Alloy material for probe
A probe material with controlled Pd, Ag, Ni, and Cu composition forms a dense intermetallic layer to inhibit diffusion, addressing wear and resistance issues, improving detection efficiency.
Patent Information
- Application Number
- CN202380030021.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-02
- Publication Date
- 2024-12-03
AI Technical Summary
Existing probe materials, such as AgPdCu alloys, experience accelerated wear and poor contact resistance due to solder component diffusion during repeated use, leading to inefficient detection processes.
A probe material composed of specific proportions of Pd, Ag, Ni, and Cu, optionally with In, Sn, or Zn, forms a dense intermetallic compound layer to inhibit solder and probe material diffusion, maintaining hardness and reducing wear.
The new alloy composition effectively suppresses solder and probe material diffusion, ensuring high hardness and stable contact resistance, enhancing detection efficiency by preventing tip wear.
Smart Images

Figure BDA0005057386290000061 
Figure BDA0005057386290000071
Abstract
Description
Technical Field
[0001] The present invention relates to an alloy material for a probe pin (hereinafter referred to as a "probe material") for detecting electrical characteristics of an integrated circuit or a liquid crystal display device on a semiconductor wafer. Background Art
[0002] In the detection of electrical characteristics of integrated circuits or liquid crystal display devices formed on semiconductor wafers, a socket or probe card equipped with multiple probes is used. This detection is performed by bringing the probe needles assembled in the socket or probe card into contact with electrodes, terminals, or conductive parts of the integrated circuit or liquid crystal display device.
[0003] This type of probe needle requires low contact resistance and hardness that can withstand repeated contact. As the probe material, beryllium copper alloy or tungsten, tungsten alloy, platinum alloy, palladium alloy, etc. are used.
[0004] Patent Document 1 discloses a palladium alloy (hereinafter referred to as an AgPdCu alloy) composed of 16% to 50% copper, about 35% to about 59% palladium, and 4% or more silver.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: U.S. Patent No. 1935897 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In the past, AgPdCu alloys with excellent plastic workability and precipitation hardening were used as probe materials due to their shape stability and low resistivity characteristics derived from their hardness. However, when used in circuit connections using solder (e.g., Sn-Bi solder), the following issues arise. That is, since the probe needle repeatedly contacts and energizes the solder during detection, solder components such as Sn and components of the probe material diffuse with each other due to Joule heat, etc., and the wear of the probe needle tip tends to accelerate. In this case, since the contact resistance changes suddenly or over time, poor detection may occur, and therefore the contact tip needs to be cleaned or replaced, which reduces the working efficiency of the detection step.
[0010] Therefore, there is an urgent need to develop a probe material having solder resistance that can suppress diffusion of solder components.
[0011] An object of the present invention is to provide a probe material which can suppress diffusion of components of the probe material and solder in a circuit connection portion to be inspected during probe inspection.
[0012] Technical solutions to solve problems
[0013] The present invention has been completed by discovering a probe material characterized by being composed of greater than 20 mass % and less than 60 mass % of Pd, 3 mass % or more and less than 20 mass % of Ag, 3 mass % or more and less than 50 mass % of Ni, and 3 mass % or more and less than 74 mass % of Cu.
[0014] The present invention was also completed by discovering a probe material characterized by being composed of greater than 20 mass % and less than 60 mass % of Pd, 20 mass % to 35 mass % of Ag, 7 mass % to 50 mass % and less than 3 mass % of Cu.
[0015] Among the above, at least one of In, Sn, Zn, and Ga may be contained in a total amount of 0.2 mass % or more and 2.0 mass % or less in place of a part of Cu.
[0016] Effects of the Invention
[0017] According to the present invention, it is possible to provide a probe material that suppresses diffusion of solder and components of the probe material in a circuit connection portion to be inspected during inspection. DETAILED DESCRIPTION
[0018] Mode for carrying out the invention
[0019] The first invention of the present invention is a probe material, characterized in that it is composed of Pd greater than 20 mass% and less than 60 mass%, Ag greater than 3 mass% and less than 20 mass%, Ni greater than 3 mass% and less than 50 mass%, and Cu greater than 3 mass% and less than 74 mass%.
