Square NaNbO3 hydrogen storage material catalyst, hydrogen storage material containing catalyst and preparation method

By combining the block-shaped NaNbO3 catalyst with magnesium hydride, the problem of poor kinetic performance of magnesium-based hydrogen storage materials is solved, efficient hydrogen absorption and release kinetic performance and long cycle life are achieved, and the application potential of hydrogen storage materials is enhanced.

CN119075971APending Publication Date: 2024-12-06CHONGQING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411199589.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The high thermodynamic stability and poor kinetic properties of magnesium-based hydrogen storage materials lead to high hydrogen release temperature and slow rate, which limits its application in the field of hydrogen storage.

Method used

The MgH2-block NaNbO3 composite hydrogen storage material was prepared by hydrothermal reaction and ball milling to improve its hydrogen release and hydrogen absorption kinetic properties.

Benefits of technology

The dehydrogenation amount of 6.14 wt.% within 3 minutes of 300°C and the hydrogen absorption amount of 4.28 wt.% within 1 min of 125°C, and has high cycle life and stable hydrogen diffusion shortcuts, which significantly improves the kinetics of hydrogen storage materials. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075971A_ABST
    Figure CN119075971A_ABST
Patent Text Reader

Abstract

The invention relates to a square NaNbO3 hydrogen storage material catalyst, a hydrogen storage material containing the catalyst and a preparation method, and belongs to the technical field of hydrogen storage. The preparation method of the NaNbO3 hydrogen storage material catalyst comprises the following steps: adding Nb2CTx MXene into a NaOH solution, uniformly mixing, then adding H2O2, uniformly mixing again to obtain a mixed solution, putting the mixed solution into a high-pressure reaction kettle, carrying out hydrothermal reaction, then carrying out centrifugal washing, and finally carrying out vacuum drying, thereby obtaining the NaNbO3 hydrogen storage material catalyst. After the catalyst is compounded with magnesium hydride, an excellent catalytic effect is shown: in the aspect of hydrogen desorption kinetics, the dehydrogenation amount of a composite hydrogen storage material at 300 DEG C within 3 minutes can reach 6.14 wt.%; in the aspect of hydrogen absorption dynamics, the hydrogen absorption amount of the composite hydrogen storage material is 4.28 wt.% at 125 DEG C within 1 min. Besides, the composite hydrogen storage material has relatively long cycle life, the hydrogen storage capacity is not obviously changed after 40 times of hydrogen absorption and desorption cycles, and the capacity retention ratio is 99.7%. The catalyst preparation method is simple, raw materials are easy to obtain, and the catalyst is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen storage, and relates to a block-shaped NaNbO3 hydrogen storage material catalyst, a hydrogen storage material containing the catalyst, and a preparation method. Background Art

[0002] Hydrogen energy has many advantages such as abundant resources, clean and efficient, and is an important part of my country's energy structure. Safe and efficient hydrogen storage and transportation technology is a key technical bottleneck restricting the development of the hydrogen energy industry. Magnesium-based hydrogen storage materials have a high hydrogen storage density. Their theoretical mass hydrogen storage density and volume hydrogen storage density are 7.6wt% and 110g / L respectively. They are also low-priced, abundant in reserves, and have stable hydrogen absorption and desorption cycle characteristics. They are currently one of the most promising hydrogen storage materials. However, due to their high thermodynamic stability and poor kinetic performance, they have high hydrogen desorption temperatures and slow rates, which seriously restrict their development. At present, catalyst doping can effectively improve the hydrogen absorption and desorption power of magnesium-based hydrogen storage materials, which has important theoretical significance for their practical applications.

