MoO3 / g-C3N4 catalyst reinforced by radio frequency plasma technology and phosphorylation reaction application of MoO3 / g-C3N4 catalyst
Molybdenum trioxide is processed through radio frequency plasma technology and doped with graphite phase carbon nitride, and reacted with phosphonoyl compounds to form an efficient MoO3/g-C3N4 catalyst, which solves the problem of insufficient light absorption in the visible light range. Highly efficient catalytic and low-pollution synthesis of sulfonate phosphonate is achieved.
Patent Information
- Application Number
- CN202411190888.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing MoO3/g-C3N4 heterojunction catalyst has limited light absorption in the visible light range, resulting in insufficient photocatalytic performance and requires surface modification to improve photocatalytic activity.
Molybdenum trioxide is treated with radio frequency plasma technology, reducing its particle size and doping it with graphite phase carbon nitride to form a larger surface area of MoO3/g-C3N4 catalyst, combined with phosphonoyl reaction, and improving the catalytic effect.
The photocatalytic activity and surface area of the catalyst are significantly improved, and the synthesis of thiophosphonate is achieved efficiently, and has the advantages of low pollution, low corrosion and reusability.
Smart Images

Figure CN119075972A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of green catalyst synthesis, and specifically relates to a MoO3 / g-C3N4 catalyst enhanced by radio frequency plasma technology and its application in phosphonylation reaction. Background Art
[0002] Molybdenum trioxide is an important transition metal oxide and semiconductor material with high thermal and chemical stability, low price and environmental protection. The inherent properties of molybdenum trioxide, such as each layer in the layered structure is bonded by weak van der Waals interactions, make molybdenum trioxide an effective catalyst. In addition, molybdenum trioxide also exhibits good photoelectric properties, but it absorbs a limited amount of light in the visible light range, so molybdenum trioxide usually requires another semiconductor material for surface modification to improve its photocatalytic performance. Graphitic carbon nitride (g-C3N4) has attracted widespread attention due to its two-dimensional structure, good stability and simple preparation method. It is an economical, non-metallic and non-toxic component that can be doped with molybdenum trioxide to make a heterojunction photocatalyst system, thereby exhibiting better photocatalytic properties.
[0003] The MoO3 / g-C3N4 heterojunction catalysts reported in the literature and patents are mainly used in the photocatalytic degradation of pollutants. For example, in 2013, Huaming Li et al. prepared a new composite photocatalyst g-C3N4 / MoO3 by a simple calcination method, and the photocatalytic activity was greatly enhanced. It was applied to the degradation of methylene blue pollutants. The best photocatalytic activity was 4.2 times and 1.9 times that of pure molybdenum trioxide and g-C3N4, respectively. The hybrid effect of molybdenum trioxide and g-C3N4 and the possible mechanism of improving photocatalytic activity were proposed. In 2019, Shengyan Pu et al. synthesized MoO3 / g-C3N4 heterojunction catalysts by a simple mixed calcination method and applied them to the degradation of rhodamine B. In the mechanism study, it was found that the application of the catalyst increased the formation of superoxide radicals and hydroxyl radicals, and superoxide radicals and superoxide radicals dominated the photocatalytic effect. In 2020, Do-HeyoungKim et al. prepared g-C3N4 / MoO3 heterojunction structures using wet chemical techniques to enhance the photocatalytic oxidation of Rhodamine B under visible light irradiation. The study found that the improvement in the catalytic activity of g-C3N4 / MoO3 microcomposites was due to the efficient photogeneration of electron-hole pairs and charge transfer caused by the favorable energy band position of C3N4 / MoO3, which is impossible to achieve with a single material. Summary of the invention
[0004] The idea of the present invention is to use radio frequency plasma technology to treat the metal oxide molybdenum trioxide, reduce the particle size of molybdenum trioxide, and increase the surface area of molybdenum trioxide. The treated molybdenum trioxide is doped with g-C3N4 to obtain a better loading effect, so that the obtained new catalyst has a larger specific surface area and a better catalytic effect than similar catalysts that have not been treated with plasma radio frequency.
