as needed.
[0134] [Method for producing purified water]
[0135] The method for producing purified water disclosed in the present invention is a method for treating arsenic-contaminated water (water contaminated with arsenic, with an arsenic concentration of, for example, 5 mM or more) with the arsenic adsorbent (or the complex) to obtain purified water (for example, purified water in which 99% by weight or more (more preferably 99.9% by weight or more) of the arsenic contained in the contaminated water is removed).
[0136] Arsenic (V) exists in the form of arsenate ions in aqueous solution. In addition, the arsenic adsorbent (or the complex) adsorbs and recovers arsenic ions by complexing with arsenate ions via hydroxyl groups of arsenate ions with trivalent iron contained in the metal particles.
[0137] The method of treating contaminated water with the arsenic adsorbent is a method of adsorbing arsenic contained in the contaminated water onto the arsenic adsorbent. The method is not particularly limited, and examples thereof include a method of filling a chromatographic column with the arsenic adsorbent and flowing the contaminated water therein; a method of adding the arsenic adsorbent to the contaminated water and stirring the contaminated water; and the like.
[0138] When treating with the arsenic adsorbent, from the viewpoint of being able to more efficiently recover arsenic, the pH of the contaminated water is preferably adjusted to, for example, 10 or less (for example, 1 to 10, preferably 2 to 10), preferably 8 or less. The pH adjustment can be performed using a known and commonly used pH adjuster.
[0139] Furthermore, after arsenic is adsorbed on the arsenic adsorbent, the volume of the arsenic adsorbent can be significantly reduced by burning the arsenic adsorbent having adsorbed arsenic, thereby reducing the cost required for treatment.
[0140] According to the method for producing purified water of the present disclosure, arsenic can be efficiently removed from water contaminated with arsenic, and purified water free of arsenic contamination can be efficiently produced.
[0141] [Water purification device]
[0142] The water purification device of the present disclosure includes the above-mentioned arsenic adsorbent (or the above-mentioned complex).
[0143] The method for preparing the arsenic adsorbent is not particularly limited, but an example thereof includes a method in which the arsenic adsorbent is prepared in a state where it is filled in a chromatography column or the like.
[0144] Therefore, the water purification device may include a chromatographic column filled with the arsenic adsorbent.
[0145] The water purification device may include necessary structures such as a device for supplying water before purification to the arsenic adsorbent and a device for discharging water purified by the arsenic adsorbent, in addition to the arsenic adsorbent.
[0146] The water purification device includes the arsenic adsorbent, and thus can efficiently remove arsenic from arsenic-contaminated water, and can efficiently produce arsenic-free purified water.
[0147] The above configurations and combinations of the configurations disclosed herein are examples, and additions, omissions, substitutions, and changes to the configurations may be appropriately made without departing from the gist of the present disclosure. The present disclosure is not limited to the embodiments but only to the description of the claims.
[0148] Example
[0149] Hereinafter, the present disclosure will be described in more detail by way of examples, but the present disclosure is not limited to these examples.
[0150] Example 1
[0151] (Adsorption process)
[0152] To 50 mL of Digi-Tube, add 0.10 g of microfibrillated cellulose (average fiber length: 0.6-0.8 mm, reference fiber diameter: 0.5-50 μm, trade name "Filter Master", manufactured by Daicel Miraizu Co., Ltd.), 0.68 g (2.5 mmol) of FeCl3·6H2O, 0.41 g (2.9 mmol) of Na2SO4, and 50 mL of purified water, and stir at room temperature using a homogenizer (OMNI tissuehomogenizer TH, OMNI international) until the microfibrillated cellulose is completely dispersed.
[0153] The homogenizer used has a weaker shear force than, for example, a high-pressure homogenizer used for preparing cellulose nanofibers, thereby making it possible to stir / disperse microfibrillated cellulose with less energy consumption.
[0154] (Hydrothermal treatment process)
[0155] After stirring, the mixture was heated at 121° C. and two atmospheres of pressure for 4.0 to 5.0 hours using a heating block type thermal decomposition system.
