Separator for non-aqueous secondary battery, and non-aqueous secondary battery

By using a heat-resistant porous layer of aromatic resin and inorganic particles and an adhesive layer containing phenyl acrylic resin in a non-aqueous secondary battery, the problems of adhesiveness and gas generation of electrodes and separators are solved, and the problem of gas generation is achieved. Improve battery stability and performance.

CN119072822APending Publication Date: 2024-12-03TEIJIN LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035709.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing non-aqueous secondary batteries are prone to gas generation during charging and discharging, resulting in changes in the distance between electrodes and short circuits. It is difficult for dry and wet hot pressing methods to achieve good adhesion between the electrodes and the separator at the same time.

Method used

The separator is made of a heat-resistant porous layer containing an aromatic resin and inorganic particles and an adhesive layer containing a phenyl acrylic resin. The strong adhesion between the electrode and the separator is ensured by dry or wet hot pressing technology, and the strong adhesion between the electrode and the separator is suppressed. Gas generation.

Benefits of technology

Excellent adhesion between the electrode and the separator under dry and wet hot pressing conditions is achieved, gas generation is reduced, and the performance stability and manufacturing yield of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005096575170000541
    Figure BDA0005096575170000541
  • Figure BDA0005096575170000551
    Figure BDA0005096575170000551
  • Figure BDA0005096575170000561
    Figure BDA0005096575170000561
Patent Text Reader

Abstract

A separator for a non-aqueous secondary battery according to one embodiment of the present invention is provided with: a heat-resistant porous layer containing an aromatic resin and inorganic particles; and an adhesive layer that is provided on the heat-resistant porous layer and contains adhesive resin particles containing a phenyl group-containing acrylic resin, the adhesive resin particles containing a phenyl group-containing acrylic resin adhere to the heat-resistant porous layer, and the inorganic particles contain barium sulfate particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a separator for a nonaqueous secondary battery and a nonaqueous secondary battery. Background Art

[0002] Non-aqueous secondary batteries represented by lithium-ion secondary batteries have been widely used as power sources for portable electronic devices such as laptop computers, mobile phones, digital cameras, and video cameras. In addition, non-aqueous secondary batteries represented by lithium-ion secondary batteries are also being studied for their high energy density as batteries for power storage or electric vehicles.

[0003] As non-aqueous secondary batteries become more widespread, there is an increasing demand for ensuring safety and stable battery characteristics. As a specific measure for ensuring safety and stable battery characteristics, there is an example of improving the adhesion between the electrode and the separator.

[0004] As a separator having improved adhesion to an electrode, a separator having an adhesive layer containing a resin having adhesion to an electrode is known. For example, the separators disclosed in Patent Documents 1 and 2 have both a heat-resistant porous layer and an adhesive layer.

[0005] Patent Document 1: International Publication No. 2019 / 130994

[0006] Patent Document 2: International Publication No. 2020 / 246497 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, the manufacturing method of a battery using a separator having an adhesive layer that shows adhesion to the electrode includes: a method of hot pressing a stack formed by arranging the separator between the positive electrode and the negative electrode in a manner that does not contain an electrolyte impregnation in the separator (hereinafter also referred to as "dry hot pressing"); and a method of housing the stack formed by arranging the separator between the positive electrode and the negative electrode in an outer packaging material and hot pressing the stack in a state where the separator is impregnated with an electrolyte (hereinafter also referred to as "wet hot pressing").

[0009] If the electrode and the diaphragm are well bonded by dry hot pressing, the electrode and the diaphragm are not easily misaligned during the manufacturing process of the battery, which can improve the manufacturing yield of the battery. However, even if the electrode and the diaphragm are bonded by dry hot pressing, there is a case where the electrode and the diaphragm are peeled off when the electrolyte is impregnated. If the electrode and the diaphragm are peeled off, there is a case where a short circuit occurs due to external impact, expansion and contraction of the electrode accompanying charging and discharging, etc. Therefore, it is expected to develop a technology that can bond the battery and the diaphragm well by any of dry hot pressing and wet hot pressing.

[0010] Furthermore, if the non-aqueous secondary battery is repeatedly charged and discharged, gas is generated in the battery due to the decomposition of the electrolyte or electrolyte, and the distance between the positive electrode and the negative electrode of the non-aqueous secondary battery will be biased, so that the uniformity of the charge and discharge reaction is sometimes lost. In addition, if the non-aqueous secondary battery expands and deforms due to gas generation, a short circuit is sometimes generated. Therefore, in order to stabilize the performance of the non-aqueous secondary battery, it is important to suppress the generation of gas in the battery.

[0011] The present disclosure has been made in view of the above-mentioned circumstances.

[0012] An object of one embodiment of the present disclosure is to provide a non-aqueous secondary battery separator that has excellent adhesion to an electrode and suppresses gas generation in both dry hot pressing and wet hot pressing.

[0013] Another embodiment of the present disclosure is to provide a non-aqueous secondary battery including the non-aqueous secondary battery separator.

[0014] Means for solving problems

[0015] Specific means for solving the problem include the following methods.

[0016] <1> A separator for a non-aqueous secondary battery, comprising:

[0017] A heat-resistant porous layer, the heat-resistant porous layer containing an aromatic resin and inorganic particles;

[0018] an adhesive layer provided on the heat-resistant porous layer and containing adhesive resin particles comprising a phenyl-containing acrylic resin, wherein the adhesive resin particles comprising a phenyl-containing acrylic resin are attached to the heat-resistant porous layer,

[0019] The inorganic particles include barium sulfate particles.

[0020] <2> The non-aqueous secondary battery separator as described in <1>, wherein the adhesive resin particles comprising a phenyl-containing acrylic resin are at least one selected from the group consisting of (i) resin particles that are a copolymer comprising an acrylic monomer unit and a styrene monomer unit, and (ii) resin particles that are a mixture of an acrylic resin and a styrene resin.

[0021] <3> The nonaqueous secondary battery separator according to <1> or <2>, wherein the adhesion amount of the adhesive resin particles comprising the phenyl-containing acrylic resin on the heat-resistant porous layer is 0.1 g / m 2 ~5.0g / m 2 .

[0022] <4> The nonaqueous secondary battery separator according to any one of <1> to <3>, wherein the adhesive layer has a phenyl group peak area S1 of 0.01 to 3 and a carbonyl group peak area S2 of 4 or less as measured by Fourier transform infrared spectroscopy.

[0023] <5> The nonaqueous secondary battery separator according to any one of <1> to <4>, wherein the aromatic resin includes at least one selected from the group consisting of wholly aromatic polyamides, polyamideimides, and polyimides.

[0024] <6> The nonaqueous secondary battery separator according to any one of <1> to <5>, wherein the inorganic particles have an average primary particle size of 0.01 μm or more and 1 μm or less.

[0025] <7> The nonaqueous secondary battery separator according to any one of <1> to <6>, further comprising a porous substrate, wherein the heat-resistant porous layer is provided on one or both surfaces of the porous substrate.

[0026] <8> A nonaqueous secondary battery comprising a positive electrode, a negative electrode, and the nonaqueous secondary battery separator according to any one of <1> to <7> disposed between the positive electrode and the negative electrode, wherein the nonaqueous secondary battery obtains an electromotive force by doping and dedoping lithium.

[0027] Effects of the Invention

[0028] According to one embodiment of the present disclosure, a non-aqueous secondary battery separator is provided which has excellent adhesion to an electrode and suppresses gas generation in both dry hot pressing and wet hot pressing.

[0029] According to another embodiment of the present disclosure, a nonaqueous secondary battery including the nonaqueous secondary battery separator is provided. DETAILED DESCRIPTION

[0030] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are examples of the embodiments and do not limit the scope of the embodiments.

[0031] In the present disclosure, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0032] In the numerical range recorded in stages in this disclosure, the upper limit or lower limit recorded in one numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in this disclosure, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment.

[0033] In the present disclosure, the term "process" includes not only independent processes but also processes that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.

[0034] In the present disclosure, when referring to the amount of each component in a composition, if there are multiple substances belonging to each component in the composition, unless otherwise specified, it means the total amount of the multiple substances present in the composition.

[0035] In the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment.

[0036] In the present disclosure, the term "solid content" refers to components other than the solvent, and liquid components such as low molecular weight components other than the solvent are also included in the "solid content" in the present disclosure.

[0037] In the present disclosure, the term "solvent" is used in a meaning including water, an organic solvent, and a mixed solvent of water and an organic solvent.

[0038] In the present disclosure, the so-called "MD (machine direction)" refers to the longitudinal direction in the porous substrate and separator manufactured into a long strip, and the so-called "TD (transverse direction)" refers to the direction orthogonal to the MD in the surface direction of the porous substrate and the separator. In the present disclosure, "TD" is also referred to as the "width direction".

[0039] In the present disclosure, "heat-resistant resin" refers to a resin having a melting point of 200°C or higher, or a resin having no melting point but a decomposition temperature of 200°C or higher. In other words, the heat-resistant resin in the present disclosure refers to a resin that does not melt or decompose in a temperature range below 200°C.

[0040] In the present disclosure, the expression "(meth)acrylic-" means "acrylic-" or "methacrylic-".

[0041] In the present disclosure, the "monomer unit" of a copolymer or resin is a structural unit of the copolymer or resin, and refers to a structural unit formed by polymerization of a monomer.

[0042] In the present disclosure, “adhesion strength when bonding by dry hot pressing” is also referred to as “dry adhesion strength”, and “adhesion strength when bonding by wet hot pressing” is also referred to as “wet adhesion strength”.

[0043] In the present disclosure, the “function of bonding by dry hot pressing” is also referred to as “dry adhesiveness”, and the “function of bonding by wet hot pressing” is also referred to as “wet adhesiveness”.

[0044] [Separator for non-aqueous secondary batteries]

[0045] The non-aqueous secondary battery separator of the present disclosure (hereinafter also referred to as "separator") comprises: a heat-resistant porous layer, the heat-resistant porous layer containing an aromatic resin and inorganic particles; and an adhesive layer, the adhesive layer being arranged on the above-mentioned heat-resistant porous layer and containing adhesive resin particles containing a phenyl-containing acrylic resin, the above-mentioned adhesive resin particles containing a phenyl-containing acrylic resin are attached to the above-mentioned heat-resistant porous layer, and the above-mentioned inorganic particles contain barium sulfate particles.

[0046] The separator of the present disclosure has the above-mentioned structure, and thus has excellent adhesion to electrodes in both dry hot pressing and wet hot pressing, and gas generation is suppressed.

[0047] Although the reason why the separator of the present disclosure can exert such an effect is not clear, the inventors of the present application speculate as follows. However, the following speculation is not to be interpreted as limiting the separator of the present disclosure, but is explained as an example.

[0048] In the diaphragm of the present disclosure, an adhesive layer containing adhesive resin particles containing phenyl-containing acrylic resin is arranged on a heat-resistant porous layer containing aromatic resin and inorganic particles, and the adhesive resin particles containing phenyl-containing acrylic resin are attached to the heat-resistant porous layer. The acrylic resin contained in the adhesive resin particles attached to the heat-resistant porous layer has a high affinity with the aromatic rings and electrodes of the aromatic resin contained in the heat-resistant porous layer in a dry state, and the phenyl groups contained in the acrylic resin contained in the adhesive resin particles have a high affinity with the aromatic rings and electrodes of the aromatic resin contained in the heat-resistant porous layer in the presence of an electrolyte (so-called wet state). As a result of these, it is speculated that the diaphragm of the present disclosure has excellent adhesion to the electrode when using either dry hot pressing or wet hot pressing.

[0049] Furthermore, compared with magnesium hydroxide particles or aluminum oxide particles, barium sulfate particles are less likely to cause decomposition of electrolyte or electrolyte, and therefore, less likely to cause gas generation. Therefore, by using barium sulfate particles as the inorganic filler of the heat-resistant porous layer, a separator that is less likely to cause degradation of cycle characteristics and less likely to cause expansion and deformation of the battery can be obtained.

[0050] [Heat-resistant porous layer]

[0051] The heat-resistant porous layer in the present disclosure contains an aromatic resin and inorganic particles.

[0052] The heat-resistant porous layer is a film having a large number of fine pores and through which gas or liquid can pass from one surface to the other surface.

[0053] In the present disclosure, the term "aromatic resin" refers to a resin having an aromatic ring in the main chain or side chain. Examples of the aromatic ring include a benzene ring, a naphthalene ring, and an anthracene ring, and among these, a benzene ring is preferred.

[0054] From the viewpoint of excellent heat resistance, the aromatic resin preferably contains at least one selected from the group consisting of wholly aromatic polyamides, polyamideimides, and polyimides, and more preferably contains at least one selected from the group consisting of wholly aromatic polyamides, polyamideimides, and polyimides.

[0055] Among aromatic resins, fully aromatic polyamide is suitable for heat-resistant porous layer from the viewpoint of durability. The so-called fully aromatic polyamide refers to a polyamide whose main chain is composed only of benzene rings and amide bonds. However, a small amount of aliphatic monomers may also be copolymerized in fully aromatic polyamide. Fully aromatic polyamide is also called "aramid".

[0056] The wholly aromatic polyamide may be of meta type or para type.

[0057] Examples of the meta-type wholly aromatic polyamide include poly(meta-phenylene isophthalamide), and examples of the para-type wholly aromatic polyamide include copolymerized p-phenylene·3,4′-oxydiphenylene·terephthalamide and poly(p-phenylene terephthalamide).

[0058] As the wholly aromatic polyamide, a meta-type wholly aromatic polyamide is preferred from the viewpoint of easy formation of a heat-resistant porous layer and excellent redox resistance in an electrode reaction.

[0059] Specifically, the wholly aromatic polyamide is preferably poly(meta-phenylene isophthalamide) or copoly(paraphenylene·3,4′-oxydiphenylene·terephthalamide), and more preferably poly(meta-phenylene isophthalamide).

[0060] Among aromatic resins, polyamide-imide and polyimide are both suitable for the heat-resistant porous layer from the viewpoint of heat resistance.

[0061] The weight average molecular weight (Mw) of the aromatic resin contained in the heat-resistant porous layer is preferably 1×10 3 ~1×10 7 , more preferably 5×10 3 ~5×10 6 , more preferably 1×10 4 ~1×10 6 .

[0062] The weight average molecular weight (Mw) of the aromatic resin contained in the heat-resistant porous layer is a value measured by gel permeation chromatography (GPC). Specifically, the following method is used for measurement. In a solution obtained by dissolving lithium chloride in dimethylformamide (DMF) in a concentration of 0.01 mol / L (liter; the same below), a polymer is dissolved in a concentration of 1% by mass to prepare a sample solution. The prepared sample solution is used as a measurement sample, and GPC measurement is performed to calculate the molecular weight distribution. In the measurement, the chromatography data processing device "Shimadzu Chromatopak C-R4A" manufactured by Shimadzu Corporation and the GPC column "GPC·KD-802" manufactured by Showa Denko (KK) are used, and the measurement is performed at a detection wavelength of 280nm. As a reference, a polystyrene molecular weight standard substance is used. When measuring a sample including a porous substrate, DMF in which lithium chloride was dissolved at a concentration of 0.01 mol / L was added, and only the aromatic resin was heated and dissolved at 80° C. to prepare a measurement sample.