[0003] Recent studies have found that two-dimensional transition metal carbon / nitrides (MXene) have shown good application prospects in the field of energy storage due to their excellent chemical and physical properties (large specific surface area, good chemical durability and good conductivity). x MXene has been extensively studied through experiments and theoretical calculations, and has shown great potential in lithium-ion batteries, medicine, photocatalysis, and other fields. x It has a higher specific surface area, which means more catalytic active sites; at the same time, Nb2CT x It has multivalent characteristics, which is conducive to electron transfer during hydrogen absorption and desorption. In addition, it has good conductivity and rich surface functional groups, which is conducive to improving Nb2CT x The overall catalytic performance after being combined with other catalysts. x The catalytic effect of Nb2CT is limited, and its slow hydrogen absorption and desorption kinetics still greatly restrict its application in hydrogen storage. Therefore, further exploration of Nb2CT x Its potential for hydrogen storage applications can be further modified. Summary of the invention

[0004] In view of this, one of the objects of the present invention is to provide a method for preparing a block-shaped NaNbO3 hydrogen storage material catalyst; a second object is to provide a block-shaped NaNbO3 hydrogen storage material catalyst; a third object is to provide a hydrogen storage material containing the catalyst; and a fourth object is to provide a method for preparing a hydrogen storage material containing the catalyst.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] 1. A method for preparing a block-shaped NaNbO3 hydrogen storage material catalyst, the method being as follows:

[0007] Nb2CT x MXene is added to a NaOH solution, H2O2 is added after mixing, and the mixture is mixed again to obtain a mixed solution, and the mixed solution is placed in a high-pressure reactor, centrifuged and washed after a hydrothermal reaction, and finally vacuum dried.

[0008] Preferably, the method is as follows

[0009] Nb2CT x MXene is added to the NaOH solution, mixed and then 30% H2O2 is added, mixed again to obtain a mixed solution, the mixed solution is placed in a high pressure reactor, subjected to hydrothermal reaction at 180-200°C for 10-14h, centrifuged and washed, and finally vacuum dried; NaOH, water, Nb2CT x The mass volume ratio of MXene and H2O2 with a mass fraction of 30% is: 11-13:10-40:50:0.88, g:mL:mg:mL.

[0010] Preferably, the centrifugal washing is specifically: centrifugal washing with deionized water at a speed of 3000-8000 rpm until the mixed system is neutral.

[0011] Preferably, the vacuum drying is specifically: vacuum drying at 60-100° C. for 8-16 hours.

[0012] Preferably, the Nb2CT x The preparation method of MXene is as follows:

[0013] LiF is dissolved in concentrated hydrochloric acid to obtain an etching solution, and then Nb2AlC is placed in the etching solution, subjected to hydrothermal reaction, centrifuged and washed, and finally vacuum dried to obtain Nb2CT. x MXene.

[0014] Preferably, the mass volume ratio of LiF, Nb2AlC and concentrated hydrochloric acid is: 1-1.4:0.8-1.2:10-30, g:g:mL; the hydrothermal reaction is specifically: reacting in a reactor at 100-150°C for 12-36h; the centrifugal washing is specifically: centrifugal washing with deionized water at a speed of 3000-8000rpm until the mixed system is neutral; the vacuum drying is specifically: vacuum drying at 60-100°C for 8-16h.

[0015] 2. A block-shaped NaNbO3 hydrogen storage material catalyst prepared by the preparation method.

[0016] 3. A MgH2-block NaNbO3 composite hydrogen storage material, which comprises, by mass percentage, 3-10 wt.% of block NaNbO3 and 90-97 wt.% of MgH2.

[0017] 4. A method for preparing a MgH2-block NaNbO3 composite hydrogen storage material, the preparation method being as follows: MgH2 and block NaNbO3 are intermittently ball-milled in an argon atmosphere at a ball-to-material ratio of 10 to 40:1 at a speed of 200 to 1200 rpm for 8 to 24 hours.

[0018] Preferably, the forward and reverse intermittent ball milling is specifically: after each ball milling for 5 to 30 minutes, there is a pause for 5 to 30 minutes.