[0156] After the heating is completed, the reaction product is filtered by suction, and the obtained filtrate is dried at 40° C. to obtain a composite (1) (Fe) containing particles (including 12% by weight or more of needle-shaped particles with a volume equivalent diameter of less than 1 μm and an aspect ratio of 2 or more) containing iron oxide (or iron oxide and iron oxyhydroxide) supported on microfibrillated cellulose. III -NN-cellulose microfibrils (CMF)). The SEM image of the obtained composite (1) is shown in Figure 1 .like Figure 1 As shown in the figure, when the composite was observed by SEM, needle-shaped particles were observed on the surface of the fine fibrous cellulose. At least 50 needle-shaped particles were observed in the circled portion within the field of view. The composite was a particle with a sharp tip on the surface of the fine fibrous cellulose, and the diameter (or width) of the particle became smaller as it approached the tip. It was observed that more than 80% of all the particles observed in the field of view were elongated particles with an aspect ratio of more than 8.
[0157] The amount of the iron (III)-containing particles supported per 1 g of fine fibrous cellulose in the composite was 2.5 mmol. The average value of the volume-equivalent diameters of ten needle-like particles randomly selected from the SEM image of the composite was 0.16 μm.
[0158] Example 2
[0159] (Adsorption process)
[0160] 0.10 g of microfibrillated cellulose (average fiber length: 0.6-0.8 mm, reference fiber diameter: 0.5-50 μm, trade name "Filter Master", manufactured by Daicel Miraizu Co., Ltd.), 0.68 g (2.5 mmol) of FeCl3·6H2O, 0.41 g (2.9 mmol) of Na2SO4, 0.088 g (0.27 mmol) of ZrCl2O·8H2O, and 50 mL of purified water were added to a 50 mL Digi-tube, and stirred at room temperature using a homogenizer (OMNI tissue homogenizer TH, OMNI international) until the microfibrillated cellulose was completely dispersed. (FeCl3 and ZrCl2O charging molar ratio [Fe / Zr (metal element conversion value)] 9 / 1)
[0161] (Hydrothermal treatment process)
[0162] After stirring, the mixture was heated at 120° C. for 5 hours using a heating block type thermal decomposition system.
[0163] After the heating was completed, the filtrate obtained by filtering was dried at 40° C. to obtain a composite (2) in which particles containing iron oxide (or iron oxide and iron oxyhydroxide) and zirconium oxide (including 13% by weight or more of needle-shaped particles having a volume equivalent diameter of less than 1 μm and an aspect ratio of 2 or more) and / or particles containing a mixed oxide of iron and zirconium (including 13% by weight or more of needle-shaped particles having a volume equivalent diameter of less than 1 μm and an aspect ratio of 2 or more) were supported on microfibrillated cellulose (Fe III / Zr(1.0)-NN-CMF). The SEM image of the obtained composite (2) is shown in Figure 2 and Figure 3 (a) (two different perspectives). Figure 2 and Figure 3 As shown in (a), the composite includes, on the surface of the fine fibrous cellulose, elongated particles with a sharp tip and an aspect ratio exceeding 2, and elongated particles whose diameter (or width) decreases toward the tip and whose aspect ratio exceeds 2. It was observed that more than 80% of all particles observed in the two fields of view were elongated particles with an aspect ratio exceeding 2.
[0164] The amount of the iron (III)-containing particles supported per 1 g of fine fibrous cellulose in the composite was 2.5 mmol. Figure 2 The average volume equivalent diameter of ten needle-shaped particles randomly selected from the Figure 3 The average value of the volume-equivalent diameters of ten needle-like particles randomly selected in (a) is 0.33 μm.
[0165] Example 3
[0166] A composite (3) (Fe III / Zr(1.0)-NN-CMF). The SEM image of the obtained composite (3) is shown in Figure 3 (b). Figure 3 As shown in (b), with respect to the composite, it was observed that, on the surface of the fine fibrous cellulose, elongated particles with a pointed tip and an aspect ratio exceeding 2, and elongated particles with a smaller diameter (or width) as they approach the tip and an aspect ratio exceeding 2, accounted for more than 90% of all particles observable in the observation field.
