Asymmetric modified rapeseed globulin-based aerogel as well as preparation method and application thereof
Through the preparation of asymmetrically modified rapeseed globulin-based aerogel, the problem of insufficient selectivity and capacity of heavy metal adsorbents is solved, efficient adsorption and mechanical performance are improved, and it is green and sustainable.
Patent Information
- Application Number
- CN202411064003.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, heavy metal removal selectivity is low, adsorption capacity is limited, and it is easy to cause secondary pollution.
The preparation method of asymmetrically modified rapeseed globulin-based aerogel is adopted to form a bicontinuous phase emulsion by dispersing rapeseed globulin solution, toluene and water, and the gel is obtained by centrifugation and cross-linking, and then prepared by freeze-drying. Aerogels with rich pore structure and high adsorption sites were produced.
It realizes efficient heavy metal adsorption, has excellent mechanical properties and biosafety, and is low in cost and green and sustainable production, solving the problems of selectivity, capacity and capacity of heavy metal adsorbents in the prior art and secondary pollution.
Smart Images

Figure CN119075926A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heavy metal adsorption, and in particular to an asymmetric modified rapeseed globulin-based aerogel and a preparation method and application thereof. Background Art
[0002] In the prior art, adsorbents play an important role in the food purification process, such as the removal of heavy metals from edible materials such as food dyes, drinking water, and heavy metal-contaminated grains. Although traditional adsorbents, such as activated carbon and clay minerals, are widely used in the food industry, they have the disadvantages of low selectivity, limited adsorption capacity, and easy to cause secondary pollution. Therefore, it is of great significance to develop natural biomacromolecule aerogels with high adsorption efficiency and green and sustainable production.
[0003] In recent years, aerogels have been widely used in the field of heavy metal adsorption as a new type of nanoporous material. Natural macromolecules are considered to be excellent raw materials for aerogel production due to their excellent environmental friendliness. At present, aerogels prepared based on natural macromolecules often have problems such as irregular pore structure, insufficient connectivity, and fragile overall structure. It is imperative to develop a natural macromolecular aerogel with superior performance. Summary of the invention
[0004] The purpose of the present invention is to provide an asymmetric modified rapeseed globulin-based aerogel and a preparation method and application thereof, so as to solve the technical problems in the prior art of low heavy metal removal selectivity, limited adsorption capacity and easy secondary pollution.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing an asymmetric modified rapeseed protein-based aerogel, comprising the following steps:
[0007] 1) using an asymmetric modified rapeseed globulin solution as an emulsifier, and toluene and water as two continuous phases, to obtain a stable bicontinuous phase emulsion after dispersion;
[0008] 2) after centrifuging the bicontinuous phase emulsion of step 1), cross-linking the upper layer of the emulsion with a glutaraldehyde solution to obtain a gel;
[0009] 3) freeze-drying the gel obtained in step 2) to obtain an asymmetric modified rapeseed protein-based aerogel.
[0010] Furthermore, in step 1), the volume ratio of toluene to water is 1:1-4.
[0011] Furthermore, in step 1), the concentration of the asymmetrically modified rapeseed globulin solution is 7-10 mg / mL.
[0012] Furthermore, in step 1), the dispersion speed is 10000-18000 rpm, and the dispersion time is 1-3 min.
[0013] Furthermore, in step 2), the temperature of the centrifugal treatment is 2 to 5° C., the speed of the centrifugal treatment is 1000 to 3000 r / min, and the time of the centrifugal treatment is 5 to 15 min.
[0014] Furthermore, in step 2), the cross-linking time is 6 to 14 hours.
[0015] Furthermore, in step 2), the concentration of the glutaraldehyde solution is 1.5-2 g / mL.
[0016] Furthermore, in step 3), the freeze-drying temperature is -60 to 80°C, and the freeze-drying time is 40 to 60 hours.
[0017] The invention provides an asymmetric modified rapeseed globulin-based aerogel.
[0018] The present invention also provides an application of an asymmetric modified rapeseed globulin-based aerogel as an adsorbent in heavy metal adsorption.