[0019] The beneficial effects of the present invention are as follows: the present invention provides a block-shaped NaNbO3 hydrogen storage material catalyst, a hydrogen storage material containing the catalyst and a preparation method. After the catalyst is compounded with magnesium hydride, it shows an excellent catalytic effect: in terms of hydrogen release kinetics, the dehydrogenation amount of the composite hydrogen storage material at 300°C and within 3 minutes can reach 6.14wt.%, while the dehydrogenation amount of ball-milled MgH2 at 300°C and within 10 minutes is only 0.2wt.%, and the dehydrogenation amount within 120 minutes is only 5.4wt.%; in terms of hydrogen absorption kinetics, the hydrogen absorption amount of the composite hydrogen storage material at 125°C and within 1 minute is 4.28wt.%, while the hydrogen absorption amount of ball-milled MgH2 at 125°C and within 1 minute is only 0.92wt.%, and the hydrogen absorption amount within 20 minutes is only 4.22wt.%. In addition, the composite hydrogen storage material has a high cycle life. After 40 cycles of hydrogen absorption and desorption, the hydrogen storage capacity does not change significantly, and the capacity retention rate is 99.7%. The catalyst preparation method is simple, and the raw materials are easily available, which is suitable for large-scale production.

[0020] The reason why the block-shaped NaNbO3 hydrogen storage material catalyst has excellent catalytic performance is that the NaNbO3 catalyst is ground with MgH2 to form NaMgH3, NbH xand Nb, and remain stable during the subsequent hydrogen absorption and desorption process. NaMgH3 and NbH x In the process of hydrogen absorption and desorption, it provides sufficient hydrogen diffusion shortcuts, promoting the dissociation and recombination of hydrogen. In addition, niobium elements in multiple valent states (Nb 5+ 、Nb、NbH x ) can accelerate the mutual conversion of Mg and MgH2.

[0021] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0023] Figure 1 Nb2CT in Example 1 x SEM image of MXene;

[0024] Figure 2 This is the SEM image of the block NaNbO3 in Example 1;

[0025] Figure 3 This is the XRD pattern of the square block NaNbO3 in Example 1;

[0026] Figure 4 The isothermal hydrogen desorption curves of the MgH2-3NaNbO3 composite hydrogen storage material, the MgH2-5NaNbO3 composite hydrogen storage material and the MgH2-10NaNbO3 composite hydrogen storage material prepared in Examples 4-6 at 300°C;

[0027] Figure 5 Isothermal hydrogen absorption curves of the MgH2-3NaNbO3 composite hydrogen storage material, the MgH2-5NaNbO3 composite hydrogen storage material and the MgH2-10NaNbO3 composite hydrogen storage material prepared in Examples 4-6 at 125°C and 30 bar;

[0028] Figure 6 is the isothermal hydrogen release curve of ball-milled MgH2 prepared in the comparative example at 300°C;

[0029] Figure 7 The isothermal hydrogen absorption curve of the ball-milled MgH2 prepared in the comparative example at 125°C and 30 bar;

[0030] Figure 8This is the cyclic hydrogen absorption and desorption curve of the MgH2-5NaNbO3 composite hydrogen storage material prepared in Example 5 at 300°C. DETAILED DESCRIPTION

[0031] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0032] Example 1

[0033] Preparation of Cube NaNbO3

[0034] (1) 1 g of LiF was dissolved in 20 mL of 12 mol / L concentrated hydrochloric acid to obtain an etching solution, and then 1 g of Nb2AlC was placed in the etching solution. After reacting in a 100 mL high-pressure reactor at 125 ° C for 24 h, it was centrifuged and washed with deionized water at a speed of 6000 rpm until the mixed system was neutral. Finally, it was vacuum dried at 60 ° C for 12 h to obtain Nb2CT. x MXene;

[0035] (2) Dissolve 12 g of NaOH in 30 mL of deionized water and stir magnetically at room temperature until the solution becomes clear to obtain a NaOH solution; add 50 mg of Nb2CT prepared in step (1) x MXene was added to NaOH solution, and after magnetic stirring for 5 minutes at room temperature, 0.88 mL of 30% H2O2 was added, and a mixed solution was obtained after magnetic stirring at 40°C for 15 minutes. The mixed solution was placed in a high-pressure reactor and subjected to hydrothermal reaction at 180°C for 12 hours; then, it was centrifuged and washed with deionized water at 6000 rpm until the mixed system was neutral, and finally vacuum dried at 60°C for 12 hours to obtain block-shaped NaNbO3.

