Heavy metal adsorbent material as well as preparation method and application thereof

The copper smelting slag-biocarbon adsorbent prepared through impregnation method and pyrolysis treatment solves the problems of resource utilization of copper smelting slag and heavy metal removal, and achieves efficient and low-cost heavy metal adsorption effect, reducing production costs and reducing Environmental pollution.

CN119075913APending Publication Date: 2024-12-06KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411363745.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to effectively utilize copper smelting slag and efficiently remove heavy metal ions in industrial wastewater, and biochar modified materials are costly to produce and difficult to separate and recover.

Method used

The copper smelting slag powder and biomass material powder were mixed in a sodium carbonate solution by impregnation method, and the copper smelting slag-biocarbon heavy metal adsorbent material was prepared by pyrolysis treatment, which was used to efficiently adsorb copper and nickel ions in wastewater.

Benefits of technology

The method of removing heavy metal ions in industrial wastewater is realized at low cost and efficiently, reducing production costs, and reducing environmental pollution through resource utilization of copper smelting slag, and the adsorption effect reaches a 100% removal rate in high-concentration heavy metal ion solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075913A_ABST
    Figure CN119075913A_ABST
Patent Text Reader

Abstract

The invention provides a heavy metal adsorbent material as well as a preparation method and application thereof, and belongs to the technical field of resource recycling, the preparation method comprises the following steps: adding biomass material powder into turbid liquid containing copper smelting slag powder by adopting an impregnation method, uniformly shaking, filtering and drying, and then carrying out pyrolysis treatment to obtain the heavy metal adsorbent material. The heavy metal adsorbent material is prepared; wherein the turbid liquid is prepared by adding copper smelting slag powder into a sodium carbonate solution and uniformly shaking. The heavy metal adsorption material prepared by the method has the advantages of large adsorption capacity and capability of quickly and efficiently removing copper and nickel ions in wastewater. In addition, the preparation method is simple and easy to implement, low in preparation cost and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resource recycling, and in particular relates to a heavy metal adsorbent material and a preparation method and application thereof. Background Art

[0002] With the development of industry, heavy metals in industrial wastewater have attracted wide attention due to their strong toxicity, difficulty in degradation and great environmental threat. At present, the main methods for removing heavy metals from wastewater are precipitation, electrochemical treatment, ion exchange, membrane separation and adsorption. Among them, adsorption has the advantages of no secondary pollution and renewable recycling, and is currently the most selected method for heavy metal treatment in wastewater.

[0003] Since biochar has low production cost and rich porous structure, it has strong adsorption capacity for heavy metals, so biochar has become the focus of heavy metal adsorption material research. However, the adsorption effect of single biochar is limited and it is not easy to separate and recycle. Therefore, many studies choose to modify biochar materials, such as magnetic modification. While improving its adsorption capacity, the material has magnetic separation ability, which overcomes the disadvantage of ordinary biochar that is difficult to separate. However, adding magnetic substances such as red mud will increase production costs. Therefore, suitable magnetic solid waste should be found to reduce the production cost of magnetic biochar.

[0004] While industrial production generates huge economic benefits, it also produces some solid wastes with high heavy metal content, such as copper smelting slag. At present, copper smelting slag is mostly stored in the open air, and the heavy metals leached out by rainfall will pollute the water environment with rainwater. At the same time, it is noted that copper smelting slag has a high iron content and rich functional groups, but a green and efficient resource utilization method has not yet been found. Therefore, the rational disposal of copper smelting slag has become an urgent issue for the clean production and high-value utilization of industrial solid waste. Summary of the invention

[0005] In view of the above technical problems, the present invention proposes a heavy metal adsorbent material and its preparation method and application, which can realize resource utilization of copper smelting slag on the one hand, and prepare an adsorbent material with high efficiency in adsorbing heavy metal ions on the other hand.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a heavy metal adsorbent material comprises the following steps:

[0008] The heavy metal adsorbent material is prepared by adding the biomass material powder into a suspension containing copper smelting slag powder by an impregnation method, mixing, filtering and drying, and then performing a pyrolysis treatment;

[0009] The suspension is prepared by adding copper smelting slag powder into sodium carbonate solution and mixing them evenly.

[0010] Preferably, the mass ratio of the biomass material powder, copper smelting slag powder and sodium carbonate is 3:0.7:(0.7-1).