[0063] As the aromatic resin, a commercially available product can be used.

[0064] Examples of commercially available wholly aromatic polyamides include Conex (registered trademark; meta-type), Technora (registered trademark; para-type), and Twaron (registered trademark; para-type) manufactured by Teijin Co., Ltd. Examples of commercially available polyamide-imide include Torlon (registered trademark) 4000TF manufactured by Solvay Co., Ltd. Examples of commercially available polyimides include Q-VR-X1444 manufactured by PI Technology Research Institute Co., Ltd.

[0065] The heat-resistant porous layer may contain only one kind of aromatic resin, or may contain two or more kinds of aromatic resin.

[0066] The volume ratio of the aromatic resin in the heat resistant porous layer is preferably 15 to 85 volume %, more preferably 20 to 80 volume %, and further preferably 25 to 75 volume % based on the total volume of the heat resistant porous layer.

[0067] The volume ratio Vb (volume %) of the aromatic resin in the heat-resistant porous layer can be obtained by the following formula.

[0068] Vb={(Xb / Db) / (Xa / Da+Xb / Db+Xc / Dc+…+Xn / Dn)}×100

[0069] Here, among the constituent materials of the heat-resistant porous layer, the aromatic resin is b, and the other constituent materials are a, c, ..., n. The mass of each constituent material contained in a predetermined area of ​​the heat-resistant porous layer is Xa, Xb, Xc, ..., Xn (g), and the true density of each constituent material is Da, Db, Dc, ..., Dn (g / cm 3 ).

[0070] Xa etc. substituted into the above formula is the mass (g) of the constituent material used to form the heat resistant porous layer of a predetermined area, or the mass (g) of the constituent material taken out from the heat resistant porous layer of a predetermined area.

[0071] Da, etc. substituted into the above formula is the true density (g / cm 3 ), or the true density (g / cm 3 ).

[0072] The volume ratio of the aromatic resin in the heat-resistant porous layer is preferably 50 volume % or more, more preferably 70 volume % or more, and further preferably 90 volume % or more relative to the total volume of all resins contained in the heat-resistant porous layer. The above volume ratio can be set to 50 volume % to 100 volume %.

[0073] The heat-resistant porous layer may contain a heat-resistant resin other than the aromatic resin.

[0074] Examples of the heat-resistant resin other than the aromatic resin include polysulfone, polyethersulfone, polyketone, polyetherketone, polyetherimide, cellulose, and polyvinylidene fluoride resins.

[0075] When the heat-resistant porous layer contains a heat-resistant resin other than the aromatic resin, the heat-resistant resin other than the aromatic resin may be contained only one kind, or may be contained two or more kinds.

[0076] Regarding the volume ratio of the heat-resistant resin other than the aromatic resin in the heat-resistant porous layer, in order to maintain the effect of the aromatic resin, it is preferably 0 volume % to 50 volume % relative to the total volume of all resins contained in the heat-resistant porous layer, more preferably 0 volume % to 30 volume %, and further preferably 1 volume % to 10 volume %.

[0077] From the viewpoint of heat resistance, the heat-resistant porous layer contains inorganic particles. The inorganic particles include barium sulfate particles. The proportion of the barium sulfate particles in the total inorganic particles contained in the heat-resistant porous layer is preferably 50 volume % or more, more preferably 70 volume % or more, further preferably 90 volume % or more, and particularly preferably 99 volume % or more.

[0078] Furthermore, by making the inorganic particles contain barium sulfate within the above range, the possibility of damage when gas is generated in the battery can be suppressed, and in order to grasp the possibility of internal short circuit, it is easy to check the positional deviation of the electrode and the separator by a simple method based on X-ray irradiation.

[0079] The inorganic particles are contained in the heat-resistant porous layer in a state of being bound and covered with, for example, an aromatic resin.

[0080] When the heat-resistant porous layer contains other inorganic particles in addition to barium sulfate, the other inorganic particles preferably include at least one selected from the group consisting of metal hydroxides, metal oxides, metal nitrides, metal carbonates, and metal sulfates.

[0081] Examples of the metal hydroxide include aluminum hydroxide, magnesium hydroxide, calcium hydroxide, chromium hydroxide, zirconium hydroxide, cerium hydroxide, nickel hydroxide, boron hydroxide, etc., preferably magnesium hydroxide. Examples of the metal oxide include silicon dioxide, aluminum oxide, zirconium oxide, magnesium oxide, etc. Examples of the metal nitride include boron nitride, aluminum nitride, etc. Examples of the metal carbonate include calcium carbonate, magnesium carbonate, etc. Examples of the metal sulfate include calcium sulfate, etc.

[0082] The inorganic particles may be those surface-modified with a silane coupling agent or the like.

[0083] The particle shape of the inorganic particles is not particularly limited, for example, it can be any of spherical, elliptical, plate-like, needle-like, or amorphous. From the viewpoint of suppressing battery short circuit, the inorganic particles contained in the heat-resistant porous layer are preferably plate-like particles. In addition, the inorganic particles contained in the heat-resistant porous layer can be agglomerated particles or non-agglomerated primary particles. From the viewpoint of suppressing battery short circuit, non-agglomerated primary particles are preferably used.

[0084] The average primary particle size of the inorganic particles is preferably 0.01 μm or more and 1.0 μm or less. When the average primary particle size of the inorganic particles is 0.01 μm or more, the aggregation of the inorganic particles can be suppressed, and a heat-resistant porous layer with higher uniformity can be formed. From such a viewpoint, the average primary particle size of the inorganic particles is preferably 0.02 μm or more, more preferably 0.03 μm or more, and further preferably 0.05 μm or more. In addition, if the average primary particle size of the inorganic particles is 1.0 μm or less, the shrinkage of the heat-resistant porous layer when exposed to high temperature is further suppressed, and then, the smoothness of the surface of the adhesive layer side of the heat-resistant porous layer is improved, and as a result, the bonding strength is also improved. From such a viewpoint, the volume average particle size of the inorganic particles is preferably 0.9 μm or less, more preferably 0.8 μm or less, and further preferably 0.7 μm or less.

[0085] The heat-resistant porous layer may include two or more inorganic particles having different average primary particle sizes. The materials of the two or more inorganic particles having different average primary particle sizes may be the same or different. When the heat-resistant porous layer includes two or more inorganic particles having different average primary particle sizes, it is preferred that the average primary particle size of each is within the above range, and it is preferred that the average primary particle size of each is within the above range and the average primary particle size of the whole (i.e., mixed particles of inorganic particles having different average primary particle sizes) is within the above range.

[0086] The average primary particle size of the inorganic particles is a value measured by the following method.

[0087] The average primary particle size of the inorganic particles contained in the heat-resistant porous layer is obtained by measuring the major diameters of 100 inorganic particles randomly selected in the observation based on the scanning electron microscope (SEM), and averaging the major diameters of the 100 particles. The sample provided for SEM observation is an inorganic particle that is a material for forming the heat-resistant porous layer, or an inorganic particle taken out from the heat-resistant porous layer of the diaphragm. There is no limitation on the method of taking out the inorganic particles from the heat-resistant porous layer of the diaphragm. The method is, for example, a method of taking out the inorganic particles by immersing the heat-resistant porous layer peeled off from the diaphragm in an organic solvent that can dissolve the resin, dissolving the resin with the organic solvent, and taking out the inorganic particles; a method of heating the heat-resistant porous layer peeled off from the diaphragm to about 800°C to make the resin disappear, and taking out the inorganic particles; and the like.

[0088] The volume ratio of the inorganic particles in the heat-resistant porous layer is not particularly limited, for example, relative to the total volume of the heat-resistant porous layer, preferably 15 volume % to 85 volume %, more preferably 20 volume % to 80 volume %, and further preferably 25 volume % to 75 volume %. When the volume ratio of the inorganic particles in the heat-resistant porous layer is more than 15 volume % relative to the total volume of the heat-resistant porous layer, the heat resistance of the separator can be suitably improved. In addition, when the volume ratio of the inorganic particles in the heat-resistant porous layer is less than 85 volume % relative to the total volume of the heat-resistant porous layer, the heat-resistant porous layer is more difficult to peel off from the porous substrate.

[0089] The volume ratio Vb (volume %) of the inorganic particles in the heat-resistant porous layer can be obtained by the following formula.

[0090] Vb={(Xb / Db) / (Xa / Da+Xb / Db+Xc / Dc+…+Xn / Dn)}×100

[0091] Here, among the constituent materials of the heat-resistant porous layer, the inorganic particles are b, and the other constituent materials are a, c, ..., n. The mass of each constituent material contained in the heat-resistant porous layer of a predetermined area is Xa, Xb, Xc, ..., Xn (g), and the true density of each constituent material is Da, Db, Dc, ..., Dn (g / cm 3 ).

[0092] Xa etc. substituted into the above formula is the mass (g) of the constituent material used to form the heat resistant porous layer of a predetermined area, or the mass (g) of the constituent material taken out from the heat resistant porous layer of a predetermined area.

[0093] Da, etc. substituted into the above formula is the true density (g / cm 3 ), or the true density (g / cm 3 ).

[0094] The heat-resistant porous layer can include the components (so-called other components) other than the aromatic resin and inorganic particles described above as needed. As other components, various additives can be mentioned. As additives, dispersants such as surfactants, wetting agents, defoamers, pH adjusting agents, etc. can be mentioned. Dispersants can be added to the coating liquid for forming the heat-resistant porous layer for the purpose of improving dispersibility, coating properties or storage stability. Wetting agents, defoamers, and pH adjusting agents can be added to the coating liquid for the purpose of making the affinity with the porous substrate good, suppressing the mixing of air into the coating liquid, and adjusting the pH.

[0095] [Characteristics of heat-resistant porous layer]

[0096] <<Thickness>>

[0097] From the viewpoint of heat resistance or operability of the separator, the thickness of the heat-resistant porous layer is preferably 0.5 μm or more on each side, and more preferably 1.0 μm or more on each side. In addition, from the viewpoint of operability of the separator or energy density of the battery, the thickness of the heat-resistant porous layer is preferably 5.0 μm or less on each side, and more preferably 4.0 μm or less on each side.

[0098] When the heat-resistant porous layer is provided on both sides of the porous substrate, the total thickness of the heat-resistant porous layer on both sides is preferably 1.0 μm or more, more preferably 2.0 μm or more, and further preferably 3.0 μm or more. In addition, the total thickness of the heat-resistant porous layer on both sides is preferably 10.0 μm or less, more preferably 8.0 μm or less, and further preferably 7.0 μm or less.

[0099] The thickness (μm) of the heat-resistant porous layer is a value measured using a contact thickness meter [LITEMATIC VL-50, manufactured by Mitutoyo]. A cylindrical terminal with a diameter of 5 mm was used as a measuring terminal, and during the measurement, the load was adjusted to apply 0.01 N. The thickness was measured at any 20 points within 10 cm×10 cm, and the average value was calculated.

[0100] When the heat resistant porous layer is provided on both surfaces of the porous substrate, the difference in thickness between the heat resistant porous layer on one surface and the heat resistant porous layer on the other surface is preferably small, for example, preferably 20% or less of the total thickness of both surfaces.

[0101] <<Mass per unit area>>

[0102] The total weight per unit area of ​​the heat-resistant porous layer on both sides is preferably 1.0 g / m 2 ~10.0g / m 2 From the viewpoint of heat resistance and handling properties of the separator, the total mass per unit area of ​​the heat-resistant porous layer on both sides is preferably 1.0 g / m 2 More preferably 2.0 g / m 2 More preferably, 3.0 g / m 2 In addition, from the viewpoint of the operability of the separator and the energy density of the battery, the mass per unit area of ​​the heat-resistant porous layer is preferably 10.0 g / m 2 Below, more preferably 8.0g / m 2 Below, more preferably 7.0 g / m 2 the following.

[0103] When a heat-resistant porous layer is provided on both sides of a porous substrate, from the viewpoint of suppressing curling of the diaphragm, the difference between the mass per unit area of ​​the heat-resistant porous layer on one side and the mass per unit area of ​​the heat-resistant porous layer on the other side is preferably less than 20 mass % relative to the total of the two sides.

[0104] The mass per unit area of ​​the heat-resistant porous layer (g / m 2 ) from the unit area weight after layer formation (g / m 2 ) minus the unit area weight before layer formation (g / m 2 ) and find the answer.

[0105] <<Porosity>>

[0106] The porosity of the heat-resistant porous layer is preferably 30% to 80%. From the viewpoint of ion permeability of the separator, the porosity of the heat-resistant porous layer is preferably 30% or more, more preferably 35% or more, and further preferably 40% or more. In addition, from the viewpoint of mechanical strength of the heat-resistant porous layer, the porosity of the heat-resistant porous layer is preferably 80% or less, more preferably 70% or less, and further preferably 60% or less.

[0107] The porosity ε (%) of the heat-resistant porous layer is determined by the following formula.

[0108] ε={1-(Wa / da+Wb / db+Wc / dc+…+Wn / dn) / t}×100

[0109] Wherein, the constituent materials of the heat-resistant porous layer are a, b, c, ..., n, and the mass of each constituent material is Wa, Wb, Wc, ..., Wn (g / cm 2 ), the true density of each constituent material is da, db, dc, ..., dn (g / cm 3 ), the thickness of the heat-resistant porous layer is t (μm).

[0110] 〔Adhesive layer〕

[0111] The adhesive layer in the present disclosure is a layer disposed on the surface of the heat-resistant porous layer and exists as the outermost layer of the separator. The adhesive layer in the present disclosure is a layer containing adhesive resin particles (i.e., specific adhesive resin particles) containing a phenyl-containing acrylic resin, and the specific adhesive resin particles are attached to the heat-resistant porous layer.

[0112] In the separator of the present disclosure, the adhesive layer may have a structure in which a large number of specific adhesive resin particles are arranged adjacent to each other on the surface of the heat-resistant porous layer to form a layer, or may have a structure in which a large number of specific adhesive resin particles are scattered on the surface of the heat-resistant porous layer. In addition, when the adhesive layer has a structure in which a large number of specific adhesive resin particles are arranged adjacent to each other on the surface of the heat-resistant porous layer to form a layer, it may have a single-layer structure in which the specific adhesive resin particles do not overlap in the thickness direction, or it may have a multilayer structure in which a plurality of specific adhesive resin particles overlap in the thickness direction to have more than 2 layers. From the viewpoint of better adhesion to the electrode, the adhesive layer in the present disclosure preferably has a structure in which a large number of specific adhesive resin particles are arranged adjacent to each other on the surface of the heat-resistant porous layer, and from the viewpoint of improving the energy density of the battery and ensuring ion permeability, it is preferably a single-layer structure in which the specific adhesive resin particles do not overlap in the thickness direction.

[0113] The adhesive layer in the present disclosure utilizes the gaps between specific adhesive resin particles to allow gas or liquid to pass from one surface to the other surface.