[0005] The technical solution adopted by the present invention is as follows:
[0006] In a first aspect, the present invention provides a method for preparing a sulfur-containing phosphonate, which specifically comprises the following steps:
[0007] Adding a sulfur-containing compound, a phosphorus-containing compound and a photocatalyst MoO3 / g-C3N4 heterojunction into a solvent;
[0008] The general structural formula of the phosphorus-containing compound is as follows:
[0009]
[0010] Wherein, R1 and R2 are independently selected from substituted or unsubstituted alkyl, substituted or unsubstituted aryl, substituted or unsubstituted heteroaryl, substituted or unsubstituted alkoxy;
[0011] The general structural formula of the sulfur-containing compound is as follows:
[0012] R-SH(II)
[0013] Wherein, R is selected from substituted or unsubstituted alkyl, substituted or unsubstituted aryl, substituted or unsubstituted heteroaryl, substituted or unsubstituted alkoxy;
[0014] The photocatalyst MoO3 / g-C3N4 heterojunction preparation method is as follows:
[0015] MoO3 is subjected to radio frequency treatment in a radio frequency plasma device under an inert gas environment for 10 to 90 minutes, with the power set to 10 to 200 W, and then the treated MoO3 and g-C3N4 are dispersed together in an alcohol solution and fully dispersed, and the alcohol solution is removed by heating, and finally the mixture is calcined at 200 to 400° C. for 2 to 6 hours to obtain a radio frequency MoO3 / g-C3N4 catalyst;
[0016] Under the light with a wavelength of 400 to 440 nm and a light intensity of 5 to 10 W, the reaction is fully carried out in a solvent to obtain a sulfur-containing phosphonate product, and the reaction formula is as follows:
[0017]
[0018] Preferably, the mass ratio of MoO3 to g-C3N4 in the MoO3 / g-C3N4 heterojunction is 1:49 to 1:10.
[0019] Preferably, in the reaction system, the molar proportions of the sulfur-containing compound, the phosphorus-containing compound and the photocatalyst MoO3 / g-C3N4 heterojunction are 50 to 150 molar proportions, 150 to 250 molar proportions and 0.5 to 2 molar proportions respectively.
[0020] Preferably, the solvent is DCE solvent.
[0021] Preferably, the reaction is carried out at room temperature for 16 hours under 420 nm, 8 W light.
[0022] Preferably, the phosphorus-containing compound includes diphenylphosphine, di(4-methylphenyl)phosphine, di(4-methoxyphenyl)phosphine, di(4-tert-butylphenyl)phosphine, di(3,5-dimethylphenyl)phosphine, dimethyl phosphite, diethyl phosphite, diisopropyl phosphite, dibutyl phosphite, diphenyl phosphite, DOPO-(9-,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide), ethyl phenyl phosphate, and phenyl n-butylphosphine.
[0023] Preferably, the sulfur-containing compound includes n-butyl mercaptan, cyclohexyl mercaptan, benzyl mercaptan, 2-naphthalenethiol, 4-methylthiophenol, 4-tert-butylthiophenol, 4-methoxythiophenol, 4-fluorothiophenol, 4-chlorothiophenol, 4-bromothiophenol, 2-methylthiophenol, 3-chlorothiophenol.
[0024] Preferably, after the reaction is completed, the solvent is removed by rotary evaporation and a purified product is obtained by column chromatography.
[0025] Furthermore, the column chromatography uses a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as an eluent.
[0026] In a second aspect, the present invention provides a photocatalyst MoO3 / g-C3N4 heterojunction, and the preparation method is as follows:
[0027] MoO3 is radio-frequency treated in a radio-frequency plasma device under an inert gas environment for 10 to 90 minutes, with the power set to 10 to 200 W. The treated MoO3 and g-C3N4 are then dispersed together in an alcohol solution and fully dispersed. The alcohol solution is removed by heating, and finally the mixture is calcined at 200 to 400°C for 2 to 6 hours to obtain a radio-frequency MoO3 / g-C3N4 catalyst.
[0028] Beneficial effects achieved by the present invention:
[0029] MoO3 / g-C3N4 heterojunction catalyst was synthesized by plasma technology, which can be used to efficiently catalyze the synthesis of thiophosphonates. Compared with traditional catalytic methods, MoO3 / g-C3N4 can not only efficiently catalyze the synthesis of thiophosphonates, but also has the advantages of low pollution, low corrosion, and reusability. After 5 cycles, the yield of thiophosphonates can still maintain 95% of the initial catalytic yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 .SEM images of MoO3 / g-C3N4: a, SEM image of g-C3N4, b, SEM image of MoO3, c, SEM image of 5wt% MoO3 / g-C3N4 treated with radio frequency, d, SEM image of 5wt% MoO3 / g-C3N4 not treated with radio frequency;
[0031] Figure 2 .FT-IR spectrum of MoO3 / g-C3N4: abscissa: Wavenumbers (cm -1 ), ordinate: Intensity (au);
[0032] Figure 3 .XRD spectrum of MoO3 / g-C3N4: abscissa: 2θ (degree), ordinate: Intensity (au);
[0033] Figure 4 .BET spectrum of MoO3 / g-C3N4;
[0034] Figure 5 .Redox potential spectrum of MoO3 / g-C3N4: horizontal axis: Potential (V vs. Ag / AgCl), vertical axis: Current;
[0035] Figure 6 .Photoexcitation and emission spectra of MoO3 / g-C3N4: Horizontal axis: Wavenumbers (cm -1 ), vertical axis: Counts; DETAILED DESCRIPTION
[0036] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention rather than limiting the patent claims of the present invention.