[0011] Beneficial effect: Within the range of the dosage ratio defined in the present invention, the heavy metal leaching rate in copper smelting slag can be effectively reduced, so that it meets the hazardous waste leaching standard and can be better used as a raw material for adsorption effect.

[0012] Preferably, the concentration of the sodium carbonate solution is 14 g / L.

[0013] Preferably, the copper smelting slag powder needs to pass through a 200-mesh nylon sieve.

[0014] Beneficial effects: The present invention controls the particle size of copper smelting slag powder to make it easier to load on the surface of biochar and provide a larger specific surface area.

[0015] Preferably, the biomass material comprises Oriole leaves and / or Eustoma leaves.

[0016] Preferably, the biomass material powder needs to be dried at 65° C. to constant weight and then passed through a 20-60 mesh nylon sieve.

[0017] Beneficial effect: The present invention is dried to constant weight at 65°C, which is lower than the pyrolysis temperature of biochar. Controlling moisture before pyrolysis can prevent side reactions of water in the subsequent pyrolysis process, which affects the heavy metal adsorption performance of the adsorption material.

[0018] Preferably, when preparing the heavy metal adsorption material, the mixture is mixed by shaking; the shaking frequency during the shaking process is 250 rpm, and the shaking is performed for 12 hours;

[0019] When preparing the suspension, the suspension was mixed by shaking at a frequency of 250 rpm for 2 h.

[0020] Preferably, the temperature during the drying process is 65° C., and the drying is performed to a constant weight.

[0021] Preferably, the parameter conditions during the pyrolysis treatment are:

[0022] In an argon atmosphere, the temperature is increased to 500-800°C at a heating rate of 5°C / min and kept for 1-2h; more preferably, the temperature is increased to 500°C, 600°C, 700°C and 800°C; further preferably, 700°C.

[0023] Beneficial effects: At a pyrolysis temperature of 700°C, zero-valent iron is generated, which greatly improves the adsorption capacity of the material.

[0024] Preferably, the gas flow rate of the argon gas is 200 mL / min.

[0025] The second technical solution of the present invention:

[0026] The heavy metal adsorbent material (heavy metal adsorbent) prepared by the above preparation method.

[0027] The third technical solution of the present invention:

[0028] The application of the heavy metal adsorbent material in the adsorption and removal of heavy metal ions in industrial wastewater.

[0029] Preferably, the heavy metal ion is Cu 2+ and / or Ni 2+ .

[0030] Preferably, the adsorption time in the process of removing heavy metal ions from industrial wastewater is 5-480 min;

[0031] The initial heavy metal ion concentration in the industrial wastewater is 10-500 mg / L.

[0032] Compared with the prior art, the present invention has the following advantages and technical effects:

[0033] (1) The present invention uses biomass material as raw material, and adopts an impregnation method to disperse copper smelting slag on the surface of the biomass material, and then pyrolysis is used to simultaneously carry out biomass carbonization and copper smelting slag loading, and finally obtains a copper smelting slag-biochar heavy metal adsorbent material; the adsorbent material prepared by this method can quickly and efficiently remove copper and nickel ions in wastewater, and has a large adsorption capacity;

[0034] (2) The preparation method of the present invention is simple and easy to implement, and the preparation cost is low, which is suitable for industrial production. In addition, the present invention uses waste copper smelting slag as raw material, which, on the one hand, turns waste into treasure and reduces production costs; on the other hand, using copper smelting slag as raw material reduces environmental pollution. Therefore, the present invention uses copper smelting slag and biochar to prepare heavy metal adsorbent materials, which provides a new idea for the resource utilization of copper smelting slag.

[0035] (3) Compared with the existing patent (CN 111715178 A), the present invention can synthesize effective adsorption materials with low energy consumption (less than 1000°C) and in a short process, and the synthesized adsorption materials also have good adsorption effects in high-concentration heavy metal ion solutions (200 mg / L) (especially the heavy metal ion removal rate of Example 1 is close to 100%), indicating that it has a huge adsorption capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0037] Figure 1 These are the SEM and BET characterization images of the heavy metal adsorbent (before adsorption) prepared in Example 1 of the present invention, wherein a is a BET characterization image and b is a SEM image;

[0038] Figure 2 The heavy metal adsorbent prepared in Example 1 of the present invention is used to adsorb Cu 2+ and Ni 2+ XRD characterization diagram before and after;

[0039] Figure 3 This is the EDS elemental analysis diagram of the heavy metal adsorbent prepared in Example 1 of the present invention;