[0114] The so-called structure in which specific adhesive resin particles are attached to the heat-resistant porous layer includes, in addition to a method in which the resin maintains the particle shape in the completed diaphragm, a method in which a part of the resin particles is melted by heat treatment or drying treatment and the particle shape is not maintained in the diaphragm completed using the resin particles as the material of the adhesive layer.

[0115] Since the adhesive layer in the present disclosure is a structure in which specific adhesive resin particles are attached to the heat-resistant porous layer, the interface failure between the heat-resistant porous layer and the adhesive layer is not likely to occur. In addition, when the adhesive layer in the present disclosure is a structure in which specific adhesive resin particles are attached and connected to each other, the toughness of the adhesive layer is excellent and the cohesive failure of the adhesive layer is not likely to occur.

[0116] With respect to the diaphragm of the present disclosure, the adhesive layer is a layer containing adhesive resin particles (specific adhesive resin particles) comprising a phenyl-containing acrylic resin, and is a layer in which the specific adhesive resin particles are attached to a heat-resistant porous layer containing an aromatic resin. Therefore, in an environment in which an electrolyte is present, the specific adhesive resin particles are continuously bonded to the heat-resistant porous layer by utilizing the interaction caused by the high affinity between the phenyl groups from the phenyl-containing acrylic resin contained in the adhesive layer and the aromatic rings from the aromatic resin contained in the heat-resistant porous layer. As a result, not only the dry adhesion to the electrode but also the wet adhesion to the electrode is excellent.

[0117] The specific adhesive resin particles are a particle-shaped resin containing a phenyl group-containing acrylic resin and having adhesiveness to the electrode of the battery. The specific adhesive resin particles are preferably resin particles that are stable in an electrolyte solution and electrochemically stable.

[0118] The adhesive resin particles (specific adhesive resin particles) containing a phenyl group-containing acrylic resin are preferably at least one selected from the group consisting of (i) resin particles that are a copolymer containing an acrylic monomer unit and a styrene monomer unit, and (ii) resin particles that are a mixture of an acrylic resin and a styrene resin.

[0119] Hereinafter, (i) resin particles that are a copolymer containing an acrylic monomer unit and a styrene monomer unit are also referred to as “resin particles A”, and (ii) resin particles that are a mixture containing an acrylic resin and a styrene resin are also referred to as “resin particles B”.

[0120] The resin particles A are particles of a copolymer containing an acrylic monomer unit and a styrene monomer unit. The acrylic monomer unit can contribute to dry adhesion, and the styrene monomer unit can contribute to wet adhesion. The copolymer may contain monomer units other than the acrylic monomer unit and the styrene monomer unit as monomer units.

[0121] As the acrylic monomer, at least one selected from the group consisting of (meth)acrylic acid, (meth)acrylate salts, and (meth)acrylate esters is preferred.

[0122] Examples of (meth)acrylates include sodium (meth)acrylate, potassium (meth)acrylate, magnesium (meth)acrylate, and zinc (meth)acrylate. Examples of (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate.

[0123] The copolymer may contain only one type of acrylic monomer unit as a monomer unit, or may contain two or more types.

[0124] The styrene-based monomer is a monomer having a phenyl group.

[0125] Examples of the styrene monomer include styrene, m-chlorostyrene, p-chlorostyrene, p-fluorostyrene, p-methoxystyrene, m-tert-butoxystyrene, p-tert-butoxystyrene, p-vinylbenzoic acid, p-methyl-α-methylstyrene, styrenesulfonic acid and salts thereof (e.g., sodium styreneate), etc. Among them, styrene is preferred as the styrene monomer.

[0126] The copolymer may contain only one type of styrene-based monomer unit as a monomer unit, or may contain two or more types.

[0127] The content of the styrene-based monomer units contained in the copolymer is preferably 10% to 99% by mass, more preferably 15% to 95% by mass, and still more preferably 20% to 90% by mass, relative to the total content of the styrene-based monomer units and the acrylic acid-based monomer units, from the viewpoint of achieving both dry adhesion and wet adhesion.

[0128] The copolymer preferably contains an acid group-containing monomer unit as a monomer unit from the viewpoint of dispersion stability during preparation of the copolymer.

[0129] As the monomer containing an acid group, there can be mentioned monomers having a carboxyl group such as (meth) acrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, etc.; monomers having a sulfonic acid group such as vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth) allyl sulfonic acid, (meth) acrylic acid-2-sulfonic acid ethyl ester, 2-acrylamide-2-methylpropanesulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, etc.; monomers having a phosphate group such as 2-(meth) acryloyloxyethyl phosphate, methyl-2-(meth) acryloyloxyethyl phosphate, ethyl-(meth) acryloyloxyethyl phosphate, etc.; monomers having a hydroxyl group such as 2-hydroxyethyl (meth) acrylate, 2-hydroxypropyl (meth) acrylate, 4-hydroxybutyl (meth) acrylate, etc. Among them, as the monomer containing an acid group, a monomer having a carboxyl group is preferred.

[0130] The copolymer may contain only one type of acid group-containing monomer unit as a monomer unit, or may contain two or more types.

[0131] The content of the acid group-containing monomer unit in the copolymer is preferably 0.1 to 20% by mass, more preferably 1 to 10% by mass, and further preferably 3 to 7% by mass, based on all structural units.

[0132] In the copolymer, from the viewpoint of adjusting the swelling degree in the electrolyte solution, it is preferred to contain a crosslinking monomer unit as a monomer unit. The crosslinking monomer unit is a monomer that can form a crosslinked structure during or after polymerization by heating or irradiation with energy rays.

[0133] As a crosslinking monomer, for example, a monomer having two or more polymerizable reactive groups (so-called multifunctional monomers) can be cited. As such a multifunctional monomer, divinyl compounds such as divinylbenzene can be cited; di(meth)acrylate compounds such as diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, 1,3-butanediol diacrylate; tri(meth)acrylate compounds such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate; ethylenically unsaturated monomers containing epoxy groups such as allyl glycidyl ether and glycidyl methacrylate; and the like. Among them, as a crosslinking monomer, from the viewpoint of easy control of swelling degree, it is preferably at least one selected from the group consisting of dimethacrylate compounds and ethylenically unsaturated monomers containing epoxy groups, and more preferably at least one selected from dimethacrylate compounds.

[0134] The copolymer may contain only one type of crosslinkable monomer unit as a monomer unit, or may contain two or more types.

[0135] If the ratio of the crosslinkable monomer unit in the copolymer increases, the degree of swelling of the copolymer in the electrolyte tends to decrease. Therefore, the ratio of the crosslinkable monomer unit in the copolymer is preferably determined in consideration of the type and amount of the monomers used.

[0136] The content of the crosslinkable monomer unit in the copolymer is preferably 0.1 to 5% by mass, more preferably 0.2 to 4% by mass, and even more preferably 0.5 to 3% by mass, based on all the structural units.

[0137] The resin particles B are particles containing a mixture of an acrylic resin and a styrene resin. The acrylic resin can contribute to dry adhesiveness, and the styrene resin can contribute to wet adhesiveness. The mixture may contain resins other than the acrylic resin and the styrene resin.

[0138] The resin particles B may be, for example, resin particles in which a part or the whole of the surface of an acrylic resin particle is coated with a styrene resin, resin particles in which a part or the whole of the surface of a styrene resin particle is coated with an acrylic resin, or resin particles in which an acrylic resin and a styrene resin are mixed in one particle. From the viewpoint of anti-blocking properties, the resin particles B are preferably resin particles in which a part or the whole of the surface of an acrylic resin particle is coated with a styrene resin.

[0139] In the present disclosure, the “acrylic resin” refers to a resin containing an acrylic monomer unit, and includes both a polymer obtained by polymerizing an acrylic monomer alone and a copolymer obtained by polymerizing an acrylic monomer and other monomers.

[0140] Examples of acrylic resins include poly(meth)acrylic acid, poly(meth)acrylate salts, poly(meth)acrylate esters, cross-linked poly(meth)acrylic acid, cross-linked poly(meth)acrylate salts, cross-linked poly(meth)acrylate esters, etc. The acrylic resin may be a modified acrylic resin. The mixture may contain only one acrylic resin or two or more.

[0141] The acrylic resin preferably contains a structural unit (acrylic monomer unit) derived from at least one acrylic monomer selected from the group consisting of (meth)acrylic acid, (meth)acrylic acid salts, and (meth)acrylic acid esters. Specific examples of (meth)acrylic acid salts and (meth)acrylic acid esters are as described above.

[0142] The content of the acrylic monomer units in the acrylic resin is preferably 50% by mass to 100% by mass based on all the monomer units.

[0143] In the present disclosure, the “styrene-based resin” refers to a resin containing a styrene-based monomer unit, and includes both a polymer obtained by polymerizing a styrene-based monomer alone and a copolymer obtained by polymerizing a styrene-based monomer and other monomers.

[0144] Specific examples of the styrene-based monomers are as described above.

[0145] The content of the styrene-based monomer units in the styrene-based resin is preferably 50% by mass to 100% by mass based on all monomer units.

[0146] The content of the styrene resin contained in the mixture is preferably 10% to 99% by mass, more preferably 20% to 95% by mass, and even more preferably 30% to 90% by mass, relative to the total content of the styrene resin and the acrylic resin, from the viewpoint of achieving both dry adhesion and wet adhesion.

[0147] The acrylic resin and / or styrene resin contained in the mixture preferably contains an acid group-containing monomer unit and / or a crosslinking monomer unit. The acid group-containing monomer unit and the crosslinking monomer unit are as described above.

[0148] The glass transition temperature of the specific adhesive resin particles is preferably 10°C to 150°C. If the glass transition temperature of the specific adhesive resin particles is 10°C to 150°C, the adhesion of the adhesive layer can be suppressed, and the adhesion (dry adhesion and wet adhesion) of the adhesive layer to the electrode can be improved. The glass transition temperature of the specific adhesive resin particles is more preferably 20°C or more, and more preferably 30°C or more. In addition, from the same point of view, the glass transition temperature is more preferably 130°C or less, and more preferably 110°C or less.

[0149] The glass transition temperature of the specific adhesive resin particles can be controlled by adjusting the copolymerization ratio of acrylic monomers, styrene monomers, etc. in the copolymer or resin according to the FOX equation.

[0150] The glass transition temperature of the specific adhesive resin particles is obtained from the differential scanning calorimetry (DSC) curve obtained by differential scanning calorimetry (DSC). As a measuring device, a differential scanning calorimeter [Q20 Differential Scanning Calorimeter, manufactured by TA Instruments] is used, and 10 mg of resin particles are used as a sample. The temperature at the point where the straight line extending the baseline on the low temperature side to the high temperature side intersects with the tangent with the largest slope among the tangents of the curve of the step-shaped change portion is taken as the glass transition temperature of the resin particles.

[0151] From the viewpoint of forming a good porous structure, the volume average particle size of the specific adhesive resin particles is preferably 0.01 μm or more, more preferably 0.05 μm or more, further preferably 0.1 μm or more, and particularly preferably 0.2 μm or more. In addition, from the viewpoint of suppressing the thickness of the adhesive layer, the volume average particle size of the specific adhesive resin particles is preferably 1.2 μm or less, more preferably 1.0 μm or less, further preferably 0.8 μm or less, and particularly preferably 0.7 μm or less.

[0152] The volume average particle size of the specific adhesive resin particles is determined by the following method.

[0153] The specific adhesive resin particles are dispersed in water containing a nonionic surfactant, and the particle size distribution is measured using a laser diffraction particle size distribution measuring device. In the volume-based particle size distribution, the particle size (D50) at which the accumulation from the small diameter side is 50% is taken as the volume average particle size (μm) of the specific adhesive resin particles.

[0154] As the nonionic surfactant, for example, Triton (registered trademark) X-100 [Compound name: polyethylene glycol tert-octylphenyl ether, manufactured by Dow Chemical Co.] can be preferably used. In addition, as the laser diffraction particle size distribution measuring apparatus, for example, Mastersizer 2000 manufactured by Sysmex Co., Ltd. can be preferably used.

[0155] The amount of the specific adhesive resin particles attached to the heat-resistant porous layer is preferably 0.1 g / m 2 ~5.0g / m 2 If the amount of the specific adhesive resin particles attached to the heat-resistant porous layer is 0.1 g / m 2 From this point of view, the amount of the specific adhesive resin particles attached to the heat-resistant porous layer is preferably 0.1 g / m 2More preferably 0.2 g / m 2 More preferably, 0.3 g / m 2 Above, particularly preferably 0.4 g / m 2 In addition, if the amount of the specific adhesive resin particles attached to the heat-resistant porous layer is 5.0 g / m 2 The specific adhesive resin particles are preferably 5.0 g / m2 in weight and 5.0 g / m2 in weight. 2 Below, more preferably 4.0g / m 2 Below, more preferably 3.0 g / m 2 Below, particularly preferably 1.0 g / m 2 When the heat-resistant porous layer is provided on both surfaces of the porous substrate, the total amount of the specific adhesive resin particles attached to both surfaces of the heat-resistant porous layer may be within the above range.

[0156] The adhesion amount (g / m 2 ) is the weight per unit area after layer formation (g / m 2 ) minus the unit area weight before layer formation (g / m 2 ) and find the answer.

[0157] From the viewpoint of sufficiently ensuring the ion permeability in the adhesive layer, the swelling degree of the specific adhesive resin particles in the electrolyte is preferably 450% or less, more preferably 430% or less, and further preferably 410% or less. The lower limit of the swelling degree of the specific adhesive resin particles in the electrolyte may be, for example, 110% or more.

[0158] The degree of swelling of the specific adhesive resin particles in the electrolyte solution is determined by the following method.

[0159] The aqueous dispersion of specific adhesive resin particles was poured onto a glass plate with a metal frame having an inner size of 50 mm × 70 mm, and dried at 150°C for 1 hour to prepare a sheet-shaped sample for measurement. About 1 g of the prepared sample for measurement was cut out, and its weight W1 (g) was accurately measured using an electronic balance, and then immersed in an electrolyte solution [1 mol / L Li BF4 ethylene carbonate: ethyl methyl carbonate (volume ratio 3:7)] at 60°C for 24 hours. The immersed sample for measurement was taken out of the electrolyte solution, and after wiping off the electrolyte solution attached to the surface, its weight W2 (g) was measured using an electronic balance, and the swelling degree (%) of the resin particles was calculated using the following formula.

[0160] Swelling degree (%) = (W2 / W1) × 100

[0161] The adhesive layer may contain resin particles other than the specific adhesive resin particles.

[0162] As resin particles other than specific adhesive resin particles, for example, homopolymers or copolymers, carboxymethyl cellulose, hydroxyalkyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, polyethers (polyethylene oxide, polypropylene oxide, etc.) or particles of a mixture of more than two of them can be cited. Among them, as resin particles other than specific adhesive resin particles, particles of polyvinylidene fluoride resin are preferably used. If the adhesive layer also includes particles of polyvinylidene fluoride resin in addition to specific adhesive resin particles, the bonding strength (wet bonding strength) between the adhesive layer and the heat-resistant porous layer can be improved. In addition, if the adhesive layer also includes particles of polyvinylidene fluoride resin in addition to specific adhesive resin particles, the swelling of the adhesive layer caused by the electrolyte can be suppressed. As a result, the adhesion (wet adhesion) of the separator and the electrode is improved, and its adhesion is well maintained.