[0167] Example 4
[0168] A composite (4) (Fe III / Zr(1.0)-NN-CMF). The SEM image of the obtained composite (4) is shown in Figure 3 (c). Figure 3 The composite observed in the circled portion within the field of view of the SEM image of (c) is a particle with a sharp tip on the surface of the microfibrous cellulose, and the diameter (or width) of the particle decreases as it approaches the tip. It was observed that the elongated particles with an aspect ratio of more than 2 accounted for about 10% of all the particles observed in the field of view.
[0169] Example 5
[0170] In the (adsorption step), except that the charging amount of FeCl3·6H2O and ZrCl2O·8H2O was changed to 0.7 weight times, a composite (5) (Fe) containing particles of iron oxide (or iron oxide and iron hydroxide) and zirconium oxide (including 9 weight % or more of the total weight of the composite and having a volume equivalent diameter of less than 1 μm (measured value: 0.1 μm (100 nm)) and an aspect ratio of 2 or more (measured value: 4)) and / or particles of a mixed oxide of iron and zirconium (including 9 weight % or more of the total weight of the composite and having a volume equivalent diameter of less than 1 μm and an aspect ratio of 4) supported on microfibrillated cellulose was obtained in the same manner as in Example 2 (Fe III / Zr(0.7)-NN-CMF). The SEM image of the obtained composite (5) is shown in Figure 4 (5000 times), and the SEM image of another field of view is shown in Fig. 9 (30,000 times). Fig. 9As shown, the composite includes elongated particles with a sharp tip and an aspect ratio of 4 on the surface of the microfibrous cellulose, and elongated particles with a smaller diameter (or width) as they get closer to the tip and an aspect ratio of 4. It was observed that more than 90% of all particles observed in the two fields of view were elongated particles with an aspect ratio exceeding 4.
[0171] The amount of the iron (III)-containing particles supported per 1 g of fine fibrous cellulose in the composite was 1.8 mmol. The average value of the volume-equivalent diameters of ten needle-like particles randomly selected from the SEM image of the composite was 0.12 μm.
[0172] Example 6
[0173] In the (adsorption process), except that the charging amounts of FeCl3·6H2O and ZrCl2O·8H2O were changed to a molar ratio of FeCl3 to ZrCl2 [Fe / Zr (metal element conversion value)] of 1 / 1, a composite (6) (Fe) containing particles of iron oxide (or iron oxide and iron hydroxide) and zirconium oxide (including 13% by weight or more of needle-shaped particles with a volume equivalent diameter of less than 1 μm and an aspect ratio of 2 or more) and / or particles of a mixed oxide of iron and zirconium (including 13% by weight or more of needle-shaped particles with a volume equivalent diameter of less than 1 μm and an aspect ratio of 2) supported on microfibrillated cellulose was obtained in the same manner as in Example 2. III / Zr(1.0)-NN-CMF). The obtained composite contained elongated particles with a sharp tip and an aspect ratio of 2 or more, and elongated particles with a smaller diameter (or width) as they approach the tip and an aspect ratio of 2 or more on the surface of the fine fibrous cellulose. It was observed that more than 90% of all particles observed in the two fields of view were elongated particles with an aspect ratio of 2 or more.
[0174] The amount of the iron (III)-containing particles supported per 1 g of the fine fibrous cellulose in the composite was 1.4 mmol.
[0175] Example 7
[0176] In the (adsorption process), TiCl4 solution (33.8 μL: Ti (8.76 mg, 0.18 mmol)) (Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of ZrCl2O·8H2O. In the same manner as in Example 5, particles containing iron oxide and titanium oxide (including 8 wt % or more of needle-shaped particles with a volume equivalent diameter of 0.1 μm (100 nm) and an aspect ratio of 2) and / or mixed oxides containing iron and titanium (Fe x Ti y O z) particles (including 8 wt % or more of needle-shaped particles having a volume equivalent diameter of 0.1 μm (100 nm) and an aspect ratio of 2 or more) supported on microfibrillated cellulose (7) (Fe III / Ti(0.7)-NN-CMF). The SEM image of the obtained composite (7) is shown in Fig.10 . It should be noted that the charging amount of FeCl3·6H2O and TiCl4 solution is the same as that in Example 5, which is 0.7 times by weight, and the molar ratio of FeCl3 to TiCl4 [Fe / Ti (metal element conversion value)] is 9 / 1. The obtained composite contains elongated particles with a sharp tip and an aspect ratio of 2 or more, and elongated particles with a smaller diameter (or width) closer to the tip and an aspect ratio of 2 or more on the surface of the fine fibrous cellulose. It was observed that: among all the particles that could be observed in the two fields of observation, more than 90% were elongated particles with an aspect ratio of 2 or more.