[0020] Furthermore, the second invention of the present invention is a probe material, characterized in that it is composed of Pd greater than 20 mass% and less than 60 mass%, Ag greater than 20 mass% and less than 35 mass%, Ni greater than 7 mass% and less than 50 mass%, and Cu greater than 3 mass% and less than 53 mass%.
[0021] Among the above, at least one of In, Sn, Zn, and Ga may be contained in a total amount of 0.2 mass % or more and 2.0 mass % or less in place of a part of Cu.
[0022] Pd has excellent corrosion resistance, but its corrosion resistance is insufficient when it is less than 20 mass %. On the other hand, if Pd exceeds 60 mass %, it is not suitable because it cannot fully suppress the diffusion of components of solder and probe material.
[0023] As another embodiment, the Pd content may be 22 to 55% by mass. As another embodiment, the Pd content may be 25 to 50% by mass.
[0024] Adding Ni to the alloy can improve the solder resistance of the alloy. According to experiments, the required amount of addition varies depending on the Ag content.
[0025] In the first invention, since the amount of Ag added is as small as less than 20 mass %, when Ni is less than 3 mass %, the diffusion of the components of the solder and the probe material cannot be fully suppressed, and if Ni exceeds 50 mass %, plastic working such as cold rolling and wire drawing becomes difficult.
[0026] In the second invention, since the amount of Ag added is as high as 20 mass % or more, when Ni is less than 7 mass %, the diffusion of components of solder and probe material cannot be fully suppressed, and when Ni is more than 50 mass %, plastic working such as cold rolling and wire drawing becomes difficult.
[0027] In the case of the first invention, as another embodiment, the Ni content may be 5 to 40 mass %. Furthermore, as another embodiment, the Ni content may be 7 to 35 mass %.
[0028] In the case of the second invention, as another embodiment, the Ni content may be 8 to 40 mass %. As another embodiment, the Ni content may be 10 to 35 mass %. As another embodiment, the Ni content may be 11 to 35 mass %.
[0029] Ag is added in combination with Pd and Cu to enhance age hardening, but the effect is insufficient when it is less than 3 mass %, and it is not suitable because the diffusion of components of solder and probe material cannot be sufficiently suppressed when it exceeds 35 mass %.
[0030] In the case of the first invention, as another embodiment, Ag may be 4 mass % to 18 mass %.
[0031] In the case of the second invention, as another embodiment, the content of Ag may be 21 to 33% by mass.
[0032] Cu has the effect of increasing hardness by forming an alloy with Pd in addition to having low resistivity. On the other hand, if a large amount is added, the corrosion resistance decreases. Therefore, when it is less than 3% by mass, sufficient hardness cannot be obtained, and when it is greater than 74% by mass, the corrosion resistance decreases.
[0033] In the case of the first invention, as another embodiment, the Cu content may be 5 to 70 mass %. As another embodiment, the Cu content may be 10 to 60 mass %. As another embodiment, the Cu content may be 15 to 50 mass %.
[0034] In the case of the second invention, as another embodiment, the Cu content may be 5 to 47 mass %. Furthermore, as another embodiment, the Cu content may be 10 to 40 mass %.
[0035] Adding at least one of In, Sn, Zn, and Ga will further improve age hardening, but when it is less than 0.2 mass%, there is almost no difference from no addition, and when it is added more than 2 mass%, plastic processing such as cold rolling and wire drawing will become difficult.
[0036] As another aspect, the total content of at least one of In, Sn, Zn, and Ga may be 0.3 to 1.5 mass %.
[0037] For the alloy of the present invention, it is important to suppress the phenomenon of wear of the probe tip caused by the diffusion of the components of the solder and the probe material. The hardness does not need to be as high as that of the existing AgPdCu alloy, but as the number of detections increases, the contact surface sometimes mechanically collapses, so it is desired to be hard. It can be used at 200HV or more, but the alloy of the present invention can obtain a hardness of 250HV or more. In addition to work hardening caused by processing, the increase in hardness can also be due to the increase in hardness due to aging treatment.
[0038] In the alloy of the present invention, the diffusion of the components of the solder and the probe material is suppressed, presumably for the following reason. That is, it is believed that the Ni added to the probe material forms a thin and dense intermetallic compound layer such as Sn-Ni at the contact interface between the solder and the probe needle, which has the effect of hindering the diffusion of the components of the solder and the probe material, thereby suppressing the easy wear of the probe needle tip.
[0039] Example
[0040] The embodiments of the present invention are described.