[0019] Beneficial effects of the present invention:
[0020] The present invention successfully prepares a bicontinuous phase emulsion for the first time using asymmetric modified rapeseed globulin with a contact angle of 90° and obtains a bicontinuous phase emulsion aerogel by combining freeze-drying technology. The aerogel prepared from the protein has rich pore structure and heavy metal adsorption sites, good biosafety, and excellent green and sustainable applicability.
[0021] The asymmetric modified rapeseed globulin-based aerogel obtained by the present invention has excellent mechanical properties as a heavy metal adsorbent and has extremely high adsorption capacity in a short time.
[0022] In the dual continuous phase structure used in the present invention, the high specific surface area and interconnected pore structure of the continuous phase endow the aerogel with more sufficient adsorption active sites and higher mechanical strength. At the same time, the freeze-drying method can well retain its pore structure and adsorption active sites, so that the produced aerogel has good mechanical properties and adsorption efficiency. The method of the present invention not only improves the adsorption efficiency of plant protein-based aerogels, but also has the characteristics of low cost and green sustainable production. Therefore, the present invention has broad application prospects in the field of heavy metal adsorption. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1SEM images of bicontinuous emulsion aerogels prepared with different oil ratios, where a is 20%, b is 30%, c is 40%, and d is 50%;
[0024] Figure 2 SEM images of bicontinuous emulsion aerogels prepared at different protein concentrations, where a is 7 mg / mL, b is 8 mg / mL, c is 9 mg / mL, and d is 10 mg / mL;
[0025] Figure 3 The N2 adsorption-desorption curves and pore size distribution diagrams of bicontinuous emulsion aerogels prepared with different oil ratios and different protein concentrations, wherein a is the N2 adsorption-desorption curves with different oil ratios, b is the pore size distribution curves with different oil ratios, c is the N2 adsorption-desorption curves with different protein concentrations, and d is the pore size distribution curves with different protein concentrations;
[0026] Figure 4 SEM images of emulsion aerogels in different phases, where a is an oil-in-water (O / W) emulsion aerogel, b is a dual-continuous phase emulsion aerogel, and c is a water-in-oil (W / O) emulsion aerogel;
[0027] Figure 5 The N2 adsorption-desorption curves and pressure curves of different phase emulsion aerogels, wherein i) is the N2 adsorption-desorption curve, and ii) is the pressure curve;
[0028] Figure 6 It is the adsorption capacity diagram of different protein concentrations and different oil ratios in heavy metal solutions with different pH values, where a is the adsorption capacity diagram of aerogels at different protein concentrations and pH values, and b is the adsorption capacity diagram of aerogels at different oil ratios and pH values;
[0029] Figure 7 This is the adsorption effect diagram of gel with different contents on Cd(Ⅱ);
[0030] Figure 8 This is a diagram showing the multiple cycle adsorption effect of the aerogel prepared when the protein concentration is 9 mg / mL and the oil phase ratio is 40% on Cd(Ⅱ);
[0031] Fig. 9 This is a graph showing the adsorption effect of the aerogel prepared when the protein concentration is 9 mg / mL and the oil phase ratio is 40% on different heavy metals. DETAILED DESCRIPTION
[0032] The present invention provides a method for preparing an asymmetric modified rapeseed protein-based aerogel, comprising the following steps:
[0033] 1) using an asymmetric modified rapeseed globulin solution as an emulsifier, and toluene and water as two continuous phases, to obtain a stable bicontinuous phase emulsion after dispersion;
[0034] 2) after centrifuging the bicontinuous phase emulsion of step 1), cross-linking the upper layer of the emulsion with a glutaraldehyde solution to obtain a gel;
[0035] 3) freeze-drying the gel obtained in step 2) to obtain an asymmetric modified rapeseed protein-based aerogel.
[0036] In the present invention, the asymmetrically modified rapeseed globulin solution is prepared from rapeseed globulin.
[0037] In the present invention, in step 1), the volume ratio of toluene to water is 1:1 to 4, preferably 1:3.