[0037] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0038] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure materials or materials with conventional purity in the field of synthesis of organic phosphorus compounds.
[0039] In order to further illustrate the present invention, the preparation method of a thiophosphate compound provided by the present invention is described in detail below in conjunction with examples. However, it should be understood that these examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the following examples.
[0040] The catalysts used in the following examples are all catalysts obtained from the following preparation examples.
[0041] Preparation Example
[0042] The 5wt% MoO3 / g-C3N4 heterojunction catalyst after radio frequency is used to catalyze the synthesis of compounds containing PS bonds, and the preparation includes the following steps:
[0043] 5 mg of MoO3 was treated with radio frequency in an RF plasma equipment under argon environment for 30 minutes with the power set to 100 W. The treated MoO3 was then dispersed together with 95 mg of g-C3N4 in ethanol and ultrasonically treated for 1 hour to fully disperse it. The ethanol was removed by heating and the mixture was calcined at 300°C for 4 hours to obtain a 5 wt.% MoO3 / g-C3N4 catalyst solid powder after radio frequency.
[0044] The same method was used but without radio frequency treatment to prepare non-radio frequency 5wt.% MoO3 / g-C3N4 catalyst solid powder as a comparison.
[0045] The structural characterization and morphological analysis of the prepared microcomposites were carried out to understand their crystal structure and surface properties. Figures 1 to 6 shown.
[0046] Example 1
[0047] Synthesis of p-Methylphenylthiodiphenylphosphine oxide
[0048]
[0049] Dissolve 0.4 mm diphenylphosphine oxide, 0.2 mm p-toluene thiophenol, and 1.0 mol% MoO3 / g-C3N4 catalyst in 2 ml of DCE solvent and react at room temperature for 16 hours under 420 nm, 8 W light. After the reaction, concentrate the organic phase and use a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent to obtain the product by column chromatography with a yield of 90%.
[0050] NMR analysis of reaction products:
[0051] 1 H NMR (600MHz, CDCl3) δ7.89–7.80 (m, 4H), 7.48 (t, J = 7.4Hz, 2H), 7.41 (ddd, J = 10.5 ,5.8,4.4Hz,4H),7.32(dd,J=8.1,1.5Hz,2H),6.98(d,J=7.8Hz,2H),2.22(s,3H). 13 CNMR (151MHz, CDCl3) δ139.2 (d, J = 2.3Hz), 135.4 (d, J = 3.8Hz), 133.1 (s), 132.4 (t, J = 8.3Hz) ,131.7(d,J=10.2Hz), 130.0(d,J=1.7Hz), 128.6(d,J=13.1Hz), 122.4(d,J=5.3Hz), 21.3(s). 31 P NMR (243MHz, CDCl3) δ41.21 (s).
[0052] According to the test, after 5 cycles, the yield of thiophosphonate can still maintain 95% of the initial catalytic yield.
[0053] Example 2
[0054] Synthesis of p-Tolylthio-p-dimethyldiphenylphosphine Oxide
[0055]
[0056] 0.4 mm p-dimethyldiphenylphosphine oxide, 0.2 mm p-toluene thiophenol, 1.0 mol% radio frequency 5 wt% MoO3 / g-C3N4 catalyst were dissolved in 2 ml of DCE solvent and reacted at room temperature for 16 hours under 420 nm, 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent, with a yield of 80%.
[0057] NMR analysis of reaction products:
[0058] 1 H NMR (600MHz, CDCl3) δ7.79–7.70 (m, 4H), 7.35 (dd, J=8.1, 1.4Hz, 2H), 7.25 (dd, J=7 .9,3.3Hz,4H),7.02(d,J=8.0Hz,2H),2.38(d,J=7.9Hz,6H),2.27(d,J=7.4Hz,3H). 13CNMR (151MHz, CDCl3) δ142.6 (d, J = 2.9Hz), 138.9 (d, J = 2.4Hz), 135.1 (d, J = 3.7Hz), 131.6 (d, J = 1 0.6Hz), 129.9 (t, J = 8.4Hz), 129.2 (t, J = 8.8Hz), 122.7 (d, J = 5.1Hz), 21.5 (d, J = 1.2Hz), 21.1 (s). 31 P NMR (243MHz, CDCl3) δ41.78 (s).