[0177] The amount of the iron (III)-containing particles supported per 1 g of fine fibrous cellulose in the composite was 1.6 mmol. The average value of the volume-equivalent diameters of ten needle-like particles randomly selected from the SEM image of the composite was 0.10 μm.
[0178] Reference Example 1
[0179] A 10 wt% FeCl3·6H2O aqueous solution (10 mL) and a buffer solution (0.5 mol / L 2-(N-morpholine)ethanesulfonic acid) were added to the flask to make a total of 50 mL of the solution, which was adjusted to pH 6 using NaOH. Thus, iron (III)-containing particles (Fe III Particles) (volume equivalent diameter: 1 μm). 10 mL of the adjusted solution and 0.10 g of cellulose nanofibers (average fiber length: 0.6-0.8 mm, reference fiber diameter: 0.5-50 μm, trade name "Filter Master", manufactured by Daicel Miraizu Co., Ltd.) were added, and stirred at room temperature for 1.0 hour using a stirrer. Then, the solid component was obtained by suction filtration, and the obtained solid component was dried to obtain a composite (8) in which iron (III)-containing particles were supported on cellulose nanofibers (Fe III -CMF). The SEM image of the obtained composite (8) is shown in Figure 5 .like Figure 5 As shown, the surface of the fine fibrous cellulose contained cubic particles having an aspect ratio of 1. It was observed that more than 90% of all particles observed in the observed field of view were cubic particles having an aspect ratio of 1.
[0180] The amount of the iron (III)-containing particles supported per 1 g of fine fibrous cellulose in the composite was 3.3 mmol. The volume equivalent diameter of the particles contained in the composite was 1.24 μm.
[0181] Comparative Example 1
[0182] 10 mL of 10 wt % FeCl3, 10 mL of 1.0 wt % ZrCl2O and buffer solution were added to the flask and stirred at room temperature for 0.5 hours using a stirrer. Next, the solution was heated to 60°C and NaOH was added to adjust the pH to 6.0, and then stirred for 30 minutes. The solid component was obtained by suction filtration, and the obtained solid component was dried to obtain particles containing iron oxide (or iron oxide and iron hydroxide) and zirconium oxide (the molar ratio of FeCl3 to ZrCl2 [Fe / Zr (metal element conversion value)] = 10 / 1 and the aspect ratio of needle-shaped particles of 2 or more could not be confirmed) and / or particles containing mixed oxides of iron and zirconium (the molar ratio of FeCl3 to ZrCl2 [Fe / Zr (metal element conversion value)] = 10 / 1 and the aspect ratio of needle-shaped particles of 2 or more could not be confirmed).
[0183] Comparative Example 2
[0184] 10 wt % FeCl3 and a buffer solution were added to the flask, and NaOH was added at room temperature to adjust the resulting solution to the target pH. The mixture was then stirred for 30 minutes, and a solid component was obtained by suction filtration. The obtained solid component was dried to obtain particles containing iron oxide (or iron oxide and iron oxyhydroxide) (needle-shaped particles with an aspect ratio of 2 or more could not be confirmed).
[0185] The composites of Examples and the particles of Comparative Examples were evaluated as follows.
[0186] (Evaluation 1)
[0187] 0.010 g of the composite of the example or the particles of the comparative example were mixed with 10 mL of water at room temperature, and stirred with a stirrer for 10 minutes to evaluate the dispersibility.
[0188] As a result, the composite obtained in the example obtained a uniform dispersion and aggregation was suppressed. It can be seen that the composite disclosed in the present invention can maintain a large surface area of the iron (III)-containing particles in water that contributes to arsenic adsorption. On the other hand, the particles of the comparative example aggregated and precipitated.
[0189] (Rating 2)
[0190] The composite obtained in the example and the Fe III / Zr particles, and the adsorption capacity of arsenic (V) was determined by the following method.