[0038] In the present invention, in step 1), the concentration of the asymmetrically modified rapeseed globulin solution is 7-10 mg / mL, preferably 8-9 mg / mL, and more preferably 8.5 mg / mL.
[0039] In the present invention, in step 1), the dispersion speed is 10000-18000 rpm, preferably 12000-16000 rpm, more preferably 14000 rpm, and the dispersion time is 1-3 min, preferably 2 min.
[0040] In the present invention, in step 2), the temperature of the centrifugal treatment is 2-5°C, preferably 3°C, the speed of the centrifugal treatment is 1000-3000r / min, preferably 1500-2500r / min, more preferably 2000r / min, and the time of the centrifugal treatment is 5-15min, preferably 8-12min, more preferably 10min.
[0041] In the present invention, in step 2), the cross-linking time is 6 to 14 hours, preferably 8 to 12 hours, and more preferably 10 hours.
[0042] In the present invention, the crosslinking is static crosslinking.
[0043] In the present invention, in step 2), the concentration of the glutaraldehyde solution is 1.5 to 2 g / mL, preferably 1.7 to 1.9 g / mL, and more preferably 1.8 g / mL.
[0044] In the present invention, the gel is cut into uniform pieces and then freeze-dried.
[0045] In the present invention, in step 3), the freeze-drying temperature is -60 to 80°C, preferably -72°C, and the freeze-drying time is 40 to 60 hours, preferably 45 to 55 hours, and more preferably 48 hours.
[0046] The invention provides an asymmetric modified rapeseed globulin-based aerogel.
[0047] The present invention also provides an application of an asymmetric modified rapeseed globulin-based aerogel as an adsorbent in heavy metal adsorption.
[0048] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0049] Example 1
[0050] 0.3 g rapeseed globulin was fully dissolved in 18 mL of NaCl solution (concentration of 10 mg / mL). Then, 2 mL of molten paraffin and 0.25 mg of Tween-20 (used to adjust the interfacial tension between molten wax and water) were added at 65 °C. The mixture was homogenized at 15000 rpm for 2 min using a high-speed disperser and then quickly cooled to room temperature. The pH of the homogenized mixture was adjusted to 10 with 1 M NaOH solution, and an appropriate amount of succinic anhydride (mass fraction 0.23%, based on protein dosage) was slowly added thereto for acylation reaction. During the reaction, the pH of the mixed solution was always stabilized at 10 with 1 M NaOH solution. After the reaction, the solid paraffin in the solution was removed by centrifugation (4000 rpm, 10 min), the paraffin surface was repeatedly rinsed with 20 mL of deionized water, and then vacuum filtered with a 0.8 μm microporous filter membrane. Finally, small molecules were removed by ultrafiltration, and freeze-dried to obtain asymmetric modified rapeseed globulin with a contact angle of 90°;
[0051] An aqueous solution of asymmetric modified rapeseed globulin with a protein concentration of 9 mg / mL was mixed with toluene to obtain a mixture of 30 mL of oil phase with oil ratios of 20% (i.e., the volume ratio of toluene to water was 2:8), 30%, 40% and 50%, respectively. The mixture was dispersed at a speed of 15000 rpm for 2 min, and the whole system was placed at 4°C and centrifuged at a speed of 2000 r / min for 10 min. The upper emulsion was mixed with a 2 g / mL glutaraldehyde solution and cross-linked at 4°C for 10 h to obtain a gel. The obtained gel was uniformly cut into 1 cm 3 The small pieces were freeze-dried at -72 °C for 48 h to obtain asymmetric modified rapeseed globulin-based aerogels.