[0036] The Nb2CT prepared in Example 1 was observed by scanning electron microscopy. x MXene and Cube NaNbO3 were characterized, and the results were as follows: Figure 1 and Figure 2 As shown by Figure 1 It can be seen that Nb2CT x MXene is in the form of micrometer-sized two-dimensional layers. Figure 2 It can be seen that Cube NaNbO3 is in the shape of micron cubes.

[0037] The Cube NaNbO3 prepared in Example 1 was characterized by X-ray diffractometer, and the results are as follows: Figure 3 As shown by Figure 3 It can be seen that it is completely consistent with the standard PDF card of sodium niobate, indicating that high-purity sodium niobate has been successfully produced.

[0038] Example 2

[0039] Preparation of Cube NaNbO3

[0040] (1) 1.2 g of LiF was dissolved in 30 mL of 12 mol / L concentrated hydrochloric acid to obtain an etching solution, and then 0.8 g of Nb2AlC was placed in the etching solution. After reacting at 100 ° C for 36 h in a 100 mL high-pressure reactor, the mixture was centrifuged and washed with deionized water at a speed of 3000 rpm until the mixed system was neutral. Finally, it was vacuum dried at 80 ° C for 16 h to obtain Nb2CT. x MXene;

[0041] (2) Dissolve 11 g of NaOH in 10 mL of deionized water and stir magnetically at room temperature until the solution becomes clear to obtain a NaOH solution; add 50 mg of Nb2CT prepared in step (1) x MXene was added to NaOH solution, and after magnetic stirring for 5 minutes at room temperature, 0.88 mL of 30% H2O2 was added, and a mixed solution was obtained after magnetic stirring at 40°C for 15 minutes. The mixed solution was placed in a high-pressure reactor and subjected to hydrothermal reaction at 200°C for 10 hours; then, it was centrifuged and washed with deionized water at 3000 rpm until the mixed system was neutral, and finally vacuum dried at 80°C for 16 hours to obtain block-shaped NaNbO3.

[0042] Example 3

[0043] Preparation of Cube NaNbO3

[0044] (1) 1.4 g LiF was dissolved in 10 mL 12 mol / L concentrated hydrochloric acid to obtain an etching solution, and then 1.2 g Nb2AlC was placed in the etching solution, reacted at 150 ° C for 12 h in a 100 mL high-pressure reactor, and then centrifuged and washed with deionized water at 8000 rpm until the mixed system was neutral, and finally vacuum dried at 100 ° C for 8 h to obtain Nb2CT x MXene;

[0045] (2) Dissolve 13 g of NaOH in 40 mL of deionized water and stir magnetically at room temperature until the solution becomes clear to obtain a NaOH solution; add 50 mg of Nb2CT prepared in step (1) xMXene was added to NaOH solution, and after magnetic stirring for 5 minutes at room temperature, 0.88 mL of 30% H2O2 was added, and a mixed solution was obtained after magnetic stirring at 40°C for 15 minutes. The mixed solution was placed in a high-pressure reactor and subjected to hydrothermal reaction at 180°C for 14 hours; then, it was centrifuged and washed with deionized water at 8000 rpm until the mixed system was neutral, and finally vacuum dried at 100°C for 8 hours to obtain block-shaped NaNbO3.

[0046] Example 4

[0047] Preparation of MgH2-3NaNbO3 composite hydrogen storage material

[0048] In a vacuum glove box, MgH2 and the block-shaped NaNbO3 prepared in Example 1 were weighed and mixed at a mass ratio of 97:3, with a total mass of 1 g, and then the mixture was poured into a ball mill, with a ball-to-material ratio of 1:20 between the mixture and 304 stainless steel balls. The ball mill was filled with 0.2 MPa argon gas and installed on a high-energy ball mill, and the mill was run at a speed of 400 rpm for 10 min forward and 10 min rest, and then reversed for 10 min and 10 min rest, with an effective ball milling time of 10 h. The composite material was recorded as MgH2-3NaNbO3.