[0163] As polyvinylidene fluoride resin, homopolymers of vinylidene fluoride (i.e., polyvinylidene fluoride), copolymers of vinylidene fluoride and other monomers (polyvinylidene fluoride copolymers), mixtures of polyvinylidene fluoride and polyvinylidene fluoride copolymers, etc. can be cited. As monomers copolymerizable with vinylidene fluoride, for example, tetrafluoroethylene, hexafluoropropylene, trifluoroethylene, chlorotrifluoroethylene, trichloroethylene, vinyl fluoride, trifluoroperfluoropropyl ether, ethylene, vinyl acetate, vinyl chloride, acrylonitrile, etc. can be cited. Copolymers can include only one structural unit (monomer unit) from these monomers, or can include two or more.

[0164] From the viewpoint of obtaining mechanical strength that can withstand pressure and heat during battery production, the polyvinylidene fluoride copolymer preferably contains 50 mol % or more of structural units derived from vinylidene fluoride (so-called vinylidene fluoride units).

[0165] The polyvinylidene fluoride copolymer is preferably a copolymer of vinylidene fluoride and tetrafluoroethylene, a copolymer of vinylidene fluoride and hexafluoropropylene, or a copolymer of vinylidene fluoride and trifluoroethylene, and more preferably a copolymer of vinylidene fluoride and hexafluoropropylene. The copolymer of vinylidene fluoride and hexafluoropropylene is preferably a copolymer containing 0.1 mol% to 10 mol% (preferably 0.5 mol% to 5 mol%) of a structural unit derived from hexafluoropropylene (so-called hexafluoropropylene unit).

[0166] The weight average molecular weight (Mw) of the polyvinylidene fluoride-based resin is preferably 1,000 to 5,000,000, more preferably 10,000 to 3,000,000, and even more preferably 50,000 to 2,000,000.

[0167] The weight average molecular weight (Mw) of the polyvinylidene fluoride resin is a value measured by gel permeation chromatography (GPC). Specifically, as a measuring device, a GPC device "GPC-900" manufactured by JASCO Corporation is used, as a column, two "TSKgel SUPER AWM-H" manufactured by Tosoh Corporation are used, and as an eluent, N,N-dimethylformamide is used, and the measurement is performed under the conditions of a column temperature of 40°C and a flow rate of 0.6 mL / min to obtain a molecular weight converted to polystyrene.

[0168] The melting point of the particles of the polyvinylidene fluoride resin is preferably 110°C to 180°C. If the melting point of the particles of the polyvinylidene fluoride resin is 110°C to 180°C, both adhesion and blocking resistance can be achieved. From this point of view, the melting point of the particles of the polyvinylidene fluoride resin is more preferably 120°C or more, and more preferably 130°C or more. In addition, from the same point of view, the melting point of the particles of the polyvinylidene fluoride resin is more preferably 170°C or less, and more preferably 160°C or less.

[0169] The melting point of the polyvinylidene fluoride resin particles can be determined from a differential scanning calorimetry curve (DSC curve) obtained by differential scanning calorimetry (DSC: Differential Scanning Calorimetry).

[0170] As a measuring device, a differential scanning calorimeter is used, and 10 mg of the resin particles are used as a sample. Under a nitrogen atmosphere, the sample is heated from 30°C to 200°C at a heating rate of 5°C / min, then cooled from 200°C to 30°C at a cooling rate of 2°C / min, and further heated from 30°C to 200°C at a heating rate of 2°C / min, and the peak top of the endothermic peak obtained at this time is used as the melting point of the resin particles. As a differential scanning calorimeter, for example, Q20 Differential Scanning Calorimeter manufactured by TA Instruments can be preferably used.

[0171] When the adhesive layer contains polyvinylidene fluoride resin particles, the mass ratio of the polyvinylidene fluoride resin particles is preferably 5 to 95 mass %, more preferably 15 to 85 mass %, based on the total mass of the adhesive layer.

[0172] The adhesive layer may contain components other than the resin particles described above (so-called other components) within the range that does not hinder the effect of the present disclosure, and the proportion of other components in the adhesive layer is preferably 10% by mass or less of the total mass of the adhesive layer, and more preferably 5% by mass or less. A more preferred embodiment is a embodiment in which the adhesive layer does not substantially contain other components.

[0173] Examples of other components include additives added to the adhesive resin particle dispersion for forming the adhesive layer. Examples of such additives include dispersants such as surfactants, wetting agents, defoaming agents, and pH adjusters.

[0174] In the adhesive resin particle dispersion used to form the adhesive layer, a dispersant may be added for the purpose of improving dispersibility, coating properties or storage stability, a wetting agent may be added for the purpose of improving affinity with the heat-resistant porous layer, a defoaming agent may be added for the purpose of suppressing the mixing of air into the adhesive resin particle dispersion, and a pH adjuster may be added for the purpose of adjusting the pH.

[0175] Surfactants are described in paragraphs

[0142] and

[0143] of International Publication No. 2019 / 130994. These descriptions are incorporated into this specification by reference.

[0176] In one embodiment, the adhesive layer preferably has a phenyl group peak area S1 of 0.01 to 3 and a carbonyl group peak area S2 of 4 or less as measured by Fourier transform infrared spectroscopy (FT-IR).

[0177] If the peak area S1 of the phenyl group is 0.01 or more and the peak area S2 of the carbonyl group is 4 or less, the adhesive layer can present a more sufficient wet adhesive strength for the heat-resistant porous layer and the electrode. If the peak area S1 of the phenyl group is 3.0 or less, the swelling of the adhesive layer caused by the electrolyte can be further suppressed. From such a viewpoint, the peak area S1 of the phenyl group is preferably 0.01 or more, more preferably 0.02 or more, and more preferably 0.05 or more. The peak area S1 of the phenyl group is preferably 3.0 or less, more preferably 2.5 or less, more preferably 2.0 or less, and particularly preferably 0.5 or less. The peak area S2 of the carbonyl group is preferably 4 or less, more preferably 3.0 or less, and more preferably 2.0 or less. The peak area S2 of the carbonyl group can be, for example, 0.01 or more, more preferably 0.05 or more, and more preferably 0.10 or more.

[0178] As for the adhesive layer, in another embodiment, it is preferred that the peak area S1 of the phenyl group obtained by Fourier transform infrared spectroscopy (FT-IR) is 0.01 to 3, the peak area S2 of the carbonyl group obtained by FT-IR is 4 or less, and the peak area S3 of the CF bond obtained by FT-IR is 0.1 to 8.

[0179] When the peak area S3 of the CF bond obtained by FT-IR is 0.1 to 8, the adhesive layer shows a more sufficient wet adhesive strength for the electrode, which can suppress swelling of the electrolyte. From such a viewpoint, the peak area S3 of the CF bond obtained by FT-IR is preferably 0.1 or more, more preferably 0.3 or more, and further preferably 0.5 or more. In addition, the peak area S3 of the CF bond obtained by FT-IR is preferably 8.0 or less, more preferably 6.0 or less, further preferably 4.0 or less, and particularly preferably 2 or less.

[0180] The peak area S1 of the phenyl group of the adhesive layer obtained by Fourier transform infrared spectroscopy (FT-IR) was determined by the following method. After obtaining the absorption spectrum of the adhesive layer by Fourier transform infrared spectroscopy (FT-IR) under the following conditions, the absorption peak of the phenyl group (694 cm -1 ~710cm -1 ) to perform baseline correction, and find the area of ​​the range surrounded by the baseline and the absorption spectrum line (unit: dimensionless). The values ​​obtained from the absorption spectra of 8 randomly selected different ranges are averaged to obtain the peak area S1 of the phenyl group in the adhesive layer.

[0181] The peak area S2 of the carbonyl group of the adhesive layer obtained by Fourier transform infrared spectroscopy (FT-IR) was determined by the following method. After obtaining the absorption spectrum of the adhesive layer by Fourier transform infrared spectroscopy (FT-IR) under the following conditions, the absorption peak of the carbonyl group (1707 cm -1 ~1753cm -1 ) to perform baseline correction, and find the area of ​​the range surrounded by the baseline and the absorption spectrum line (unit: dimensionless). The values ​​obtained from the absorption spectra of 8 randomly selected different ranges are averaged to obtain the peak area S2 of the carbonyl group of the adhesive layer.

[0182] In addition, the peak area S3 of the CF bond obtained by Fourier transform infrared spectroscopy (FT-IR) was determined by the following method. After obtaining the absorption spectrum of the adhesive layer by Fourier transform infrared spectroscopy (FT-IR) under the following conditions, the absorption peak of the CF bond (862 cm -1 ~901cm -1 ) to perform baseline correction, and find the area of ​​the range surrounded by the baseline and the absorption spectrum line (unit: dimensionless). The values ​​obtained from the absorption spectra of 8 randomly selected different ranges are averaged to obtain the peak area S3 of the CF bond of the adhesive layer.

[0183] Each area is calculated using the function of the measuring device.

[0184] At 1707cm -1 ~1753cm -1The carbonyl absorption peak observed in the range of 862 cm-1 is believed to be derived from the carbonyl group of the (meth) acrylic acid compound in the adhesive layer. -1 ~901cm -1 The absorption peak of the CF bond observed in the range of 500 Å is considered to be derived from the CF bond of the vinylidene fluoride in the adhesive layer.

[0185] -condition-

[0186] Measuring device: Fourier transform infrared spectrophotometer [IRAffinity-1, manufactured by Shimadzu Corporation]

[0187] Measurement wavelength range: 400cm -1 ~4000cm -1

[0188] Measurement mode: transmittance

[0189] Apodization function: Happ-Genzel

[0190] Resolution: 4cm -1

[0191] Cumulative times: 10 times

[0192] Number of samples measured: n = 8

[0193] 〔Porous substrate〕

[0194] The separator of the present disclosure preferably further includes a porous substrate.

[0195] When the separator of the present disclosure further includes a porous substrate, the heat-resistant porous layer described above is preferably provided on one or both surfaces of the porous substrate.

[0196] If the heat-resistant porous layer is present on both sides of the porous substrate, the heat resistance of the separator is more excellent, and the safety of the battery can be further improved. In addition, curling is not easy to occur in the separator, and the operability during the manufacture of the battery is excellent. If the heat-resistant porous layer is only present on one side of the porous substrate, the ion permeability of the separator is more excellent. In addition, the thickness of the separator as a whole can be suppressed, and a battery with higher energy density can be manufactured.

[0197] In the present disclosure, the term "porous substrate" refers to a substrate having pores or voids inside. Examples of such substrates include microporous membranes, porous sheets formed of fibrous materials (e.g., nonwoven fabrics, paper, etc.), and the like.

[0198] As the porous substrate in the present disclosure, a microporous membrane is preferably used from the viewpoint of thin film and strength of the separator. In the present disclosure, the so-called "microporous membrane" refers to a membrane having a structure with a large number of micropores inside and these micropores connected, and gas or liquid can pass from one side to the other side.

[0199] The material of the porous base material is preferably an electrically insulating material, and may be an organic material or an inorganic material.

[0200] In order to impart shutdown function to the porous substrate, it is desirable that the porous substrate contains a thermoplastic resin. The so-called "shutdown function" refers to the following function: when the battery temperature rises, the constituent material melts and blocks the pores of the porous substrate, thereby blocking the movement of ions and preventing thermal runaway of the battery. As the thermoplastic resin, a thermoplastic resin with a melting point below 200°C is preferred.

[0201] Examples of the thermoplastic resin include polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; and the like.

[0202] Among them, polyolefin is preferred as the thermoplastic resin.

[0203] The porous substrate is preferably a microporous film made of polyolefin (also referred to as "polyolefin microporous film"). Examples of the polyolefin microporous film include polyolefin microporous films suitable for existing battery separators, and it is desirable to select a polyolefin microporous film having sufficient mechanical properties and ion permeability.

[0204] From the viewpoint of exhibiting the shutdown function, the polyolefin microporous membrane is preferably a microporous membrane containing polyethylene (also referred to as a "polyethylene microporous membrane"). When the polyolefin microporous membrane contains polyethylene, the polyethylene content is preferably 95% by mass or more relative to the total mass of the polyolefin microporous membrane.

[0205] The polyolefin microporous membrane is preferably a microporous membrane made of polypropylene from the viewpoint of having heat resistance such that the membrane is less likely to be damaged when exposed to high temperatures.

[0206] From the viewpoint of having a shutdown function and heat resistance that is not easily damaged when exposed to high temperature, the polyolefin microporous membrane is preferably a microporous membrane containing polyethylene and polypropylene. As such a polyolefin microporous membrane, for example, there can be mentioned: a microporous membrane in which polyethylene and polypropylene are mixed in one layer; and a microporous membrane in which at least one layer contains polyethylene and at least one layer contains polypropylene, which has a laminated structure of more than two layers.

[0207] When the polyolefin microporous membrane is a microporous membrane containing polyethylene and polypropylene, from the viewpoint of having both the shutdown function and the above-mentioned heat resistance in a well-balanced manner, the content of polyethylene and the content of polypropylene are preferably 95% by mass or more and 5% by mass or less, respectively, relative to the total mass of the polyolefin microporous membrane.

[0208] The weight average molecular weight (Mw) of the polyolefin contained in the polyolefin microporous membrane is preferably 100,000 to 5,000,000.

[0209] If the Mw of the polyolefin contained in the polyolefin microporous membrane is 100,000 or more, sufficient mechanical properties can be imparted to the microporous membrane. On the other hand, if the Mw of the polyolefin contained in the polyolefin microporous membrane is 5,000,000 or less, the shutdown properties of the microporous membrane become better and it is easier to form a microporous membrane.

[0210] The weight average molecular weight (Mw) of the polyolefin contained in the polyolefin microporous membrane is a value measured by gel permeation chromatography (GPC). Specifically, it can be obtained by the following method: the polyolefin microporous membrane is heated and dissolved in o-dichlorobenzene to prepare a sample solution, and as a measuring device, a GPC device "HLC-8321GPC / HT type" manufactured by Tosoh (Strain) is used, as a column, "TSKgel GMH6-HT" and "TSKgel GMH6-HTL" manufactured by Tosoh (Strain) are used, and as an eluent, o-dichlorobenzene (containing 0.025% by mass of 2,6-di-tert-butyl-4-methylphenol) is used, and the column temperature is 140°C and the flow rate is 1.0 mL / min. The conditions for measurement. In the calibration of molecular weight, monodisperse polystyrene [Tosoh (Strain)] is used.

[0211] As a method for manufacturing a polyolefin microporous membrane, the following methods can be cited: a method of extruding a molten polyolefin from a T-die to form a sheet, subjecting the sheet to a crystallization treatment, then stretching it, and then heat treating it to form a microporous membrane; a method of extruding a molten polyolefin together with a plasticizer such as liquid paraffin from a T-die, cooling it to form a sheet, stretching it, extracting the plasticizer, and then heat treating it to form a microporous membrane; and the like.