[0052] BET Analysis:
[0053] The morphology, mechanical properties, specific surface area and porosity (BET) of the asymmetric modified rapeseed protein-based aerogels prepared with oil-phase ratios of 20%, 30%, 40% and 50% were tested and analyzed. The gel was cut into 1 mm thick slices, fixed on a conductive glue and fully sprayed with gold. The overall morphology of the gel was observed under vacuum using a scanning electron microscope (SEM). 3The aerogel was placed on a food physical property analyzer to measure the stress-strain curve and compression performance of the aerogel, where the probe pressing speed was set to 1mm / s. The aerogel after nitrogen adsorption was fully degassed at 120℃ for 12h, and the pore structure of the sample was analyzed using a fully automatic specific surface area and porosity analyzer. Large specific surface area, high porosity, high adsorption capacity and good mechanical properties are the necessary structural properties of aerogel as a heavy metal adsorbent, so the above method was used to characterize the structural properties of the obtained aerogel.
[0054] Table 1 shows the BET analysis results of the aerogels prepared with different oil ratios.
[0055] Table 1 BET analysis of aerogels with different oil ratios
[0056]
[0057]
[0058] It can be seen from Table 1 that when the oil phase ratio is 40%, the prepared aerogel has the largest specific surface area, pore volume, average pore diameter and the highest porosity.
[0059] Heavy metal adsorption experiment:
[0060] Adsorption of Cd(Ⅱ) by aerogels obtained with different oil ratios: 30 mg of aerogels prepared with different oil ratios were placed in 20 mL of 20 ppm Cd(Ⅱ) solution with different pH gradients (7.2, 7.6, 8, 8.4, 8.8, 9.2), and fully shaken at room temperature for 30 min, and the sample solutions before and after adsorption were retained.
[0061] Adsorption of Cd(Ⅱ) by aerogels with different contents: 5 mg, 10 mg, 15 mg, 20 mg, 25 mg, 30 mg, 35 mg, and 40 mg of aerogel (protein concentration was 9 mg / mL, oil phase ratio was 40%) were added to 70 mL of 30 ppm, pH 8 cadmium chloride solution, and the solution was fully shaken at room temperature for 30 min, and the sample solutions before and after adsorption were retained.
[0062] Aerogel's multiple cycles of adsorption of Cd(Ⅱ): 30 mg of aerogel (protein concentration of 9 mg / mL and oil phase ratio of 40%) was added to 20 mL of cadmium chloride solution with a concentration of 30 ppm and a pH of 8, and the solution was fully shaken at room temperature for 30 minutes, and the sample solution before and after adsorption was retained; the aerogel after adsorption once (protein concentration of 9 mg / mL, oil phase ratio of 40%) was then placed in 40 mL of deionized water solution adjusted to pH 3 by HCl for acid washing for 30 minutes to remove the adsorbed metal ions, and the steps were repeated twice, and then the residual acid on the aerogel was completely washed with deionized water. The above adsorption and desorption experiments were repeated several times, and the sample solution before and after each adsorption was retained.
[0063] Adsorption of Cu and Pb by aerogel: 30 mg of aerogel (protein concentration of 9 mg / mL and oil ratio of 40%) was placed in 70 mL of 50 ppm Cu(Ⅱ) and Pb(Ⅱ) solutions with different pH gradients (4, 5, 6, 7, 8, 9, 10), and the solutions were fully shaken at room temperature for 30 min, and the sample solutions before and after adsorption were retained.
[0064] The heavy metal adsorption effect of the aerogel obtained in Example 1 was evaluated: the heavy metal element content of the sample solution before and after the above-mentioned adsorption was detected by inductively coupled plasma mass spectrometry (ICP-MS), and the helium flow rate was set to 5mL / min for 20min, then the argon valve was opened and the temperature control was enabled, and the plasma gas, auxiliary gas, carrier gas and compensation / dilution gas flow rates were set to 15mL / min, 1mL / min, 1mL / min and 1mL / min respectively, and the peristaltic pump parameter was set to 0.1rps to purge the machine again for 10min. After the purge was completed, the plasma ignition was started, and the analysis mode was entered to select the adsorbed heavy metal element to automatically start the start item tuning to determine the adsorption of heavy metal elements by different aerogel samples.