[0191] In a 100 mL centrifuge tube, 10 mL of a 1000 mg / L As(V) aqueous solution (pH 7) and 0.010 g of the composite of the example or the particles of the comparative example were added, and the mixture was stirred at 25° C. for 20 minutes using a shaker.
[0192] The solution was filtered using a membrane filter (nitrocellulose, pore size: 0.45 μm), and the arsenic ion concentration (Ce: mol / L) in the filtrate was quantified using an ICP emission spectrometer (iCAP6300 manufactured by ThermoFischer Scientific). The initial concentration of arsenic ions in the solution was set as C0 (μmol / L), the amount of liquid added was set as V0 (L), and the weight of the arsenic adsorbent used was set as m (g), and the adsorption capacity (μmol / g) was calculated according to the following formula.
[0193] Adsorption capacity = (C0-Ce) × V0 / m
[0194] (Rating 3)
[0195] Regarding the composites obtained in Examples, the volume reduction rate was measured by the following method.
[0196] 0.10 g (w1) of the composite was burned at 800°C for 1 hour, the weight of the ash remaining after the combustion was measured (w2), and the volume reduction rate was calculated according to the following formula.
[0197] Volume reduction rate (%) = (w1-w2) / w1×100
[0198] The results are shown in Table 1 below.
[0199] [Table 1]
[0200]
[0201]
[0202] As can be seen from Table 1, if needle-shaped particles containing iron oxide are supported on the surface of fine fibrous cellulose, the arsenic adsorption amount is significantly improved. In addition, it can be seen that if needle-shaped particles containing iron oxide and zirconium oxide (and / or a mixed oxide of iron and zirconium), or iron oxide and titanium oxide (and / or a mixed oxide of iron and titanium) are supported on the surface of fine fibrous cellulose, the arsenic adsorption capacity is further improved.
[0203] Furthermore, it is known that the composite of the present invention can efficiently adsorb and recover arsenic in the solution, can significantly reduce the arsenic concentration in the solution, and after arsenic is adsorbed on the composite, the volume can be significantly reduced by calcination, which can significantly reduce the cost required for treatment such as landfill.
[0204] (Rating 4)
[0205] The composite obtained in the example was filled into a Teflon tube with an inner diameter of 2 mm and a length of 5 cm, and both ends were filled with Teflon wool to prepare a solid phase chromatography column. An arsenic removal test was carried out using the column.
[0206] 20 mL of 0.1 mol / L buffer was passed into the solid phase chromatography column to adjust the pH in the column. Then, 5 mL of arsenic-containing buffer (initial arsenic concentration C0 = 5 μmol / L) was passed at a flow rate of about 1 mL / min, and the arsenic ion concentration (C0) in the distillate and the arsenic-containing buffer was measured using an ICP emission spectrometer (iCAP6300 manufactured by Thermo Fischer Scientific). e : μmol / L) for quantification. The initial concentration of arsenic ions in the distillate was set to C0 (μmol / L), and the removal rate (%) was calculated according to the following formula. As a result, for all the composites (1), (2), (5), (6), and (7), 99.9% by weight of arsenic in the aqueous solution could be removed.
[0207] Removal rate (%) = (C0-C e ) / C0×100
[0208] (Rating 5)
[0209] For the composite (1), an arsenic aqueous solution (initial arsenic concentration: 10 μmol / L) whose pH was adjusted to 2 to 12 using 0.01 mol / L nitric acid or a buffer solution was prepared, and the pH dependence of the arsenic removal rate was evaluated.
[0210] 0.02 g of the complex (1) was added to 10 mL of the arsenic aqueous solution, and the mixture was stirred at 25° C. for 20 minutes using a shaker. The mixture was filtered using a membrane filter (nitrocellulose, pore size: 0.45 μm), and the arsenic ion concentration (C 2 ) in the filtrate was measured using an ICP emission spectrometer (iCAP6300 manufactured by Thermo Fischer Scientific). e The initial concentration of arsenic ions in the solution was set to C0 (μmol / L), and the removal rate (%) was calculated according to the following formula.