[0049] Example 5

[0050] Preparation of MgH2-5NaNbO3 composite hydrogen storage material

[0051] The difference from Example 4 is that MgH2 and the block-shaped NaNbO3 prepared in Example 1 are weighed and mixed at a mass ratio of 95:5. The composite material is recorded as MgH2-5NaNbO3.

[0052] Example 6

[0053] Preparation of MgH2-10NaNbO3 composite hydrogen storage material

[0054] The difference from Example 4 is that MgH2 and the block-shaped NaNbO3 prepared in Example 1 are weighed and mixed at a mass ratio of 90:10. The composite material is recorded as MgH2-10NaNbO3.

[0055] Comparative Example

[0056] Preparation of ball-milled MgH2

[0057] In a vacuum glove box, pour 1g of MgH2 into a ball mill with a ball-to-material ratio of MgH2 to 304 stainless steel balls of 1:20. Fill the ball mill with 0.2Mpa argon and install it on a high-energy ball mill. Run it forward at 400rpm for 10min, rest for 10min, then reverse for 10min, rest for 10min. The effective ball milling time is 10h.

[0058] Example 7

[0059] Test on hydrogen absorption and desorption performance of MgH2-NaNbO3 composite hydrogen storage material

[0060] In a glove box, 125 mg of the MgH2-3NaNbO3 composite hydrogen storage material, MgH2-5NaNbO3 composite hydrogen storage material and MgH2-10NaNbO3 composite hydrogen storage material prepared in Examples 4-6 were weighed respectively and placed in a special sample tube of a high-pressure gas adsorption-desorption instrument in sequence. The samples were placed in a PCT-PRO hydrogen storage performance test device, and the dehydrogenation performance test was performed at 300°C and the hydrogen absorption performance test was performed at 125°C. The results are shown in FIG. Figure 4 and Figure 5 As shown. Among them, Figure 4 The isothermal dehydrogenation curves of three composite hydrogen storage materials, MgH2-3NaNbO3, MgH2-5NaNbO3 and MgH2-10NaNbO3 at 300°C. It can be seen from the figure that the dehydrogenation rate is 5wt.%>3wt.%>10wt.%; the dehydrogenation amount is 3wt.%>5wt.%>10wt.%. Figure 5 The isothermal hydrogen absorption curves of three composite hydrogen storage materials, MgH2-3NaNbO3, MgH2-5NaNbO3 and MgH2-10NaNbO3, at 125°C and 30 bar, show that in terms of hydrogen absorption rate, 5wt.%>3wt.%>10wt.%; in terms of hydrogen absorption amount, 3wt.%>5wt.%>10wt.%. By comparison, considering the hydrogen absorption and desorption amount and hydrogen absorption and desorption rate, the performance of the MgH2-5NaNbO3 composite hydrogen storage material is the best, that is, the optimal doping ratio of the NaNbO3 catalyst is 5wt.%.

[0061] 125 mg of the ball-milled MgH2 prepared in the comparative example was weighed in a glove box and placed in a special sample tube of a high-pressure gas adsorption-desorption instrument. The sample was placed in a PCT-PRO hydrogen storage performance test device and subjected to a dehydrogenation performance test at 300°C and a hydrogen absorption performance test at 125°C. The results are shown in FIG. Figure 6 and Figure 7 shown.

[0062] By comparing the isothermal dehydrogenation curves of ball-milled MgH2 and MgH2-5NaNbO3 composite hydrogen storage materials at 300°C, it can be seen that the MgH2-5 NaNbO3 composite hydrogen storage material rapidly releases 6.14wt.% of hydrogen within 3min at 300°C, while the dehydrogenation amount of ball-milled MgH2 within 10min at 300°C is only 0.2wt.%, and the dehydrogenation amount within 120min reaches 5.4wt.%.

[0063] By comparing the isothermal hydrogen absorption curves of ball-milled MgH2 and MgH2-5NaNbO3 composite hydrogen storage materials at 125℃ and 30bar, it can be seen that the hydrogen absorption amount of MgH2-5NaNbO3 composite hydrogen storage material within 125℃ and 1min can reach 4.28wt.%, while the hydrogen absorption amount of ball-milled MgH2 within 125℃ and 1min is only 0.92wt.%, and the hydrogen absorption within 20min is only 4.22wt.%.