[0065] Example 2
[0066] Different from Example 1, in this example, 7 mg / mL, 8 mg / mL, 9 mg / mL and 10 mg / mL of asymmetric modified rapeseed globulin aqueous solution were respectively mixed with toluene to obtain 30 mL of a mixture with an oil phase ratio of 40% (i.e., a volume ratio of toluene to water of 4:6), dispersed at a speed of 18000 rpm for 3 min, and then the whole system was placed at 4°C and centrifuged at a speed of 3000 r / min for 15 min, the upper emulsion was mixed with a 2 g / mL glutaraldehyde solution, and cross-linked at 4°C for 14 h to obtain a gel; the obtained gel was evenly cut into 1 cm 3 The small pieces were freeze-dried at -72 °C for 48 h to obtain asymmetric modified rapeseed globulin-based aerogels.
[0067] BET Analysis:
[0068] The morphology, mechanical properties, specific surface area and porosity (BET) of the asymmetric modified rapeseed globulin-based aerogels prepared at protein concentrations of 7 mg / mL, 8 mg / mL, 9 mg / mL and 10 mg / mL were detected and analyzed using the same detection method as in Example 1.
[0069] Table 2 shows the BET analysis results of aerogels prepared at different protein concentrations.
[0070] Table 2 BET analysis of aerogels with different protein concentrations
[0071]
[0072] It can be seen from Table 2 that when the protein concentration is 9 mg / mL, the pore capacity of the prepared aerogel is relatively larger.
[0073] Heavy metal adsorption experiment:
[0074] 30 mg of aerogels prepared with different protein concentrations were placed in 20 mL of 20 ppm Cd(II) solution with different pH gradients (7.2, 7.6, 8, 8.4, 8.8, 9.2), and fully shaken at room temperature for 30 min, and the sample solutions before and after adsorption were retained.
[0075] The heavy metal adsorption effect evaluation method is the same as that in Example 1.
[0076] Comparative Example 1
[0077] Different from Example 1, in this comparative example, 2 mg / mL of asymmetric modified rapeseed globulin solution was mixed with toluene to obtain 30 mL of a mixture with an oil phase ratio of 40% (i.e., a volume ratio of toluene to water of 4:6), dispersed at a speed of 15000 rpm for 2 min, and then the entire system was placed at 4°C and centrifuged at a speed of 2000 r / min for 15 min, the upper emulsion was mixed with a 2 g / mL glutaraldehyde solution, and cross-linked at 4°C for 10 h to obtain a gel; the obtained gel was uniformly cut into 1 cm 3 The small pieces were freeze-dried at -72 °C for 48 h to obtain oil-in-water (O / W) emulsion aerogel.
[0078] BET Analysis:
[0079] The morphology, mechanical properties, specific surface area and porosity (BET) of the oil-in-water (O / W) emulsion aerogel obtained in this comparative example were detected and analyzed, and the detection method was the same as that in Example 1.
[0080] Comparative Example 2
[0081] Different from Example 1, in this comparative example, 11 mg / mL of an asymmetric modified rapeseed globulin aqueous solution was mixed with toluene to obtain 30 mL of a mixture with an oil-to-water ratio of 40% (i.e., a volume ratio of toluene to water of 4:6), dispersed at a speed of 15000 rpm for 2 min, and then the entire system was placed at 4°C and centrifuged at a speed of 2000 r / min for 10 min, the upper emulsion was mixed with a 2 g / mL glutaraldehyde solution, and cross-linked at 4°C for 10 h to obtain a gel; the obtained gel was uniformly cut into 1 cm 3 The small pieces were freeze-dried at -72 °C for 48 h to obtain water-in-oil (W / O) emulsion aerogel.
[0082] BET Analysis:
[0083] The morphology, mechanical properties, specific surface area and porosity (BET) of the water-in-oil (W / O) emulsion aerogel obtained in this comparative example were detected and analyzed, and the detection method was the same as that in Example 1.
[0084] Table 3 shows the BET analysis results of the oil-in-water (O / W) type, water-in-oil (W / O) type emulsion aerogels and dual-continuous phase emulsion aerogels (protein concentration of 9 mg / mL, oil phase ratio of 40%) obtained in Comparative Examples 1 and 2.