[0040] Figure 4 The heavy metal adsorbent prepared in Example 1 of the present invention adsorbs Cu 2+ EDS element analysis diagram after

[0041] Figure 5 The heavy metal adsorbent prepared in Example 1 of the present invention adsorbs Ni 2+ EDS elemental analysis diagram. DETAILED DESCRIPTION

[0042] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0043] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0044] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0045] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0046] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0047] A method for preparing a heavy metal adsorbent material using copper smelting slag and biochar comprises the following steps:

[0048] (1) The copper smelting slag is pretreated to be powdered and passed through a 200-mesh nylon sieve. The main components of the copper smelting slag are shown in Table 1:

[0049] Table 1

[0050] Element <![CDATA[Fe 2 THE 3 ]]> <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> CuO CaO Content (wt.%) 54.7 27.5 5.0 2.7 1.8

[0051] (2) pre-treating the biomass material into powder, and passing the powder through a 20-60 mesh nylon sieve to obtain a pre-treated biomass material;

[0052] (3) adding the copper smelting slag powder obtained in (1) into the sodium carbonate solution and shaking well to obtain a suspension;

[0053] (4) adding the pretreated biomass material obtained in (2) to the suspension obtained in (3), shaking well, filtering and drying to obtain a copper smelting slag-biomass mixed material;

[0054] (5) The copper smelting slag-biomass mixed material obtained in (4) is heated to 500-800° C. in an Ar atmosphere for pyrolysis treatment to obtain a heavy metal adsorbent material.

[0055] In some preferred embodiments, the biomass material is yellow warbler grass leaves.

[0056] In some preferred embodiments, in step (3), the mass ratio of copper smelting slag to sodium carbonate is 0.7:0.7-1, the concentration of sodium carbonate solution is 14 g / L, the shaking frequency is 250 rpm, and the shaking is performed for 2 hours.

[0057] In some preferred embodiments, in step (4), the mass ratio of biomass material, copper smelting slag and sodium carbonate is 3:0.7:0.7-1, the shaking frequency is 250 rpm, the shaking is for 12 hours, and the solid after filtration is dried at 65°C.

[0058] In some preferred embodiments, in step (5), the temperature is increased to 500-800° C. at a heating rate of 5° C. / min, maintained for 1 h, and the Ar gas flow rate is 200 mL / min.

[0059] The "room temperature" in the present invention refers to 20-30°C unless otherwise specified.

[0060] The raw materials used in the present invention are all purchased from the market.

[0061] The technical solution of the present invention is further illustrated by the following embodiments.

[0062] Example 1

[0063] A method for preparing a heavy metal adsorbent material using copper smelting slag and biochar comprises the following steps:

[0064] (1) grinding copper smelting slag at room temperature, passing through a 200-mesh nylon sieve for later use, and obtaining copper smelting slag powder; drying the biomass material (yellow warbler grass leaves) at 65° C., grinding the biomass material and passing through a 20-mesh nylon sieve for later use, and obtaining biomass material powder;

[0065] (2) taking the copper smelting slag powder of step (1), adding the copper smelting slag to a sodium carbonate solution with a concentration of 14 g / mL according to a mass ratio of the copper smelting slag to sodium carbonate of 1:1, and then shaking at a frequency of 250 rpm at room temperature for 2 hours to obtain a suspension;

[0066] (3) After the shaking in step (2) is completed, the biomass material powder is added to the suspension obtained in step (2) at a mass ratio of biomass material powder to copper smelting slag powder of 3:0.7, and the suspension is continuously shaken at a frequency of 250 rpm at room temperature for 12 hours to obtain a suspension of copper smelting slag-biomass mixed material, and the filtered mixed material solid is dried at 65° C. to obtain copper smelting slag-biomass mixed material particles;

[0067] (4) The copper smelting slag-biomass mixed material particles obtained in step (3) are placed in a tubular furnace and heated to 700°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a copper smelting slag-biochar heavy metal adsorbent.

[0068] Example 2

[0069] The difference from Example 1 is that:

[0070] (4) The copper smelting slag-biomass mixed material particles obtained in step (3) are placed in a tubular furnace and heated to 600°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a copper smelting slag-biochar heavy metal adsorbent.

[0071] Example 3

[0072] The difference from Example 1 is that:

[0073] (4) The copper smelting slag-biomass mixed material particles obtained in step (3) are placed in a tubular furnace and heated to 500°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a copper smelting slag-biochar heavy metal adsorbent.