[0212] Examples of porous sheets formed from fibrous materials include porous sheets formed from the following fibrous materials (for example, nonwoven fabrics, paper, etc.): polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; heat-resistant resins such as wholly aromatic polyamide, polyamideimide, polyimide, polyethersulfone, polysulfone, polyetherketone, and polyetherimide; cellulose; and the like.

[0213] For a porous substrate, various surface treatments can be carried out within the range that does not damage the properties of the porous substrate. If a surface treatment is performed on the porous substrate, the wettability with the coating liquid for forming the heat-resistant porous layer or the resin particle dispersion liquid for forming the adhesive layer can be improved.

[0214] Examples of the surface treatment include corona treatment, plasma treatment, flame treatment, ultraviolet irradiation treatment, etc.

[0215] 〔Properties of the porous substrate〕

[0216] <<Thickness>>

[0217] From the viewpoint of improving the energy density of the battery, the thickness of the porous substrate is preferably 10.0 μm or less, more preferably 9.0 μm or less. In addition, from the viewpoints of the manufacturing yield of the separator and the manufacturing yield of the battery, the thickness of the porous substrate is preferably 3.0 μm or more, more preferably 4.0 μm or more.

[0218] The thickness of the porous substrate is the value measured using a contact type thickness gauge (LITEMATIC, manufactured by Mitutoyo Corporation) with a cylindrical measuring terminal having a diameter of 5 mm. During the measurement, it is adjusted to apply a load of 0.01 N, and 20 arbitrary points within 10 cm × 10 cm are measured, and the average value is calculated.

[0219] <<Gurley value>>

[0220] From the viewpoint of obtaining good ion permeability, the Gurley value of the porous substrate is preferably 50 seconds / 100 mL or more, more preferably 60 seconds / 100 mL or more. In addition, from the viewpoint of suppressing the short circuit of the battery, the Gurley value of the porous substrate is preferably 400 seconds / 100 mL or less, more preferably 200 seconds / 100 mL or less.

[0221] The Gurley value of the porous substrate is the value measured in accordance with JIS P8117:2009. As the measuring device, for example, the Gurley type air permeability measuring instrument G-B2C manufactured by Toyo Seiki Co., Ltd. can be preferably used.

[0222] <<Porosity>>

[0223] From the viewpoints of obtaining appropriate membrane resistance and shut-off function, the porosity of the porous substrate is preferably 20% to 60%.

[0224] The porosity of the porous substrate is calculated by the following formula. It should be noted that the weight per unit area is the mass per unit area.

[0225] ε={1 - Ws / (ds·t)}×100

[0226] Where Ws represents the weight per unit area of ​​the porous substrate (g / m 2 ), ds represents the true density of the porous substrate (g / cm 3 ), t represents the thickness of the porous substrate (μm).

[0227] The porosity ε (%) of the laminated body in which the porous substrate and the heat-resistant porous layer are laminated is determined by the following formula.

[0228] ε={1-(Wa / da+Wb / db+Wc / dc+…+Wn / dn) / t}×100

[0229] Wherein, the constituent materials of the porous substrate and the heat-resistant porous layer are a, b, c, ..., n, and the mass of each constituent material is Wa, Wb, Wc, ..., Wn (g / cm 2 ), the true density of each constituent material is da, db, dc, ..., dn (g / cm 3 ), the total thickness of the porous substrate and the heat-resistant porous layer is t (μm).

[0230] <<Punch Strength>>

[0231] From the viewpoint of the manufacturing yield of the separator and the manufacturing yield of the battery, the puncture strength of the porous substrate is preferably 200 g or more, and more preferably 250 g or more.

[0232] The penetration strength of the porous substrate refers to the maximum penetration load (g) measured by a penetration test using a KES-G5 hand-held compression tester manufactured by Kato Tech Co., Ltd., under the conditions of a curvature radius of the needle tip of 0.5 mm and a penetration speed of 2 mm / sec.

[0233] [Characteristics of diaphragm]

[0234] <<Thickness>>

[0235] From the viewpoint of mechanical strength of the separator, the thickness of the separator of the present disclosure is preferably 6.0 μm or more, more preferably 7.0 μm or more. From the viewpoint of battery energy density, the thickness of the separator of the present disclosure is preferably 20.0 μm or less, more preferably 15.0 μm or less.

[0236] The thickness of the separator was measured using a contact thickness gauge (LITEMATIC, manufactured by Mitutoyo Co., Ltd.) using a cylindrical measuring terminal with a diameter of 5 mm. During the measurement, a load of 0.01 N was applied, and 20 random points within 10 cm×10 cm were measured, and the average value was calculated.

[0237] <<Puncture Strength>>

[0238] From the viewpoints of the mechanical strength of the separator and the short-circuit resistance of the battery, the puncture strength of the separator of the present disclosure is preferably 200 g to 1000 g, more preferably 250 g to 600 g.

[0239] The puncture strength of the separator refers to the maximum puncture load (g) measured by performing a puncture test using a KES-G5 hand-held compression tester manufactured by Kato Tech under the conditions that the radius of curvature of the needle tip is 0.5 mm and the puncture speed is 2 mm / second.

[0240] <<Porosity>>

[0241] From the viewpoints of adhesiveness to the electrode, operability of the separator, ion permeability, and mechanical strength, the porosity of the separator of the present disclosure is preferably 30% to 60%.

[0242] The porosity ε (%) of the separator is obtained by the following formula.

[0243] ε = {1 - (Wa / da + Wb / db + Wc / dc + … + Wn / dn) / t} × 100

[0244] In the formula, the constituent materials of the separator are a, b, c, …, n, the mass of each constituent material is Wa, Wb, Wc, …, Wn (g / cm 2 ), the true density of each constituent material is da, db, dc, …, dn (g / cm 3 ), and the thickness of the separator is t (cm).

[0245] <<Membrane Resistance (Ion Permeability)>>

[0246] From the viewpoint of the load characteristics of the battery, the membrane resistance of the separator of the present disclosure is preferably 0.5 ohm·cm 2 to 10 ohm·cm 2 , more preferably 1 ohm·cm 2 to 8 ohm·cm 2 .

[0247] The membrane resistance of the separator refers to the resistance value in a state where the separator is impregnated with an electrolytic solution and is a value measured by an AC method. The measurement is performed at 20°C using 1 mol / L LiBF4 propylene carbonate / ethylene carbonate (1 / 1 [mass ratio]) as the electrolytic solution.

[0248] <<Gurley Value>>

[0249] From the viewpoint of the balance between mechanical strength and ion permeability, the Gurley value of the diaphragm of the present disclosure is preferably 50 seconds / 100 mL or more, more preferably 80 seconds / 100 mL or more, and further preferably 100 seconds / 100 mL or more. From the same viewpoint, the Gurley value of the diaphragm is preferably 800 seconds / 100 mL or less, more preferably 500 seconds / 100 mL or less, and further preferably 400 seconds / 100 mL or less.

[0250] The Gurley value of the separator is a value measured in accordance with JIS P8117: 2009. As a measuring apparatus, for example, a Gurley Densometer G-B2C manufactured by Toyo Seiki Co., Ltd. can be preferably used.

[0251] For the separator of the present disclosure, from the viewpoint of ion permeability, the value obtained by subtracting the Gurley value of the porous substrate from the Gurley value of the separator (a state in which a heat-resistant porous layer and an adhesive layer are formed on the porous substrate) is preferably 300 seconds / 100mL or less, more preferably 280 seconds / 100mL or less, and further preferably 275 seconds / 100mL or less. In addition, for the separator of the present disclosure, from the viewpoint of having an amount of adhesive resin particles sufficient to adhere to the electrode, the value obtained by subtracting the Gurley value of the porous substrate from the Gurley value of the separator is preferably 20 seconds / 100mL or more, more preferably 50 seconds / 100mL or more, and further preferably 55 seconds / 100mL or more.

[0252] <<Heat Shrinkage>>

[0253] The separator of the present disclosure preferably has a shrinkage in the MD direction (also referred to as "heat shrinkage") when heat treated at 130°C for 60 minutes of 15% or less, more preferably 12% or less, and even more preferably 9% or less. The heat shrinkage is preferably greater than 0%, and more preferably 1% or more.

[0254] The thermal shrinkage rate of the separator was determined by the following method.

[0255] Cut the diaphragm with 100 mm in MD direction and 100 mm in TD direction. Then, draw a reference line of 70 mm in length along the MD direction by passing through the center of the cut diaphragm to make a test piece. After arranging the test piece between two A4-sized papers, let it stand in an oven at 130°C for 60 minutes. Measure the length of the test piece in the MD direction before and after the heat treatment, and calculate the thermal shrinkage rate using the following formula. Perform the above operation twice more, average the thermal shrinkage rates of the three test pieces, and calculate the thermal shrinkage rate of the diaphragm.

[0256] Thermal shrinkage (%) = {(length in MD direction before heat treatment - length in MD direction after heat treatment) / length in MD direction before heat treatment} × 100

[0257] [Method for manufacturing diaphragm]

[0258] The separator of the present disclosure can be produced, for example, by the following production method A or production method B. In the production method A and the production method B, the heat-resistant porous layer may be formed by a wet coating method or a dry coating method.

[0259] The manufacturing method B may be any of the following modes B-1 to B-7. Modes B-1 to B-4 are modes in which the heat-resistant porous layer is formed by a wet coating method. Modes B-5 to B-7 are modes in which the heat-resistant porous layer is formed by a dry coating method.

[0260] In the present disclosure, the wet coating method refers to a method of solidifying a coating layer in a solidifying liquid, and the dry coating method refers to a method of drying a coating layer to solidify the coating layer.

[0261] Manufacturing method A (discontinuous manufacturing method):

[0262] After forming a heat-resistant porous layer on the porous substrate drawn out from the reel to obtain a laminate of the porous substrate and the heat-resistant porous layer, the laminate is temporarily wound on another reel. Next, an adhesive layer is formed on the laminate drawn out from the reel to obtain a separator, and the obtained separator is wound on another reel.

[0263] Manufacturing method B (continuous manufacturing method):

[0264] A heat-resistant porous layer and an adhesive layer are formed continuously or simultaneously on the porous substrate unwound from the reel, and the resulting separator is wound around another reel.

[0265] Method B-1:

[0266] A coating liquid for forming a heat-resistant porous layer is applied to a porous substrate, and the substrate is immersed in a coagulation liquid to solidify the coating layer, pulled out of the coagulation liquid, washed with water and dried. Subsequently, an adhesive resin particle dispersion is applied and dried.

[0267] Method B-2:

[0268] A coating liquid for forming a heat-resistant porous layer is applied to a porous substrate, and the substrate is immersed in a coagulation liquid to solidify the coating layer, and then pulled out of the coagulation liquid and washed with water. Subsequently, an adhesive resin particle dispersion is applied and the substrate is dried.

[0269] Method B-3:

[0270] The heat-resistant porous layer-forming coating liquid and the adhesive resin particle dispersion liquid are simultaneously coated on the porous substrate in two layers, and the substrate is immersed in a coagulation liquid to solidify the former coating layer, which is then pulled out of the coagulation liquid, washed with water, and dried.

[0271] Method B-4:

[0272] A coating liquid for forming a heat-resistant porous layer is applied to a porous substrate, and the substrate is immersed in a coagulation liquid to solidify the coating layer, and the substrate is pulled out of the coagulation liquid and transported in a water bath containing adhesive resin particles to thereby wash the substrate with water and allow the adhesive resin particles to adhere, and the substrate is pulled out of the water bath and dried.

[0273] Method B-5:

[0274] A heat-resistant porous layer-forming coating liquid is applied onto a porous substrate and dried, and then an adhesive resin particle dispersion is applied thereto and dried.

[0275] Method B-6:

[0276] A heat-resistant porous layer-forming coating liquid is applied onto a porous substrate, and then an adhesive resin particle dispersion liquid is applied thereto, followed by drying.

[0277] Method B-7:

[0278] The heat-resistant porous layer-forming coating liquid and the adhesive resin particle dispersion liquid are simultaneously applied as two layers on the porous substrate and dried.

[0279] Hereinafter, the details of the steps included in the production method will be described by taking the production method B of embodiment B-1 as an example.

[0280] In the manufacturing method B of the embodiment B-1, a heat-resistant porous layer is formed on at least one surface of a porous substrate by a wet coating method to obtain a laminate of the porous substrate and the heat-resistant porous layer, and then an adhesive layer is formed on at least one surface of the laminate by a dry coating method. The manufacturing method B of the embodiment B-1 includes the following steps (1) to (7), and the steps (1) to (7) are performed in sequence.

[0281] Step (1): Preparation of coating liquid for forming heat-resistant porous layer

[0282] The coating liquid for forming the heat-resistant porous layer (hereinafter referred to as "coating liquid" in the description of the manufacturing method) is prepared by dissolving or dispersing an aromatic resin and inorganic particles in a solvent. In the coating liquid, components other than the aromatic resin and the inorganic particles are dissolved or dispersed as needed.

[0283] The solvent used for preparing the coating liquid includes a solvent that dissolves the aromatic resin (hereinafter also referred to as a "good solvent"). Examples of the good solvent include polar amide solvents such as N-methylpyrrolidone, dimethylacetamide, and dimethylformamide.

[0284] From the viewpoint of forming a heat-resistant porous layer with a good porous structure, the solvent used to prepare the coating liquid preferably contains a phase separation agent that induces phase separation. Therefore, the solvent used to prepare the coating liquid is preferably a mixed solvent of a good solvent and a phase separation agent. The phase separation agent is preferably mixed with the good solvent in an amount that can ensure a range of viscosity suitable for coating. As the phase separation agent, water, methanol, ethanol, propanol, butanol, butanediol, ethylene glycol, propylene glycol, tripropylene glycol, etc. can be cited.

[0285] As a solvent for preparing the coating liquid, from the viewpoint of forming a heat-resistant porous layer having a good porous structure, a mixed solvent is preferably used, which is a mixed solvent of a good solvent and a phase separation agent, containing 60% by mass or more of a good solvent and 5% to 40% by mass of a phase separation agent.

[0286] From the viewpoint of forming a heat-resistant porous layer having a good porous structure, the concentration of the aromatic resin in the coating liquid is preferably 1% by mass to 20% by mass.

[0287] From the viewpoint of forming a heat-resistant porous layer having a good porous structure, the concentration of the inorganic particles in the coating liquid is preferably 2% by mass to 50% by mass.

[0288] Step (2): Preparation of Adhesive Resin Particle Dispersion

[0289] The adhesive resin particle dispersion is prepared by dispersing adhesive resin particles in water. A surfactant may be added to the adhesive resin particle dispersion to improve the dispersibility of the adhesive resin particles in water. The adhesive resin particle dispersion may be a commercial product or a diluted solution of a commercial product.

[0290] From the viewpoint of coating suitability, the concentration of the adhesive resin particles in the adhesive resin particle dispersion is preferably 1% by mass to 60% by mass.