[0064] In summary, the blocky NaNbO3 has a good catalytic effect on the dehydrogenation kinetics and hydrogen absorption kinetics of MgH2.

[0065] Example 8

[0066] Cyclic hydrogen absorption and desorption performance test of MgH2-NaNbO3 composite hydrogen storage material

[0067] 125 mg of the MgH2-5NaNbO3 composite hydrogen storage material prepared in Example 5 was weighed in a glove box and placed in a special sample tube of a high-pressure gas adsorption and desorption instrument. The sample was placed in a PCT-PRO hydrogen storage performance test device and a cyclic hydrogen absorption and desorption performance test was performed at 300°C. The results are shown in FIG. Figure 8 As shown by Figure 8 It can be seen that after 40 cycles, there is no trend of hydrogen storage capacity decreasing, and the capacity retention rate is 99%, indicating that the composite hydrogen storage material of the present invention has an excellent cycle life.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a block-shaped NaNbO3 hydrogen storage material catalyst, characterized in that: The method is as follows: Nb2CT x MXene is added to a NaOH solution, H2O2 is added after mixing, and the mixture is mixed again to obtain a mixed solution, and the mixed solution is placed in a high-pressure reactor, centrifuged and washed after a hydrothermal reaction, and finally vacuum dried.

2. The preparation method according to claim 1, characterized in that The method is as follows: Nb2CT x MXene is added to the NaOH solution, mixed and then 30% H2O2 is added, mixed again to obtain a mixed solution, the mixed solution is placed in a high pressure reactor, subjected to hydrothermal reaction at 180-200°C for 10-14h, centrifuged and washed, and finally vacuum dried; NaOH, water, Nb2CT x The mass volume ratio of MXene and H2O2 with a mass fraction of 30% is: 11-13:10-40:50:0.88, g:mL:mg:mL.

3. The preparation method according to claim 1 or 2, characterized in that: The centrifugal washing specifically includes: centrifugal washing with deionized water at a speed of 3000-8000 rpm until the mixed system is neutral.

4. The preparation method according to claim 1 or 2, characterized in that: The vacuum drying is specifically: vacuum drying at 60-100° C. for 8-16 hours.

5. The preparation method according to claim 1 or 2, characterized in that: The Nb2CT x The preparation method of MXene is as follows: LiF is dissolved in concentrated hydrochloric acid to obtain an etching solution, and then Nb2AlC is placed in the etching solution, subjected to hydrothermal reaction, centrifuged and washed, and finally vacuum dried to obtain Nb2CT. x MXene.

6. The preparation method according to claim 5, characterized in that: The mass volume ratio of LiF, Nb2AlC and concentrated hydrochloric acid is: 1-1.4:0.8-1.2:10-30, g:g:mL; the hydrothermal reaction is specifically: reacting in a reactor at 100-150°C for 12-36h; the centrifugal washing is specifically: centrifugal washing with deionized water at a speed of 3000-8000rpm until the mixed system is neutral; the vacuum drying is specifically: vacuum drying at 60-100°C for 8-16h.

7. A block-shaped NaNbO3 hydrogen storage material catalyst prepared by the preparation method according to any one of claims 1 to 6.

8. A MgH2-block NaNbO3 composite hydrogen storage material, characterized in that: Calculated by mass percentage, the composite hydrogen storage material comprises: 3-10wt.% of block-shaped NaNbO3 and 90-97wt.% of MgH2.

9. A method for preparing a MgH2-block NaNbO3 composite hydrogen storage material, characterized in that: The preparation method is as follows: MgH2 and block-shaped NaNbO3 are intermittently ball-milled in an argon atmosphere at a ball-to-material ratio of 10 to 40:1 at a rotation speed of 200 to 1200 rpm for 8 to 24 hours.

10. The preparation method according to claim 9, characterized in that: The forward and reverse intermittent ball milling specifically includes: a pause of 5 to 30 minutes after each ball milling of 5 to 30 minutes.