[0074] Example 4

[0075] The difference from Example 1 is that:

[0076] The mass ratio of biomass material powder, copper smelting slag powder and sodium carbonate is 3:0.7:1.

[0077] Example 5

[0078] The difference from Example 1 is that:

[0079] (4) The copper smelting slag-biomass mixed material particles obtained in step (3) are placed in a tubular furnace and heated to 700°C at a heating rate of 5°C / min, and kept warm for 2 hours. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a copper smelting slag-biochar heavy metal adsorbent.

[0080] Example 6

[0081] The difference from Example 1 is that

[0082] In step (1), the biomass material is Eustoma grandiflorum leaves.

[0083] Example 7

[0084] The difference from Example 1 is that

[0085] The temperature during the pyrolysis treatment in step (4) is 800°C.

[0086] Comparative Example 1

[0087] The difference from Example 1 is that:

[0088] (2) Take the copper smelting slag powder of step (1), add the copper smelting slag into deionized water at a liquid-to-solid ratio of 50:0.7 (mL / g, the same below), and then shake at a frequency of 250 rpm at room temperature for 2 hours to obtain a suspension.

[0089] Comparative Example 2

[0090] The difference from Example 2 is that:

[0091] (2) Take the copper smelting slag powder of step (1), add the copper smelting slag into deionized water at a liquid-to-solid ratio of 50:0.7, and then shake at a frequency of 250 rpm for 2 hours at room temperature to obtain a suspension.

[0092] Comparative Example 3

[0093] The difference from Example 3 is that:

[0094] (2) Take the copper smelting slag powder of step (1), add the copper smelting slag into deionized water at a liquid-to-solid ratio of 50:0.7, and then shake at a frequency of 250 rpm for 2 hours at room temperature to obtain a suspension.

[0095] Comparative Example 4

[0096] The difference from Example 1 is that:

[0097] (2) Take the copper smelting slag powder of step (1), add the copper smelting slag into deionized water at a liquid-to-solid ratio of 50:0.7, and then shake at a frequency of 250 rpm for 2 hours at room temperature to obtain a suspension.

[0098] (4) The copper smelting slag-biomass mixed material particles obtained in step (3) are placed in a tubular furnace and heated to 400°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a copper smelting slag-biochar heavy metal adsorbent.

[0099] Comparative Example 5

[0100] (1) drying the biomass material (leaves of yellow warbler grass) at 65° C., grinding the biomass material and passing it through a 20-mesh nylon sieve for later use, and obtaining a biomass material powder;

[0101] (2) The biomass material powder obtained in step (1) is placed in a tubular furnace and heated to 700°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a biochar heavy metal adsorbent.

[0102] Comparative Example 6

[0103] (1) drying the biomass material (leaves of yellow warbler grass) at 65° C., grinding the biomass material and passing it through a 20-mesh nylon sieve for later use, and obtaining a biomass material powder;

[0104] (2) The biomass material powder obtained in step (1) is placed in a tubular furnace and heated to 600°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a biochar heavy metal adsorbent.

[0105] Comparative Example 7

[0106] (1) drying the biomass material (leaves of yellow warbler grass) at 65° C., grinding the biomass material and passing it through a 20-mesh nylon sieve for later use, and obtaining a biomass material powder;

[0107] (2) The biomass material powder obtained in step (1) is placed in a tubular furnace and heated to 500°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a biochar heavy metal adsorbent.

[0108] Comparative Example 8

[0109] (1) drying the biomass material (leaves of yellow warbler grass) at 65° C., grinding the biomass material and passing it through a 20-mesh nylon sieve for later use, and obtaining a biomass material powder;

[0110] (2) The biomass material powder obtained in step (1) is placed in a tubular furnace and heated to 400°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a biochar heavy metal adsorbent.

[0111] Comparative Example 9

[0112] The difference from Example 1 is that the mass ratio of biomass material powder, copper smelting slag powder and sodium carbonate is 3:1:0.7.

[0113] Comparative Example 10

[0114] The difference from Example 1 is that the mass ratio of biomass material powder, copper smelting slag powder and sodium carbonate is 3.5:0.7:0.7.

[0115] Comparative Example 11

[0116] The difference from Example 1 is that:

[0117] (4) The copper smelting slag-biomass mixed material particles obtained in step (3) are placed in a tubular furnace and heated to 400°C at a heating rate of 5°C / min, and kept warm for 1 hour. The sintering atmosphere is Ar gas, and the Ar gas flow rate is 200 mL / min to obtain a copper smelting slag-biochar heavy metal adsorbent.