[0291] Step (3): Application of coating liquid

[0292] The coating liquid is applied to at least one surface of the porous substrate to form a coating layer on the porous substrate. As the coating method of the coating liquid on the porous substrate, knife coating, Meyer rod coating, die coating, reverse roll coating, roller coating, gravure coating, screen printing, inkjet, spraying, etc. can be cited. In the case of forming a heat-resistant porous layer on both sides of the porous substrate, it is preferred to apply the coating liquid to both sides of the porous substrate at the same time from the viewpoint of productivity.

[0293] Step (4): Curing of the coating layer

[0294] The porous substrate having the coating layer formed thereon is immersed in a coagulation liquid to induce phase separation in the coating layer while solidifying the aromatic resin to form a heat-resistant porous layer. Thus, a laminate composed of the porous substrate and the heat-resistant porous layer is obtained.

[0295] The coagulation liquid generally contains a good solvent and a phase separation agent used in the preparation of the coating liquid, and water. From the production point of view, the mixing ratio of the good solvent and the phase separation agent is preferably consistent with the mixing ratio of the mixed solvent used in the preparation of the coating liquid. From the viewpoint of the formation of the porous structure and productivity, the water content in the coagulation liquid is preferably 40% to 90% by mass. The temperature of the coagulation liquid is, for example, 20°C to 50°C.

[0296] Step (5): Washing and drying of the coating layer

[0297] The laminate is lifted from the coagulation liquid and washed with water. The coagulation liquid is removed from the laminate by washing with water. Furthermore, water is removed from the laminate by drying. Washing with water is performed, for example, by conveying the laminate in a water bath. Drying is performed, for example, by conveying the laminate in a high temperature environment, blowing air on the laminate, or contacting the laminate with a hot roller. The drying temperature is preferably 40°C to 80°C.

[0298] Step (6): Application of Adhesive Resin Particle Dispersion

[0299] The adhesive resin particle dispersion is applied to at least one surface of the laminate. Examples of the method for applying the adhesive resin particle dispersion include knife coating, gravure coating, Meyer bar coating, die coating, reverse roll coating, roll coating, screen printing, inkjet, and spray coating.

[0300] Step (7): Drying of Adhesive Resin Particle Dispersion

[0301] The adhesive resin particle dispersion on the laminate is dried to allow the adhesive resin particles to adhere to the surface of the laminate. Drying is performed, for example, by conveying the laminate in a high temperature environment or blowing air to the laminate. The drying temperature is preferably 40°C to 100°C.

[0302] The manufacturing method A for manufacturing a separator or the manufacturing method B of the aspects B-2 to B-7 can be implemented by omitting or changing a part of the above-mentioned steps (1) to (7).

[0303] [Non-aqueous secondary battery]

[0304] The nonaqueous secondary battery of the present disclosure is a nonaqueous secondary battery that obtains electromotive force by doping and dedoping lithium, and includes a positive electrode, a negative electrode, and a separator for a nonaqueous secondary battery of the present disclosure disposed between the positive electrode and the negative electrode.

[0305] The so-called "doping" refers to storage, loading, adsorption, or insertion, and refers to the phenomenon that lithium ions enter the active material of an electrode such as a positive electrode.

[0306] In addition, the non-aqueous secondary battery of the present disclosure is a non-aqueous secondary battery comprising a positive electrode, a negative electrode and a separator arranged between the positive electrode and the negative electrode, wherein the non-aqueous secondary battery comprises a heat-resistant porous layer containing an aromatic resin and inorganic particles, and an adhesive layer arranged on the heat-resistant porous layer, wherein the adhesive layer is formed by attaching adhesive resin particles containing a phenyl-containing acrylic resin to the heat-resistant porous layer, and the separator is bonded to the positive electrode or the negative electrode via the adhesive layer, and when the separator and the electrode are peeled off, the adhesive resin particles are attached to both the heat-resistant porous layer and the electrode.

[0307] The "separator" herein has the same meaning as the separator for a non-aqueous secondary battery in the present disclosure, and the preferred embodiments are also the same.

[0308] The nonaqueous secondary battery of the present disclosure has a structure in which a battery element (a negative electrode and a positive electrode facing each other via a separator) is sealed in an outer packaging material together with an electrolyte. The nonaqueous secondary battery of the present disclosure is suitable for nonaqueous electrolyte secondary batteries, especially lithium ion secondary batteries.

[0309] The nonaqueous secondary battery of the present disclosure has excellent battery productivity and battery cycle characteristics (capacity retention rate) because the separator of the present disclosure has excellent adhesion to the electrode in either dry hot pressing or wet hot pressing.

[0310] Hereinafter, examples of the positive electrode, the negative electrode, the electrolyte solution, and the outer casing material included in the non-aqueous secondary battery of the present disclosure will be described.

[0311] As an embodiment example of the positive electrode, there can be mentioned a structure in which an active material layer including a positive electrode active material and a binder resin is formed on a current collector. The active material layer may further include a conductive auxiliary agent.

[0312] Examples of the positive electrode active material include lithium-containing transition metal oxides, specifically LiCoO2, LiNiO2, LiMn 1 / 2 Ni 1 / 2 O2、LiCo 1 / 3 Mn 1 / 3 Ni 1 / 3O2, LiMn2O4, LiFePO4, LiCo 1 / 2 Ni 1 / 2 O2、LiAl 1 / 4Ni 3 / 4 O2 and other compounds.

[0313] Examples of the binder resin include polyvinylidene fluoride resins and styrene-butadiene copolymers.

[0314] Examples of the conductive auxiliary agent include carbon materials such as acetylene black, Ketjen black, and graphite powder.

[0315] Examples of the current collector include metal foils such as aluminum foil, titanium foil, and stainless steel foil having a thickness of 5 μm to 20 μm.

[0316] As an embodiment example of the negative electrode, there can be mentioned a structure in which an active material layer including a negative electrode active material and a binder resin is formed on a current collector. The active material layer may further include a conductive auxiliary agent.

[0317] Examples of the negative electrode active material include materials that can electrochemically absorb lithium, and specifically, carbon materials; alloys of lithium and silicon, tin, aluminum, etc.; Wood's alloys; and the like.

[0318] Examples of the binder resin include polyvinylidene fluoride resins and styrene-butadiene copolymers.

[0319] Examples of the conductive auxiliary agent include carbon materials such as acetylene black, Ketjen black, and graphite powder.

[0320] Examples of the current collector include metal foils such as copper foil, nickel foil, and stainless steel foil having a thickness of 5 μm to 20 μm. Alternatively, a metal lithium foil may be used as the negative electrode instead of the negative electrode described above.

[0321] The electrolyte solution is a solution obtained by dissolving a lithium salt in a non-aqueous solvent.

[0322] Examples of the lithium salt include compounds such as LiPF6, LiBF4, and LiClO4. The lithium salt may be used alone or in combination of two or more.

[0323] Examples of the non-aqueous solvent include cyclic carbonates such as ethylene carbonate, propylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and fluorinated products thereof; cyclic esters such as γ-butyrolactone and γ-valerolactone; and other solvents. The non-aqueous solvent may be used alone or in combination of two or more.

[0324] As the electrolyte solution, a solution prepared by mixing a cyclic carbonate and a chain carbonate at a mass ratio of 20:80 to 40:60 (cyclic carbonate:chain carbonate) and dissolving a lithium salt in a range of 0.5 mol / L to 1.5 mol / L is suitable.

[0325] Examples of the outer packaging material include metal cases and aluminum laminated film packaging.

[0326] The shape of the battery includes, for example, square, cylindrical, button, etc. The separator of the present disclosure is suitable for any shape.

[0327] [Method for producing non-aqueous secondary battery]

[0328] As a method for manufacturing a non-aqueous secondary battery of the present disclosure, for example, there can be cited a first manufacturing method comprising the following steps: a stacking step of manufacturing a stacked body in which the separator of the present disclosure is arranged between the positive electrode and the negative electrode; a dry bonding step of performing dry hot pressing on the stacked body so that at least one of the positive electrode and the negative electrode is bonded to the separator; and a sealing step of sealing the stacked body that has undergone the dry bonding step together with the electrolyte inside the outer packaging material.

[0329] In addition, as a method for manufacturing a non-aqueous secondary battery of the present disclosure, for example, a second manufacturing method can be cited, which includes the following steps: a stacking step, in which a stack is manufactured by arranging the separator of the present disclosure between the positive electrode and the negative electrode; a sealing step, in which the stack is sealed together with the electrolyte inside the outer packaging material; and a wet bonding step, in which the stack that has undergone the sealing step is wet hot-pressed from above the outer packaging material to bond at least one of the positive electrode and the negative electrode to the separator.

[0330] (First Manufacturing Method)

[0331] The lamination step is a step of manufacturing a laminated body in which the separator of the present disclosure is arranged between the positive electrode and the negative electrode. The lamination step may be, for example, a step of manufacturing a wound body (so-called wound-type laminated body) by arranging the separator of the present disclosure between the positive electrode and the negative electrode and winding it in the length direction, or a step of manufacturing a laminated body by sequentially laminating at least one layer of the positive electrode, the separator, and the negative electrode.

[0332] The dry bonding step is a step of bonding at least one of the positive electrode and the negative electrode to the separator by dry hot pressing the laminate.

[0333] The dry bonding process may be performed before the stack is placed in an outer packaging material (e.g., an aluminum laminated film package), or after the stack is placed in the outer packaging material. That is, the stack formed by bonding the electrode and the separator by dry hot pressing may be placed in the outer packaging material, or after the stack is placed in the outer packaging material, dry hot pressing may be performed from above the outer packaging material to bond the electrode and the separator.

[0334] The pressing temperature in the dry bonding step is preferably 50°C to 120°C, more preferably 60°C to 110°C, and even more preferably 70°C to 100°C.

[0335] When the pressing temperature in the bonding process is within the above range, the bonding between the electrode and the separator is moderately good, and the separator can be moderately expanded in the width direction, so there is a tendency that the battery is not prone to short circuit. In addition, since the electrode and the separator are moderately bonded, there is a tendency that the impregnation of the electrolyte is not easily hindered.

[0336] The pressurization pressure in the dry bonding step is preferably 0.1 MPa to 10 MPa, more preferably 0.5 MPa to 5 MPa.

[0337] The pressing time in the dry bonding step is preferably adjusted according to the pressing temperature and the pressing pressure, and is adjusted within the range of, for example, 0.1 minutes to 60 minutes.

[0338] After the lamination step and before the dry bonding step, the laminate may be temporarily bonded by applying pressurization at room temperature (pressurization at room temperature).

[0339] The sealing step is a step of sealing the laminated body that has undergone the dry bonding step together with the electrolyte solution inside the outer packaging material.

[0340] In the sealing process, for example, after injecting the electrolyte into the outer packaging material containing the laminate, the opening of the outer packaging material is sealed. The opening of the outer packaging material can be sealed, for example, by bonding the opening of the outer packaging material with an adhesive; or by heating and pressurizing the opening of the outer packaging material to perform thermocompression bonding. Before sealing the opening of the outer packaging material, it is preferred that the interior of the outer packaging body is in a vacuum state.

[0341] In the sealing process, it is preferred that the opening of the outer packaging material is heated and pressurized for thermocompression bonding, and the laminate is thermocompressed from above the outer packaging material. By performing the thermocompression treatment (so-called wet thermocompression) in the state where the laminate and the electrolyte coexist, the bonding between the electrode and the separator is more firmly achieved.

[0342] The pressing temperature of the wet hot pressing performed in the sealing step is preferably 60° C. to 110° C., the pressing pressure is preferably 0.5 MPa to 5 MPa, and the pressing time is preferably adjusted according to the pressing temperature and the pressing pressure, for example, within the range of 0.5 minutes to 60 minutes.

[0343] (Second Manufacturing Method)

[0344] The lamination step is a step of manufacturing a laminated body in which the separator of the present disclosure is arranged between the positive electrode and the negative electrode. The lamination step is similar to the lamination step in the first manufacturing method, for example, it can be a step of arranging the separator of the present disclosure between the positive electrode and the negative electrode and winding it in the length direction to manufacture a wound body (so-called wound-type laminated body), or it can be a step of laminating the positive electrode, the separator, and the negative electrode in sequence by at least one layer each to manufacture a laminated body.

[0345] The sealing step is a step of sealing the laminate together with the electrolyte solution inside the outer packaging material.

[0346] In the sealing process, for example, after injecting the electrolyte into the outer packaging material (for example, an aluminum laminated film package) containing the laminate, the opening of the outer packaging material is sealed. The opening of the outer packaging material can be sealed, for example, by bonding the opening of the outer packaging material with an adhesive; or by heating and pressurizing the opening of the outer packaging material for thermocompression bonding. Before sealing the opening of the outer packaging material, it is preferred that the interior of the outer packaging body is in a vacuum state.

[0347] The wet bonding step is a step of subjecting the laminated body that has undergone the sealing step, i.e., the laminated body housed in the outer packaging material together with the electrolyte, to hot pressing (so-called wet hot pressing) from above the outer packaging material to bond at least one of the positive electrode and the negative electrode to the separator.

[0348] The pressing temperature in the wet bonding step is preferably 60°C to 110°C, more preferably 70°C to 100°C, and even more preferably 70°C to 90°C.

[0349] When the pressing temperature in the wet bonding step is within the above range, decomposition of the electrolyte solution can be suppressed, and adhesion between the electrode and the separator becomes good. In addition, the separator can appropriately expand in the width direction, so short circuiting of the battery tends to be less likely to occur.

[0350] The pressurization pressure in the wet bonding step is preferably 0.1 MPa to 5 MPa, more preferably 0.5 MPa to 3 MPa.

[0351] The pressing time in the wet bonding step is preferably adjusted according to the pressing temperature and the pressing pressure, and is adjusted within the range of, for example, 0.1 minutes to 60 minutes.

[0352] Example

[0353] Hereinafter, the separator and the non-aqueous secondary battery of the present disclosure are described in more detail by way of examples. The materials, usage amounts, ratios, processing steps, etc. shown in the following examples may be appropriately changed without departing from the gist of the present invention. Therefore, the scope of the separator and the non-aqueous secondary battery of the present disclosure should not be interpreted restrictively based on the specific examples shown below.

[0354] [Measurement method and evaluation method]

[0355] The measuring methods and evaluation methods used in Examples and Comparative Examples are as follows.

[0356] [Thickness of porous substrate, separator and heat-resistant porous layer]

[0357] The thickness (μm) of the porous substrate, separator, and heat-resistant porous layer was measured using a contact-type thickness meter [LITEMATIC VL-50, manufactured by Mitutoyo Corporation].

[0358] A cylindrical terminal with a diameter of 5 mm was used as a measurement terminal, and during the measurement, the load was adjusted so as to apply 0.01 N. The thickness was measured at 20 points randomly selected within 10 cm×10 cm, and the average value thereof was determined.

[0359] 〔Weight per unit area〕

[0360] For unit area weight (per 1m 2 Mass, g / m 2 ), the sample was cut into 10 cm × 30 cm, the mass was measured, and the mass was divided by the area to obtain the mass.