[0085] Table 3 BET analysis results of aerogels of different phases
[0086]
[0087]
[0088] Figure 1 SEM images of bicontinuous emulsion aerogels prepared with different oil ratios. Figure 1 It can be seen that the macroscopic structural density of the co-continuous phase emulsion aerogel shows a trend of first increasing and then decreasing with the increase of the oil phase ratio. When the oil phase ratio is 40%, the pore density of the entire aerogel structure is optimal.
[0089] Figure 2 The SEM images of the bicontinuous emulsion aerogels prepared with different protein concentrations are shown in Figure 2. Figure 2 It can be seen that with the increase of protein concentration, the structural density of aerogel also shows a trend of first increasing and then decreasing. When the protein concentration is 9 mg / mL, the entire aerogel system presents the best structural density in the macroscopic sense.
[0090] Figure 3The N2 adsorption-desorption curves and pore size distribution diagrams of double continuous emulsion aerogels prepared at different oil phase ratios and different protein concentrations. From a and b, we can see that the adsorption amount of aerogels prepared with an oil phase ratio of 40% has a significantly higher increase trend than aerogels prepared under other oil phase ratio conditions. This is most likely due to the larger pore size and pore volume and higher porosity of aerogels prepared under the 40% oil phase ratio. It can also be seen that when the oil phase ratio is 40%, the aerogels have more large pore size distributions; from c and d, when the oil phase ratio is constant, the N2 adsorption-desorption curves of aerogels prepared within this protein concentration range are relatively similar, and all have good adsorption trends, indicating that they all have good pore conditions. However, from the pore size distribution diagram ( Figure 3 d) It can be seen that the aerogel prepared at a protein concentration of 9 mg / mL has a relatively larger large pore capacity;
[0091] Figure 4 The SEM images of different phase emulsion aerogels are shown in Figure 2. Figure 4 It can be seen that the aerogel structure prepared by O / W emulsion has uneven pores and loose structure ( Figure 4 a), the aerogel structure prepared by W / O type emulsion has fewer pores ( Figure 4 c), while the dual-phase emulsion aerogel ( Figure 4 b) Uniform pore distribution and high porosity;
[0092] Figure 5 The N2 adsorption-desorption curve and pressure curve of different phase emulsion aerogels are shown in the figure. Figure 5 i) and pressure curve characteristics are the best, which can be attributed to the fact that the dual-continuous phase aerogel has the largest specific surface area, porosity and interconnected and complementary spatial structure;
[0093] Figure 6 This is a graph of the adsorption capacity of different protein concentrations and different oil phase ratios in heavy metal solutions at different pH values. It can be seen from the figure that the aerogel prepared when the protein concentration is 9 mg / mL and the oil phase ratio is 40% has the largest amount of heavy metal adsorption. Combined with the above structural analysis of the aerogel, it can be determined that this is because the aerogel prepared under this condition has a large specific surface area, pore size and porosity, and has more heavy metal adsorption sites and large mass transfer channels. It can also be seen that regardless of the protein concentration and oil phase ratio conditions, the adsorption performance of the aerogel is best when pH = 8, and the adsorption amount reaches 172.196 mg / g within 30 minutes;
[0094] Figure 7The figure shows the adsorption effect of gel with different contents on Cd(Ⅱ). As can be seen from the figure, with the increase of gel content, the removal efficiency of Cd(Ⅱ) in the sample also increases. After 30 mg, the improvement of gel removal efficiency slows down. This may be due to the limited concentration of Cd(Ⅱ) in the sample, and the gel cannot be fully utilized.
[0095] Figure 8 The figure shows the effect of multiple cycles of adsorption of Cd(Ⅱ) by aerogel prepared when the protein concentration is 9 mg / mL and the oil phase ratio is 40%. As can be seen from the figure, with the increase of the number of cycles of adsorption, the cadmium ion adsorption efficiency decreases, but it always remains above 150 mg / g, indicating that the aerogel has good cyclic reusability;
[0096] Fig. 9 The figure shows the adsorption effect of aerogels prepared at a protein concentration of 9 mg / mL and an oil phase ratio of 40% on different heavy metals. It can be seen from the figure that under pH = 8, the aerogel has the largest adsorption capacity for Cu (Ⅱ) and Pb (Ⅱ), and the adsorption capacity is greater than 200 mg / g, indicating that the prepared aerogel also has a good adsorption effect on these two types of heavy metal ions.