[0118] Effect verification example 1

[0119] The heavy metal adsorbents prepared in Examples 1-7 and Comparative Examples 1-11 were subjected to a copper and nickel polluted wastewater treatment test, and the specific steps are as follows:

[0120] The prepared heavy metal adsorbents were added to 200 mg / L heavy metal solution (specifically, Cu(NO 3 ) 2 ·3H 2 O and NiCl 2 6H 2 O were used as copper source and nickel source respectively to prepare 200 mg / L Cu 2+ and Ni 2+ The heavy metal solutions were used for subsequent adsorption experiments; 1 M NaOH and 1 M HNO 3 Adjust the pH value of heavy metal solution, where Cu 2+ The pH of the heavy metal solution is 3, Ni 2+ The pH of the heavy metal solution was 4), and the mixture was shaken in a constant temperature shaking box, and adsorption was performed for 6 hours at room temperature. After the adsorption was completed, a 0.45 μm water filter membrane was used to separate the solid adsorbent and the adsorption liquid, and an atomic absorption spectrometer was used to detect the remaining heavy metal ion concentration in the adsorption liquid. The adsorption amount of the heavy metal adsorbent was calculated according to formula (I), and the heavy metal removal rate was calculated according to formula (II). The results are shown in Table 2.

[0121]

[0122] Where q e is the adsorption capacity of heavy metals by the adsorbent, mg / g; C 0 is the initial concentration of the adsorption solution, mg / L; C e is the concentration of the remaining heavy metals in the solution after adsorption, mg / L; V is the volume of the adsorption solution added (L); m is the mass of the added adsorbent, g; R is the heavy metal removal rate, %.

[0123] Table 2

[0124]

[0125] As can be seen from Table 2, the copper smelting slag-biochar heavy metal adsorbent prepared in the present invention has excellent adsorption performance for copper and nickel heavy metal ions and can be used as a wastewater heavy metal adsorbent.

[0126] Among them, compared with Example 1, Comparative Examples 1-4 did not use sodium carbonate to modify the copper smelting slag and biochar. As a result, the obtained heavy metal adsorbents had poor adsorption effects on copper and nickel. This is because sodium carbonate can increase the specific surface area of ​​biochar, provide more adsorption sites, and the sodium ions compounded into the material can increase the ion exchange capacity, thereby improving the adsorption capacity of the heavy metal adsorbent for heavy metal ions.

[0127] Comparative Examples 5-8 Compared with Example 1, copper smelting slag was not loaded on the surface of biochar. As a result, the heavy metal adsorbent obtained had poor adsorption effect on copper and nickel. This is because the copper smelting slag contains a high content of iron. After heating to 600°C, the substance with low iron content begins to transform into the substance with high iron content (i.e., high-valent iron transforms into low-valent iron), such as ferric oxide is reduced to zero-valent iron, from Figure 2 It can be seen that the heavy metal adsorbent has shown the characteristic peak of zero-valent iron. Zero-valent iron can cause the complexation, oxidation-reduction and surface precipitation of the functional groups on the surface of the material, and the copper smelting slag surface has rich functional groups, which is conducive to improving the adsorption capacity of the adsorbent.

[0128] Compared with Example 1, in Comparative Example 9, the proportion of copper smelting slag is too high, which may cause a large number of adsorption pores to be occupied by copper smelting slag, resulting in poor adsorption effect. Compared with Example 1, in Comparative Example 10, the proportion of biochar is too high, resulting in limited effect of increasing the specific surface area of ​​sodium carbonate, resulting in poor adsorption effect. Compared with Example 1, in Comparative Example 11, when the pyrolysis temperature is 400°C, biochar synthesis is insufficient, and the iron-containing substances in the copper smelting slag are not fully converted into zero-valent iron with strong reducibility, resulting in poor adsorption effect.