[0361] [Mass per unit area of ​​heat-resistant porous layer]

[0362] The mass per unit area of ​​the heat-resistant porous layer (g / m 2 ) is the weight per unit area after layer formation (g / m 2 ) minus the unit area weight before layer formation (g / m 2 ) and thus find out.

[0363] [Amount of adhesive resin particles attached to the heat-resistant porous layer]

[0364] The adhesion amount (g / m 2 ) is the weight per unit area after layer formation (g / m 2 ) minus the unit area weight before layer formation (g / m 2 ) is thus obtained.

[0365] [Gurley value]

[0366] The Gurley value (seconds / 100 mL) of the porous substrate and the separator was measured by a method in accordance with JIS P 8117: 2009. As a measuring apparatus, a Gurley type air permeometer [G-B2C, manufactured by Toyo Seiki Co., Ltd.] was used.

[0367] [Porosity (porous substrate, porous substrate + heat-resistant porous layer)]

[0368] The porosity ε (%) of the porous substrate and the laminate of the porous substrate and the heat-resistant porous layer can be determined by the following formula.

[0369] ε={1-(Wa / da+Wb / db+Wc / dc+…+Wn / dn) / t}×100

[0370] Wherein, the constituent materials of the porous substrate and the heat-resistant porous layer are a, b, c, ..., n, and the mass of each constituent material is Wa, Wb, Wc, ..., Wn (g / cm 2 ), the true density of each constituent material is da, db, dc, ..., dn (g / cm 3 ), the total thickness of the porous substrate and the heat-resistant porous layer is t (μm).

[0371] [Glass transition temperature of resin particles contained in adhesive layer]

[0372] The glass transition temperature of the resin particles contained in the adhesive layer is obtained from the differential scanning calorimetry (DSC) curve obtained by differential scanning calorimetry (DSC). As a measuring device, a differential scanning calorimeter [Q20 Differential Scanning Calorimeter, manufactured by TA Instruments] is used, and 10 mg of resin particles are used as a sample. The temperature at the point where the straight line extending the baseline on the low temperature side to the high temperature side intersects with the tangent with the largest slope among the tangents of the curve of the step-shaped change portion is taken as the glass transition temperature of the resin particles.

[0373] [Melting point of resin particles contained in adhesive layer]

[0374] The melting point of the resin particles contained in the adhesive layer is determined from a differential scanning calorimetry curve (DSC curve) obtained by differential scanning calorimetry (DSC: Differential Scanning Calorimetry). As a measuring device, a differential scanning calorimeter [Q20 Differential Scanning Calorimeter, manufactured by TA Instruments] is used, and 10 mg of resin particles are used as a sample. Under a nitrogen atmosphere, the sample is heated from 30°C to 200°C at a heating rate of 5°C / min, then cooled from 200°C to 30°C at a cooling rate of 2°C / min, and further heated from 30°C to 200°C at a heating rate of 2°C / min. The peak top of the endothermic peak obtained at this time is taken as the melting point of the resin particles.

[0375] [Average primary particle size of inorganic particles contained in the heat-resistant porous layer]

[0376] The average primary particle size of the inorganic particles contained in the heat-resistant porous layer is obtained by measuring the major diameters of 100 inorganic particles randomly selected in the observation based on a scanning electron microscope (SEM), and averaging the major diameters of the 100 particles. The sample for SEM observation is an inorganic particle as a material for forming the heat-resistant porous layer. There is no restriction on the method of removing the inorganic particles from the heat-resistant porous layer of the separator.

[0377] [Volume average particle size of resin particles contained in adhesive layer]

[0378] The resin particles were dispersed in water containing Triton (registered trademark) X-100 [Compound name: polyethylene glycol tert-octylphenyl ether, manufactured by Dow Chemical Co.] as a nonionic surfactant, and the particle size distribution was measured using a laser diffraction particle size distribution measuring device [Mastersize 2000, manufactured by Sysmex Co., Ltd.]. In the volume-based particle size distribution, the particle size (D50) at which the accumulation from the smaller diameter side is 50% was taken as the volume average particle size (μm) of the resin particles.

[0379] [Peak area S1 of phenyl group in adhesive layer obtained by Fourier transform infrared spectroscopy]

[0380] The absorption spectrum of the adhesive layer was obtained by Fourier transform infrared spectroscopy (FT-IR) under the following conditions. The absorption peak of the phenyl group (694 cm -1 ~710cm -1) to perform baseline correction, and find the area of ​​the range surrounded by the baseline and the absorption spectrum line (unit: dimensionless). The values ​​obtained from the absorption spectra of 8 different ranges selected at random are averaged to obtain the peak area S1 of the phenyl group in the adhesive layer. The conditions of FT-IR are shown below.

[0381] -condition-

[0382] Measuring device: Fourier transform infrared spectrophotometer [IRAffinity-1, manufactured by Shimadzu Corporation]

[0383] Measurement wavelength range: 400cm -1 ~4000cm -1

[0384] Measurement mode: transmittance

[0385] Apodization function: Happ-Genzel

[0386] Resolution: 4cm -1

[0387] Cumulative times: 10 times

[0388] Number of samples measured: n = 8

[0389] [Peak area of ​​carbonyl group S2]

[0390] The absorption spectrum of the adhesive layer was obtained by Fourier transform infrared spectroscopy (FT-IR) under the following conditions. The absorption peak of the carbonyl group (1707 cm -1 ~1753cm -1 ) to perform baseline correction, and find the area of ​​the range surrounded by the baseline and the absorption spectrum line (unit: dimensionless). The values ​​obtained from the absorption spectra of 8 different ranges selected at random are averaged to be the peak area S2 of the carbonyl group of the adhesive layer. The conditions of FT-IR are the same as those of the peak area S1.

[0391] [Peak area of ​​CF bond S3]

[0392] The absorption spectrum of the adhesive layer was obtained by Fourier transform infrared spectroscopy (FT-IR) under the following conditions, and the absorption peak of the CF bond (862 cm -1 ~901cm -1 ) to perform baseline correction, and find the area of ​​the range surrounded by the baseline and the absorption spectrum line (unit: dimensionless). The values ​​obtained from the absorption spectra of 8 different ranges selected at random are averaged to be the peak area S3 of the CF bond of the adhesive layer. The conditions of FT-IR are the same as those of the peak area S1.

[0393] [Swelling degree of resin particles contained in adhesive layer]

[0394] The aqueous dispersion of resin particles was poured onto a glass plate with a metal frame having an inner size of 50 mm × 70 mm, and dried at 150°C for 1 hour to prepare a sheet-shaped sample for measurement. About 1 g of the sample for measurement prepared above was cut out, and its weight W1 (g) was accurately measured using an electronic balance, and then immersed in an electrolyte solution [1 mol / L LiBF4 ethylene carbonate: ethyl methyl carbonate (volume ratio 3:7)] at 60°C for 24 hours. The immersed sample for measurement was taken out of the electrolyte solution, and after wiping off the electrolyte solution attached to the surface, its weight W2 (g) was measured using an electronic balance, and the swelling degree (%) of the resin particles was calculated using the following formula.

[0395] Swelling degree (%) = (W2 / W1) × 100

[0396] [Thermal shrinkage of diaphragm]

[0397] Cut the diaphragm with 100 mm in MD direction and 100 mm in TD direction. Then, draw a reference line of 70 mm in length along the MD direction by passing through the center of the cut diaphragm to make a test piece. After arranging the test piece between two A4-sized papers, let it stand in an oven at 130°C for 60 minutes. Measure the length of the test piece in the MD direction before and after the heat treatment, and calculate the thermal shrinkage rate using the following formula. Perform the above operation twice more, average the thermal shrinkage rates of the three test pieces, and calculate the thermal shrinkage rate of the diaphragm.

[0398] Thermal shrinkage (%) = {(length in MD direction before heat treatment - length in MD direction after heat treatment) / length in MD direction before heat treatment} × 100

[0399] [Bond strength between electrode and separator: dry hot pressing]

[0400] A double-arm mixer was used to stir and mix 97 g of lithium cobalt oxide powder as a positive electrode active material, 1.5 g of acetylene black as a conductive aid, 1.5 g of polyvinylidene fluoride as a binder, and an appropriate amount of N-methylpyrrolidone to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum foil having a thickness of 20 μm, and pressed after drying to obtain a positive electrode (single-sided coating) having a positive electrode active material layer.

[0401] The positive electrode obtained above is cut out with a width of 15 mm and a length of 70 mm, the separator is cut out with a width of 18 mm in the TD direction and a length of 75 mm in the MD direction, and the aluminum foil with a thickness of 20 μm is cut out with a width of 15 mm and a length of 70 mm. A laminate is made by overlapping the positive electrode / separator / aluminum foil in the order of positive electrode / separator / aluminum foil, and the laminate is placed in an aluminum laminate package as an outer packaging material. Then, after the package is vacuumed using a vacuum sealer, the package is sealed. Then, a hot press is used to hot-press the laminate together with the package (temperature of 85 ° C, load of 1 MPa, and pressing time of 30 seconds) to bond the positive electrode in the package to the separator. Then, the package is unsealed, the laminate is taken out, and the product obtained by removing the aluminum foil from the laminate is used as a test piece.

[0402] The diaphragm of the test piece is fixed to the lower chuck of Tensilon [STB-1225S, manufactured by A&D Co., Ltd.]. At this time, the diaphragm is fixed to Tensilon in such a way that the length direction of the test piece (i.e., the MD direction of the diaphragm) becomes the direction of gravity. The positive electrode is peeled off from the diaphragm by about 2 cm from one end of the lower part, and the end is fixed to the upper chuck for a 180° peeling test. The tensile speed of the 180° peeling test is set to 100 mm / min. After the start of the measurement, the load (N) from 10 mm to 40 mm is collected at intervals of 0.4 mm, and the average value is calculated. The loads of the three test pieces are further averaged as the bonding strength (N / 15 mm) between the electrode and the diaphragm when dry hot pressing is performed. In Tables 3 and 4, the bonding strength between the electrode and the diaphragm when dry hot pressing is performed is expressed as "dry bonding strength between the electrode and the diaphragm".

[0403] [Bond strength between electrode and separator: wet hot pressing]

[0404] A double-arm mixer was used to stir and mix 97 g of lithium cobalt oxide powder as a positive electrode active material, 1.5 g of acetylene black as a conductive aid, 1.5 g of polyvinylidene fluoride as a binder, and an appropriate amount of N-methylpyrrolidone to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum foil having a thickness of 20 μm, and pressed after drying to obtain a positive electrode (single-sided coating) having a positive electrode active material layer.

[0405] The positive electrode obtained above was cut into a width of 15 mm and a length of 70 mm, the separator was cut into a width of 18 mm in the TD direction and a length of 75 mm in the MD direction, and the aluminum foil with a thickness of 20 μm was cut into a width of 15 mm and a length of 70 mm. A laminate was made by overlapping the positive electrode / separator / aluminum foil in the order of positive electrode / separator / aluminum foil, and the laminate was placed in an aluminum laminate package as an outer packaging material, and then an electrolyte (1 mol / L LiBF4-ethylene carbonate: diethyl carbonate: propylene carbonate [mass ratio of 1:1:1]) was injected, and vacuum degassing was repeated 5 times. Then, the excess electrolyte was removed, the package was sealed, and it was left for 24 hours. Then, a hot press was used to hot-press the laminate together with the package (temperature of 85°C, load of 1 MPa, and pressing time of 15 seconds) to bond the positive electrode in the package to the separator. Then, the package was opened, the laminate was taken out, and the aluminum foil was removed from the laminate to be used as a test piece.

[0406] The diaphragm of the test piece is fixed to the lower chuck of Tensilon [STB-1225S, manufactured by A&D Co., Ltd.]. At this time, the diaphragm is fixed to Tensilon in such a way that the length direction of the test piece (i.e., the MD direction of the diaphragm) becomes the direction of gravity. The positive electrode is peeled off from the diaphragm by about 2 cm from one end of the lower part, and the end is fixed to the upper chuck for a 180° peeling test. The tensile speed of the 180° peeling test is set to 100 mm / min. After the start of the measurement, the load (N) from 10 mm to 40 mm is collected at intervals of 0.4 mm, and the average value is calculated. The loads of the three test pieces are further averaged as the bonding strength (N / 15 mm) between the electrode and the diaphragm during wet hot pressing. In Tables 3 and 4, the bonding strength between the electrode and the diaphragm during wet hot pressing is expressed as "wet bonding strength between the electrode and the diaphragm".

[0407] [Gas generation]

[0408] Cut the diaphragm to 600 cm 2 of size, put it into an aluminum laminated film package, inject an electrolyte into the package, impregnate the electrolyte into the diaphragm, seal the package, and obtain a test battery. As the electrolyte, a 1 mol / L mixed solution of LiPF6-ethylene carbonate and ethyl methyl carbonate (LiPF6-ethylene carbonate: ethyl methyl carbonate = 3:7 [mass ratio]) was used. The test battery was placed in an environment with a temperature of 85°C for 20 days, and the volume of the test battery before and after heat treatment was measured. By subtracting the volume V1 of the test battery before heat treatment from the volume V2 of the test battery after heat treatment, the gas generation amount V (= V2-V1, unit: mL) was calculated. The gas generation amount V of the 10 test batteries was then averaged.

[0409] [Clearance of the diaphragm in the X-ray image]

[0410] (Production of negative electrode)

[0411] A double-arm mixer was used to stir 300 g of artificial graphite as a negative electrode active material, 7.5 g of a water-soluble dispersion of a modified body of a styrene-butadiene copolymer containing 40% by mass as a binder, 3 g of carboxymethyl cellulose as a thickener, and an appropriate amount of water to prepare a negative electrode slurry. The negative electrode slurry was applied to both sides of a copper foil having a thickness of 10 μm as a negative electrode collector, and the obtained coating was dried and pressed to prepare a negative electrode having a negative electrode active material layer on both sides.

[0412] (Production of positive electrode)

[0413] A double-arm mixer was used to stir 89.5 g of lithium cobalt oxide powder as a positive electrode active material, 4.5 g of acetylene black as a conductive aid, 6 g of polyvinylidene fluoride as a binder, and an appropriate amount of N-methylpyrrolidone to prepare a positive electrode slurry. The positive electrode slurry was applied to both sides of an aluminum foil with a thickness of 20 μm as a positive electrode collector, and the obtained coating was dried and pressed to prepare a positive electrode having a positive electrode active material layer on both sides.

[0414] (Preparation of samples for observation)

[0415] The positive electrode was cut into a rectangle of 30 mm × 50 mm, the negative electrode was cut into a rectangle of 30 mm × 50 mm, and the separator was cut into a rectangle of 34 mm × 54 mm. The positive electrode, separator, negative electrode, and separator were stacked in this order to produce a laminate having three layers of positive electrode and negative electrode, respectively, and five layers of separator. The laminate was inserted into an aluminum laminate film package, and the inside of the package was sealed in a vacuum state using a vacuum sealer to obtain an observation sample.