[0211] Removal rate (%) = (C0-C e ) / C0×100
[0212] The buffer was prepared using acetic acid (pH 3-5), 2-(N-morpholine)-ethanesulfonic acid (pH 6), 4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid (pH 7-8), ammonium chloride (pH 9), 3-[N-tris(hydroxymethyl)methyl-3-amino]-1-propanesulfonic acid (pH 9), 3-cyclohexylaminopropanesulfonic acid (pH 10-12) and sodium hydroxide.
[0213] The results are shown in Figure 6 .Depend on Figure 6 It is found that the composite (2) obtained in the example shows an arsenic adsorption rate exceeding 90% at a pH of 10 or less, and it is found that the composite (2) shows an arsenic adsorption rate close to 100% at a pH of 8 or less.
[0214] (Rating 6)
[0215] For complex (2), sodium chloride, sodium sulfate, sodium phosphate, and the buffer solution (refer to Evaluation 5) were used to prepare arsenic aqueous solutions (initial arsenic concentration: 10 μmol / L, pH 3) in which chloride ions, sulfate ions, and phosphate ions coexisted at concentrations of 0.1 mmol / L, 1 mmol / L, or 100 mmol / L, and the changes in arsenic removal rate under the coexistence of anions were evaluated.
[0216] 0.02 g of the complex (2) was added to 10 mL of the arsenic aqueous solution, and the mixture was stirred at 25° C. for 20 minutes using a shaker. The arsenic ion concentration (C e The arsenic adsorption rate was calculated to confirm the change of the arsenic adsorption rate of the complex (2) in the presence of anions.
[0217] Removal rate = (C0-C e ) / C0×100
[0218] The results are shown in Figure 7 .Depend on Figure 7 It is found that the complex (2) obtained in the example efficiently adsorbs arsenic (V) even when anions coexist (especially phosphorus, which has chemical properties similar to those of arsenic).
[0219] (Rating 7)
[0220] For complexes (1), (2), (5), (6), and (7), trivalent iron was eluted in the form of iron (III) ions by adding hydrochloric acid, and the concentration of iron (III) ions in the eluate was measured to evaluate the total amount of iron carried per 1 g of fine fibrous cellulose (converted into iron element value).
[0221] Add 0.01 g of the complex (1) and 5 mL of 6 mol / L hydrochloric acid to a 50 mL centrifuge tube and stir at room temperature for 20 minutes using an oscillator. Filter using a membrane filter (nitrocellulose, pore size: 0.45 μm) and quantify the iron ion concentration (Ce: mol / L) in the filtrate using an ICP emission spectrometer (iCAP6300 manufactured by ThermoFischer Scientific). The weight of the complex is set to m (g), the amount of hydrochloric acid used is set to V (mL), and the total amount of iron supported per 1 g of the complex (converted value of the iron element) is evaluated according to the following formula.
[0222] Total loading = Ce × V / m
[0223] The weight of the fine fibrous cellulose was evaluated by subtracting the iron loading amount determined as described above from the weight of the composite, and the iron loading amount per 1 g of the fine fibrous cellulose was calculated (iron content per 1 g of CMF, Table 1).
[0224] As a summary of the above, the configuration of the present disclosure and its modifications are described below.
[0225] [1] A composite comprising fine fibrous cellulose and iron (III)-containing particles supported on the fine fibrous cellulose, wherein at least a portion of the iron (III)-containing particles have an aspect ratio of 2 or more.
[0226] [2] The composite according to [1], wherein the amount of the iron (III)-containing particles supported per 1 g of the fine fibrous cellulose (calculated as iron element) is 1 to 100 mmol.
[0227] [3] The composite according to [1] or [2], wherein the fine fibrous cellulose is microfibrillated cellulose.
[0228] [4] The composite according to any one of [1] to [3], wherein the particle diameter of a volume equivalent sphere of the iron (III)-containing particle is less than 1 μm.
[0229] [5] The composite according to any one of [1] to [4], wherein the iron (III)-containing particles contain at least one iron compound selected from the group consisting of iron oxide, iron hydroxide, and iron oxyhydroxide.
[0230] [6] A composite according to any one of [1] to [5], wherein the iron (III)-containing particles contain at least one iron compound selected from iron oxide, iron hydroxide and iron oxyhydroxide, and an oxide, hydroxide or oxyhydroxide of at least one metal selected from zirconium and titanium, and the molar ratio [iron / (zirconium and / or titanium)] of the iron compound (converted value as iron element) to the oxide, hydroxide or oxyhydroxide of the metal (converted value as metal element; the total amount when two or more are contained) is 1 to 100.