[0129] Effect verification example 2

[0130] The heavy metal adsorbents prepared in Example 2, Comparative Example 2 and Comparative Example 6 were subjected to a copper and nickel mixed polluted wastewater treatment test, and the specific steps were as follows:

[0131] The prepared heavy metal adsorbents were added to 200 mg / L heavy metal solution at a solid-liquid ratio of 2 g: 1 L. Specifically, Cu(NO 3 ) 2 ·3H 2 O and NiCl 2 6H 2 O were used as copper source and nickel source, respectively, to prepare 200 mg / LCu 2+ and Ni 2+ The mixed solution of heavy metals (where the concentration of both ions was 200 mg / L) was used for subsequent adsorption experiments; 1 M NaOH and 1 M HNO 3The pH value of the heavy metal mixed solution was adjusted to 5, and it was shaken in a constant temperature shaking box, and adsorption was carried out at room temperature for 6 hours. The test method was consistent with the effect verification example 1. The test results are shown in Table 3:

[0132] Table 3

[0133]

[0134] Effect Example 2 Compared with Effect Example 1, Cu 2+ The adsorption effect of Ni 2+ The adsorption effect of Cu 2+ Occupies most adsorption sites, the material preferentially adsorbs Cu 2+ .

[0135] Figure 1 The SEM and BET characterization images of the heavy metal adsorbent (before adsorption) prepared in Example 1 of the present invention, wherein a is a BET characterization image and b is a SEM image. Figure 1 It can be seen that the surface of the heavy metal adsorbent is loaded with copper smelting slag (rough surface) and a large number of pores are distributed inside it, with a specific surface area of ​​up to 186m 2 / g, which can effectively adsorb heavy metals.

[0136] Figure 2 The heavy metal adsorbent prepared in Example 1 of the present invention is used to adsorb Cu 2+ and Ni 2+ XRD characterization diagram before and after Figure 2 It can be seen that the adsorption of Cu 2+ The adsorbent after CuCl appeared at around 25° 2 The characteristic peak of Ni 2+ The adsorbent after that showed Ni(OH) at around 39° 2 The characteristic peaks of Cu 2+ and Ni 2+ Successfully adsorbed by heavy metal adsorbent.

[0137] Figure 3 This is the EDS elemental analysis diagram of the heavy metal adsorbent prepared in Example 1 of the present invention;

[0138] Figure 4 The heavy metal adsorbent prepared in Example 1 of the present invention adsorbs Cu 2+ EDS element analysis diagram after

[0139] Figure 5 The heavy metal adsorbent prepared in Example 1 of the present invention adsorbs Ni 2+ EDS element analysis diagram after Figure 3-5It can be seen that before the adsorption of heavy metals, there is almost no Cu and Ni in the heavy metal adsorbent ( Figure 3 ), while in the adsorption of Cu 2+ After that, Cu 2+ The content has increased significantly ( Figure 4 ), heavy metal adsorbent adsorbs Ni 2+ After that, 2+ The content was significantly increased ( Figure 5 ), indicating that Cu 2+ and Ni 2+ Successfully adsorbed by heavy metal adsorbent.

[0140] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a heavy metal adsorbent material, characterized in that: The following steps are involved: The biomass material powder is added into the suspension containing the copper smelting slag powder by an impregnation method, mixed, filtered and dried, and then pyrolyzed to prepare the heavy metal adsorbent material; The suspension is obtained by adding copper smelting slag powder into sodium carbonate solution and mixing them evenly.

2. The method for preparing a heavy metal adsorbent material according to claim 1, characterized in that: The mass ratio of the biomass material powder, copper smelting slag powder and sodium carbonate is 3:0.7:0.7-1.

3. The method for preparing a heavy metal adsorbent material according to claim 1, characterized in that: The concentration of the sodium carbonate solution is 14 g / L.

4. The method for preparing a heavy metal adsorbent material according to claim 1, characterized in that: The biomass material includes leaves of Eustoma grandiflorum and / or leaves of Eustoma grandiflorum.

5. The method for preparing a heavy metal adsorbent material according to claim 1, characterized in that: The mixing process was performed by shaking; the shaking frequency during the shaking process was 250 rpm.

6. The method for preparing a heavy metal adsorbent material according to claim 1, characterized in that: The temperature during the drying process is 65°C.

7. The method for preparing a heavy metal adsorbent material according to claim 1, characterized in that: The parameter conditions during the pyrolysis treatment are: In an argon atmosphere, heat to 500-800°C at a heating rate of 5°C / min and keep warm for 1-2h.

8. A heavy metal adsorbent material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 7.

9. Use of the heavy metal adsorbent material as claimed in claim 8 in the adsorption and removal of heavy metal ions in industrial wastewater.

10. The use according to claim 9, characterized in that: The heavy metal ion is Cu 2+ and / or Ni 2+ .