[0097] It can be seen from the above embodiments that the present invention provides an asymmetric modified rapeseed globulin-based aerogel and its preparation method and application. The dual-continuous phase emulsion aerogel prepared under the conditions of a protein concentration of 9 mg / mL and an oil-to-water ratio of 40% has the best mechanical properties, the largest specific surface area, pore size and porosity, and the best mass transfer channel. The adsorption effect of the heavy metal element Cd(Ⅱ) is the best under the condition of pH=8, and the adsorption capacity of 30 mg aerogel reaches 172.196 mg / g in half an hour. At the same time, the aerogel also has a good adsorption effect on heavy metal elements Cu(Ⅱ) and Pb(Ⅱ) other than Cd(Ⅱ). It can be seen that the asymmetric modified rapeseed globulin-based aerogel provided by the present invention has excellent mechanical properties, a large specific surface area, pore size and porosity, and a large mass transfer channel, and has better structure and performance than water-in-oil and oil-in-water aerogels. When applied to heavy metal adsorption, the asymmetric modified rapeseed globulin-based aerogel of the present invention has a rich pore structure and heavy metal adsorption sites. It not only has an extremely high adsorption capacity for a variety of heavy metals in a short period of time, but also has good recycling reusability, solving the technical problems in the prior art of low heavy metal removal selectivity, limited adsorption capacity and easy secondary pollution.
[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an asymmetric modified rapeseed protein-based aerogel, characterized in that: The following steps are involved: 1) using an asymmetric modified rapeseed globulin solution as an emulsifier, and toluene and water as two continuous phases, to obtain a stable bicontinuous phase emulsion after dispersion; 2) after centrifuging the bicontinuous phase emulsion of step 1), cross-linking the upper layer of the emulsion with a glutaraldehyde solution to obtain a gel; 3) freeze-drying the gel obtained in step 2) to obtain an asymmetric modified rapeseed protein-based aerogel.
2. The method for preparing the asymmetric modified rapeseed protein-based aerogel according to claim 1, characterized in that: In step 1), the volume ratio of toluene to water is 1:1-4.
3. The method for preparing the asymmetric modified rapeseed protein-based aerogel according to claim 1 or 2, characterized in that: In step 1), the concentration of the asymmetrically modified rapeseed globulin solution is 7-10 mg / mL.
4. The method for preparing the asymmetric modified rapeseed protein-based aerogel according to claim 3, characterized in that: In step 1), the dispersion speed is 10000-18000 rpm, and the dispersion time is 1-3 min.
5. The method for preparing the asymmetric modified rapeseed protein-based aerogel according to claim 1, 2 or 4, characterized in that: In step 2), the temperature of the centrifugal treatment is 2-5° C., the speed of the centrifugal treatment is 1000-3000 r / min, and the time of the centrifugal treatment is 5-15 min.
6. The method for preparing the asymmetric modified rapeseed protein-based aerogel according to claim 1, characterized in that: In step 2), the cross-linking time is 6 to 14 hours.
7. The method for preparing the asymmetric modified rapeseed protein-based aerogel according to claim 1 or 6, characterized in that: In step 2), the concentration of the glutaraldehyde solution is 1.5-2 g / mL.
8. The method for preparing the asymmetric modified rapeseed protein-based aerogel according to claim 1, characterized in that: In step 3), the freeze-drying temperature is -60 to 80°C, and the freeze-drying time is 40 to 60 hours.
9. Asymmetrically modified rapeseed protein-based aerogel prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the asymmetric modified rapeseed protein-based aerogel according to claim 9 as an adsorbent in heavy metal adsorption.