[0231] [7] A method for producing a composite, comprising mixing fine fibrous cellulose and an iron compound in water in the presence of a crystal medium, allowing the iron compound to adsorb to the fine fibrous cellulose, and then subjecting the mixture to a heat treatment to produce a composite as described in any one of [1] to [6].
[0232] [8] The method for producing a composite according to [7], wherein in the step of adsorbing the iron compound on the fine fibrous cellulose, the iron compound and at least one metal compound selected from the group consisting of a zirconium compound and a titanium compound are adsorbed together.
[0233] [9] An arsenic adsorbent comprising the composite according to any one of [1] to [6].
[0234]
[10] Use of the complex described in any one of [1] to [6] as an arsenic adsorbent.
[0235]
[11] A method for producing purified water, wherein purified water is obtained by treating arsenic-contaminated water with the arsenic adsorbent described in [9].
[0236]
[12] A method for producing purified water, comprising treating arsenic-contaminated water with the composite according to any one of [1] to [6] to obtain purified water.
[0237]
[13] A water purification device comprising the arsenic adsorbent described in [9].
[0238]
[14] A water purifier comprising the composite body according to any one of [1] to [6].
[0239]
[15] A method for using the composite described in any one of [1] to [6] as an arsenic adsorbent.
[0240] Industrial Applicability
[0241] The composite disclosed in the present invention can efficiently adsorb and recover arsenic dissolved in water. Furthermore, by burning the adsorbed arsenic to reduce its volume, the cost required for treatment such as landfill can be greatly reduced. Therefore, the composite can be preferably used for purification of water contaminated by arsenic.
[0242] Description of Reference Numerals
[0243] 1: Microfibrous cellulose;
[0244] 2: Particles containing iron (III).
Claims
1. A composite comprising fine fibrous cellulose and iron (III)-containing particles supported on the fine fibrous cellulose, At least a portion of the iron (III)-containing particles are particles having an aspect ratio of 2 or more.
2. The composite according to claim 1, wherein The amount of the iron (III)-containing particles supported per 1 g of the fine fibrous cellulose, ie, the iron element conversion value, is 1 to 100 mmol.
3. The complex according to claim 1 or 2, wherein: The microfibrous cellulose is microfibrillated cellulose.
4. The complex according to claim 1 or 2, wherein: The iron (III)-containing particles contain at least one iron compound selected from the group consisting of iron oxide, iron hydroxide, and iron oxyhydroxide.
5. The complex according to claim 1 or 2, wherein: The iron (III)-containing particles contain at least one iron compound selected from iron oxide, iron hydroxide and iron oxyhydroxide, and an oxide, hydroxide or oxyhydroxide of at least one metal selected from zirconium and titanium. The molar ratio of the iron compound calculated as iron element to the oxide, hydroxide or oxyhydroxide of the metal calculated as metal element, i.e., iron / (zirconium and / or titanium), is 1 to 100. The metal element conversion value refers to the total amount of the oxides, hydroxides or oxyhydroxides of two or more of the metals when the particles contain the oxides, hydroxides or oxyhydroxides.
6. The complex according to claim 1 or 2, wherein: The particle diameter of a volume equivalent sphere of the iron (III)-containing particles is less than 1 μm.
7. A method for producing a composite, wherein: The composite according to claim 1 or 2 is produced by mixing fine fibrous cellulose and an iron compound in water in the presence of a crystal modifier, allowing the iron compound to adsorb to the fine fibrous cellulose, and then subjecting the mixture to a heat treatment.
8. The method for producing a composite according to claim 5, wherein: In the step of adsorbing the iron compound on the fine fibrous cellulose, the iron compound and at least one metal compound selected from the group consisting of a zirconium compound and a titanium compound are adsorbed together.
9. An arsenic adsorbent, comprising the composite according to claim 1 or 2.
10. A method for producing purified water, wherein: Arsenic-contaminated water is treated with the arsenic adsorbent as claimed in claim 9 to obtain purified water. 11 . A water purification device comprising the arsenic adsorbent according to claim 9 .