[0416] (X-ray CT observation)

[0417] The X-ray CT image was picked up using a microfocus X-ray CT system (inspeXioSMX-225CT FPD HR) manufactured by Shimadzu Corporation. The X-ray tube voltage was set to 220 kV, the X-ray tube current was set to 100 μA, and the exposure time was set to 1 sec. The thickness cross section of the laminate was imaged at the end of the sample for measurement. The GV (gray value) value of the diaphragm portion was measured from the X-ray CT image, and the clarity of the diaphragm in the X-ray image was graded according to the following criteria based on the value. The larger the GV value, the better.

[0418] Level 5: 37301 and above

[0419] Level 4: 36501 or above and 37300 or below

[0420] Level 3: 35701 or above and 36500 or below

[0421] Level 2: 35251 or above and 35700 or below

[0422] Level 1: 35250 or less

[0423] [Production of diaphragm]

[0424] (Example 1)

[0425] Meta-aramid [poly(m-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and barium sulfate particles [average primary particle size 0.05 μm; inorganic particles] are stirred and mixed in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a concentration of meta-aramid to 5 mass%, thereby obtaining a coating liquid for forming a heat-resistant porous layer.

[0426] A resin particle dispersion for forming an adhesive layer (solid content concentration of 7% by weight) was prepared by dispersing adhesive resin particles (A) containing a phenyl-containing acrylic resin [resin particles as a copolymer containing an acrylic monomer unit and a styrene monomer unit, the content mass ratio (styrene monomer unit:acrylic monomer unit) in the copolymer being 62:38, a glass transition temperature of 52°C, and a volume average particle size of 0.5 μm] and polyvinylidene fluoride (PVDF) resin particles [melting point of 140°C, volume average particle size of 0.25 μm] in water at a mixing mass ratio of 50:50.

[0427] A proper amount of coating liquid for forming a heat-resistant porous layer is loaded on a pair of Meyer rods, and a polyethylene microporous membrane (thickness 8 μm, porosity 33%, Gurley value 160 seconds / 100 mL) as a porous substrate is passed between the Meyer rods, and an equal amount of coating liquid for forming a heat-resistant porous layer is applied on both sides. It is immersed in a coagulation liquid (DMAc:TPG:water=30:8:62 [mass ratio], liquid temperature 25°C) to solidify the coating layer, and then washed in a water washing tank at a water temperature of 25°C and dried. Next, it is passed between a pair of rod coaters loaded with an appropriate amount of resin particle dispersion for forming an adhesive layer, and an equal amount of resin particle dispersion for forming an adhesive layer is applied on both sides, and dried. The above operation is performed to obtain a polyethylene microporous membrane having heat-resistant porous layers (mass per unit area 6.0 g / m 2 (total of both sides), thickness 4.0 μm (total of both sides)] and adhesive layer [mass per unit area 0.5 g / m 2(total of both sides)〕a separator (composition: adhesive layer / heat-resistant porous layer / porous substrate / heat-resistant porous layer / adhesive layer).

[0428] (Example 2)

[0429] A diaphragm was produced in the same manner as in Example 1, except that the adhesive layer-forming resin particle dispersion was changed to an adhesive layer-forming resin particle dispersion (solid content concentration: 7% by mass) containing adhesive resin particles (B) of a phenyl-containing acrylic resin [resin particles of a copolymer containing acrylic monomer units and styrene monomer units, the copolymer having a mass ratio (styrene monomer units:acrylic monomer units) of 89:11, a glass transition temperature of 50°C, and a volume average particle size of 0.5 μm] and polyvinylidene fluoride (PVDF) resin particles [melting point of 140°C, volume average particle size of 0.25 μm] dispersed in water in a mixing mass ratio of 50:50.

[0430] (Example 3)

[0431] A diaphragm was produced in the same manner as in Example 1, except that the adhesive layer-forming resin particle dispersion was changed to an adhesive layer-forming resin particle dispersion (solid content concentration: 7% by mass) containing adhesive resin particles (C) of a phenyl-containing acrylic resin [resin particles of a copolymer containing acrylic monomer units and styrene monomer units, the copolymer having a mass ratio (styrene monomer units: acrylic monomer units) of 18:82, a glass transition temperature of 54°C, and a volume average particle size of 0.5 μm] and polyvinylidene fluoride (PVDF) resin particles [melting point of 140°C, volume average particle size of 0.25 μm] dispersed in water in a mixing mass ratio of 50:50.

[0432] (Example 4)

[0433] A diaphragm was produced in the same manner as in Example 1, except that the resin particle dispersion for forming an adhesive layer was changed to a resin particle dispersion for forming an adhesive layer (solid content concentration is 7% by weight) containing adhesive resin particles (A) of a phenyl-containing acrylic resin [resin particles of a copolymer containing acrylic monomer units and styrene monomer units, the copolymer having a mass ratio (styrene monomer units: acrylic monomer units) of 62:38, a glass transition temperature of 52°C, and a volume average particle size of 0.5 μm] dispersed in water.

[0434] (Example 5)

[0435] A diaphragm was produced in the same manner as in Example 1, except that the adhesive layer-forming resin particle dispersion was changed to an adhesive layer-forming resin particle dispersion (solid content concentration: 7% by mass) containing adhesive resin particles (A) of a phenyl-containing acrylic resin [resin particles of a copolymer containing acrylic monomer units and styrene monomer units, the copolymer having a mass ratio (styrene monomer units: acrylic monomer units) of 62:38, a glass transition temperature of 52°C, and a volume average particle size of 0.5 μm] and polyvinylidene fluoride (PVDF) resin particles [melting point of 140°C, volume average particle size of 0.25 μm] dispersed in water at a mixing mass ratio of 90:10.

[0436] (Example 6)

[0437] A diaphragm was produced in the same manner as in Example 1, except that the adhesive layer-forming resin particle dispersion was changed to an adhesive layer-forming resin particle dispersion (solid content concentration: 7% by mass) containing adhesive resin particles (A) of a phenyl-containing acrylic resin [resin particles of a copolymer containing acrylic monomer units and styrene monomer units, the copolymer having a mass ratio (styrene monomer units: acrylic monomer units) of 62:38, a glass transition temperature of 52°C, and a volume average particle size of 0.5 μm] and polyvinylidene fluoride (PVDF) resin particles [melting point of 140°C, volume average particle size of 0.25 μm] dispersed in water at a mixing mass ratio of 70:30.

[0438] (Example 7)

[0439] A diaphragm was produced in the same manner as in Example 1, except that the adhesive layer-forming resin particle dispersion was changed to an adhesive layer-forming resin particle dispersion (solid content concentration: 7% by mass) containing adhesive resin particles (A) of a phenyl-containing acrylic resin [resin particles of a copolymer containing acrylic monomer units and styrene monomer units, the copolymer having a mass ratio (styrene monomer units: acrylic monomer units) of 62:38, a glass transition temperature of 52°C, and a volume average particle size of 0.5 μm] and polyvinylidene fluoride (PVDF) resin particles [melting point of 140°C, volume average particle size of 0.25 μm] dispersed in water at a mixing mass ratio of 30:70.

[0440] (Example 8)

[0441] A diaphragm was produced in the same manner as in Example 1, except that the adhesive layer-forming resin particle dispersion was changed to an adhesive layer-forming resin particle dispersion (solid content concentration: 7% by mass) containing adhesive resin particles (A) of a phenyl-containing acrylic resin [resin particles of a copolymer containing acrylic monomer units and styrene monomer units, the copolymer having a mass ratio (styrene monomer units: acrylic monomer units) of 62:38, a glass transition temperature of 52°C, and a volume average particle size of 0.5 μm] and polyvinylidene fluoride (PVDF) resin particles [melting point of 140°C, volume average particle size of 0.25 μm] dispersed in water at a mixing mass ratio of 10:90.

[0442] (Example 9)

[0443] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid obtained by stirring and mixing meta-aramid [poly(m-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and barium sulfate particles [average primary particle size 0.01 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a meta-aramid concentration of 5 mass%.

[0444] (Example 10)

[0445] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid obtained by stirring and mixing meta-aramid [poly(m-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and barium sulfate particles [average primary particle size 0.3 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a meta-aramid concentration of 5 mass%.

[0446] (Example 11)

[0447] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid for forming a heat-resistant porous layer obtained by stirring and mixing meta-aramid [poly(meta-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and barium sulfate particles [average primary particle size 0.45 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a meta-aramid concentration of 5 mass%.

[0448] (Example 12)

[0449] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid obtained by stirring and mixing meta-aramid [poly(m-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and barium sulfate particles [average primary particle size 0.7 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a meta-aramid concentration of 5 mass%.

[0450] (Example 13)

[0451] In addition to changing the mass per unit area of ​​the heat-resistant porous layers formed on both sides of the polyethylene microporous membrane to 3.0 g / m 2 A separator was produced in the same manner as in Example 1 except that the thickness was 2.0 μm (total of both surfaces) and the thickness was 2.0 μm (total of both surfaces).

[0452] (Example 14)

[0453] In addition to changing the mass per unit area of ​​the heat-resistant porous layers formed on both sides of the polyethylene microporous membrane to 2.4 g / m 2 A separator was produced in the same manner as in Example 1 except that the thickness was 1.5 μm (total of both surfaces) and the thickness was 1.5 μm (total of both surfaces).

[0454] (Example 15)

[0455] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid for forming a heat-resistant porous layer obtained by stirring and mixing polyamide-imide [Tor lon (registered trademark) 4000TF, manufactured by Solvay; aromatic resin] and barium sulfate particles [average primary particle size 0.05 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a polyamide-imide concentration of 8 mass %.

[0456] (Example 16)

[0457] A diaphragm was prepared in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid for forming a heat-resistant porous layer obtained by stirring and mixing polyimide [Q-VR-X1444, PI Technology Laboratory Co., Ltd.; aromatic resin] and barium sulfate particles [average primary particle size 0.05 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a polyimide concentration of 6 mass %.

[0458] (Example 17)

[0459] In addition to changing the weight per unit area of ​​the adhesive layers formed on both sides of the polyethylene microporous membrane to 1.0 g / m 2 A separator was produced in the same manner as in Example 1 except that the thickness of the membrane was 0.14 mm (total of both surfaces).

[0460] (Example 18)

[0461] In addition to changing the weight per unit area of ​​the adhesive layers formed on both sides of the polyethylene microporous membrane to 0.3 g / m 2 A separator was produced in the same manner as in Example 1 except that the thickness of the membrane was 0.14 mm (total of both surfaces).

[0462] (Comparative Example 1)

[0463] A diaphragm was produced in the same manner as in Example 1 except that the adhesive layer-forming resin particle dispersion was changed to an adhesive layer-forming resin particle dispersion (solid content concentration: 7% by mass) in which phenyl-free acrylic resin particles (glass transition temperature: 56°C, volume average particle size: 0.5 μm) were dispersed in water.

[0464] (Comparative Example 2)

[0465] A diaphragm was produced in the same manner as in Example 1, except that the adhesive layer-forming resin particle dispersion was changed to an adhesive layer-forming resin particle dispersion (solid content concentration: 7% by mass) in which polyvinylidene fluoride (PVDF)-based resin particles (melting point 140°C, volume average particle size 0.25 μm) were dispersed in water.

[0466] (Comparative Example 3)

[0467] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid for forming a heat-resistant porous layer obtained by stirring and mixing meta-aramid [poly(meta-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and magnesium hydroxide particles [average primary particle size 0.3 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a meta-aramid concentration of 5 mass%.

[0468] (Comparative Example 4)

[0469] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid for forming a heat-resistant porous layer obtained by stirring and mixing meta-aramid [poly(meta-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and magnesium hydroxide particles [average primary particle size 0.8 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a meta-aramid concentration of 5 mass%.

[0470] (Comparative Example 5)

[0471] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid obtained by stirring and mixing meta-aramid [poly(meta-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and alumina particles [average primary particle size 0.01 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a meta-aramid concentration of 5 mass%.

[0472] (Comparative Example 6)

[0473] A diaphragm was produced in the same manner as in Example 1, except that the coating liquid for forming a heat-resistant porous layer was changed to a coating liquid obtained by stirring and mixing meta-aramid [poly(m-phenylene isophthalamide), Conex (registered trademark) manufactured by Teijin Ltd.; aromatic resin] and alumina particles [average primary particle size 0.3 μm; inorganic particles] in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG=90:10 [mass ratio]) in a mass ratio of 20:80 and a meta-aramid concentration of 5 mass%.

[0474] [Table 1]

[0475]

[0476] [Table 2]

[0477]

[0478] [Table 3]

[0479]

[0480] [Table 4]

[0481]

[0482] As shown in Tables 3 and 4, the separators of Examples were excellent in adhesion to electrodes in both dry hot pressing and wet hot pressing. In addition, the separators of Examples generated less gas.

[0483] The entire disclosure of Japanese patent application No. 2022-075457 filed on April 28, 2022 is incorporated into this specification by reference.

[0484] All documents, patent applications, and technical standards described in this specification are incorporated into this specification by reference to the same extent as if each document, patent application, and technical standard was specifically and individually described.

Claims

1. A separator for a non-aqueous secondary battery, comprising: a heat-resistant porous layer comprising an aromatic resin and inorganic particles; and an adhesive layer provided on the heat-resistant porous layer and containing adhesive resin particles comprising a phenyl-containing acrylic resin, wherein the adhesive resin particles comprising a phenyl-containing acrylic resin are attached to the heat-resistant porous layer, The inorganic particles include barium sulfate particles.

2. The non-aqueous secondary battery separator according to claim 1, wherein The adhesive resin particles comprising a phenyl group-containing acrylic resin are at least one selected from the group consisting of (i) resin particles that are a copolymer comprising an acrylic monomer unit and a styrene monomer unit, and (ii) resin particles that are a mixture of an acrylic resin and a styrene resin.

3. The non-aqueous secondary battery separator according to claim 1, wherein The adhesion amount of the adhesive resin particles containing the phenyl group-containing acrylic resin on the heat-resistant porous layer was 0.1 g / m 2 ~5.0g / m 2 .

4. The non-aqueous secondary battery separator according to claim 1, wherein The peak area S1 of the phenyl group of the adhesive layer obtained by Fourier transform infrared spectroscopy is 0.01 to 3, and the peak area S2 of the carbonyl group is 4 or less.

5. The non-aqueous secondary battery separator according to claim 1, wherein The aromatic resin includes at least one selected from the group consisting of wholly aromatic polyamides, polyamide-imides, and polyimides.

6. The non-aqueous secondary battery separator according to claim 1, wherein The average primary particle size of the inorganic particles is 0.01 μm or more and 1 μm or less. 7 . The nonaqueous secondary battery separator according to claim 1 , further comprising a porous substrate, wherein the heat-resistant porous layer is provided on one or both surfaces of the porous substrate.

8. A non-aqueous secondary battery comprising a positive electrode, a negative electrode, and the non-aqueous secondary battery separator according to any one of claims 1 to 7 disposed between the positive electrode and the negative electrode, wherein the non-aqueous secondary battery obtains an electromotive force by doping and dedoping lithium.