[0041] First, Ag, Pd, Cu, Ni, In, Sn, Zn, and Ga were mixed to the composition shown in Table 1, and then melted by arc melting in an argon atmosphere to produce alloy ingots. The composition and properties of the alloys of the Examples and Comparative Examples are shown in Table 1.
[0042] Each of the alloy ingots was repeatedly rolled and heat treated to prepare a plate having a rolling ratio [=((thickness before rolling-thickness after rolling) / thickness before rolling)×100] of 75% as a test piece for evaluating hardness and solder resistance.
[0043] At this time, as a workability investigation, the evaluation of the sheet material with a rolling ratio of 75% was ○, and the evaluation of the sheet material that could not be produced was ×. For alloy compositions that could not produce a sheet material with a rolling ratio of 75% and whose workability was × (Comparative Examples 4 and 9), no subsequent tests were performed.
[0044] The test pieces of each alloy produced were subjected to the following evaluations. Table 2 shows the results.
[0045] The hardness is measured by using a Micro-Vickers hardness tester at the center of the cross section of the test piece, with a load of 200 gf and a holding time of 10 seconds. The hardness at this time is called "processed material hardness". In addition, the center of the cross section of the test piece (called aged material) that has been aged at 300-400°C for 1 hour is measured using a Micro-Vickers hardness tester at a load of 200 gf and a holding time of 10 seconds. The hardness at this time is called "aged material hardness".
[0046] Solder resistance is measured by placing Sn-Bi solder on a test piece (10mm×10mm×thickness 0.5mm) and heat treating it at 250℃ for 1h in a N2 gas environment to melt the solder on the test piece. After heat treatment, the test piece is embedded in a resin to expose the cross section, and the interface between the solder and the test piece is analyzed vertically by EPMA. The layer where Sn and Pd coexist is regarded as a diffusion layer due to the mutual diffusion of Sn from the solder and Pd from the alloy, and its thickness is measured.
[0047] The thinner the measured diffusion layer thickness is, the higher the solder resistance is judged to be. Alloys with a diffusion layer thickness of less than 100 μm are evaluated as ◎, alloys with a diffusion layer thickness of 100 to 200 μm are evaluated as ○, and alloys with a diffusion layer thickness of 200 μm or more are evaluated as ×. The evaluation results are shown in Table 2.
[0048] The resistivity was calculated by measuring the resistance of each sample at room temperature and using Formula 1 as the test piece, with a rolling ratio of 90% [= ((thickness before rolling - thickness after rolling) / thickness before rolling) × 100].
[0049] Formula 1: Resistivity = (resistance × cross-sectional area) / measurement length [Table 1]
[0050] Table 1
[0051]
[0052] [Table 2]
[0053] Table 2
[0054]
[0055] The above results show that the alloy produced according to the present invention has high solder resistance and has the hardness, age hardening ability and resistivity required for probe materials. Therefore, according to the present invention, a material suitable as a probe material with solder resistance can be provided.
Claims
1. An alloy material for a detection needle, Its characteristics are: It is composed of the following ingredients: More than 20 mass % and less than 60 mass % of Pd, 3 mass % or more and less than 20 mass % of Ag, 3 mass % to 50 mass % Ni, and 3 mass % to 74 mass % Cu.
2. The alloy material for a probe needle according to claim 1, Its characteristics are: At least one of In, Sn, Zn, and Ga is contained in an amount of 0.2 mass % to 2.0 mass % in substitution for a portion of Cu.
3. An alloy material for a detection needle, Its characteristics are: It is composed of the following ingredients: More than 20 mass % and less than 60 mass % of Pd, 20 mass % or more and 35 mass % or less of Ag, 7 mass % to 50 mass % Ni, and 3 mass % or more and 53 mass % or less of Cu.
4. The alloy material for a probe needle according to claim 3, Its characteristics are: At least one of In, Sn, Zn, and Ga is contained in an amount of 0.2 mass % to 2.0 mass % in substitution for a portion of Cu.
Citation Information
Patent Citations
Precious metal alloy
US1935897A
Cited By
High-hardness and high-strength palladium-silver-copper-nickel quaternary alloy rod for probe and preparation method thereof
CN121087343A
A high-hardness and high-strength palladium-silver-copper-nickel quaternary alloy rod for a probe and a preparation method thereof