[0059] Example 3
[0060] Synthesis of p-Tolylthio-p-Chlorodiphenylphosphine Oxide
[0061]
[0062] 0.4 mm of p-chlorodiphenylphosphine oxide, 0.2 mm of p-toluene thiophenol, 1.0 mol% of 5 wt% MoO3 / g-C3N4 catalyst after radio frequency were dissolved in 2 ml of DCE solvent and reacted at room temperature for 16 hours under 420 nm and 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent, with a yield of 75%.
[0063] NMR analysis of reaction products:
[0064] 1 H NMR (600MHz, CDCl3) δ7.80–7.70(m,4H),7.46–7.39(m,4H),7.30(dd,J=8.1,1.6Hz,2H),7.04(d,J=8.1Hz,2H),2.27(s,3H). 13 C NMR (151MHz, CDCl3) δ139.6(d,J=2.4Hz), 139.1(d,J=3.6Hz), 135.3(d,J=3.8Hz), 132.9(d,J=11.2 Hz), 131.2 (s), 130.48 (s), 130.2 (d, J = 1.8Hz), 129.0 (d, J = 13.8Hz), 121.4 (d, J = 5.3Hz), 21.2 (s). 31 P NMR (243MHz, CDCl3) δ39.08 (s).
[0065] Example 4
[0066] Synthesis of p-Tolylthio-dinaphthylphosphine Oxide
[0067]
[0068] 0.4 mm of dinaphthylphosphine oxide, 0.2 mm of p-toluene thiophenol, 1.0 mol% of 5 wt% MoO3 / g-C3N4 catalyst after radio frequency were dissolved in 2 ml of DCE solvent and reacted at room temperature for 16 hours under 420 nm and 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent. The yield was 72%.
[0069] NMR analysis of reaction products:
[0070] 1 H NMR (600MHz, CDCl3) δ8.48(d,J=14.8Hz,2H),7.89(ddd,J=28.7,13.1,4.8Hz,8H),7.55(dt d,J=16.2,6.9,1.1Hz,4H),7.39(dd,J=8.1,1.5Hz,2H),6.97(d,J=8.0Hz,2H),2.19(s,3H). 13 C NMR (151MHz, CDCl3) δ139.1 (d, J = 2.3Hz), 135.3 (d, J = 3.7Hz), 134.7 (d, J = 2.5Hz), 133.9 (d, J = 9.4Hz), 132.3 (d, J = 14.3Hz), 130.2–1 29.9 (m), 129.4 (s), 129.0 (s), 128.3 (t, J = 6.5Hz), 127.7 (s), 126.9 (s), 126.2 (d, J = 11.5Hz), 122.2 (d, J = 5.2Hz), 21.0 (d, J = 6.3Hz). 31 PNMR (243MHz,CDCl3)δ41.36(s).
[0071] Example 5
[0072] Synthesis of p-Tolylthiophenylbenzylphosphine oxide
[0073]
[0074] 0.4 mm of phenylbenzyl phosphine oxide, 0.2 mm of p-toluene thiophenol, 1.0 mol% of 5 wt% MoO3 / g-C3N4 catalyst after radio frequency were dissolved in 2 ml of DCE solvent and reacted at room temperature for 16 hours under 420 nm and 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent. The yield was 78%.
[0075] NMR analysis of reaction products:
[0076] 1 H NMR(600MHz, CDCl3)δ7.66–7.62(m,2H),7.46(ddt,J=7.1,4.2,1.4Hz,1H),7.38–7.33(m,4H),7.21–7.1 7(m,3H),7.08(dt,J=4.9,2.7Hz,2H),7.05(d,J=8.1Hz,2H),3.55(dd,J=14.9,3.9Hz,2H),2.28(s,3H). 13 C NMR (151MHz, CDCl3) δ 139.2 (d, J = 2.2Hz), 135.3 (d, J = 3.6Hz), 132.1 (d, J = 3.0Hz), 131.7 (t, J = 8.3Hz), 130.8 (d, J = 8.3Hz), 130.1 ( dd,J=12.2,3.7Hz),128.4(d,J=3.1Hz),128.2(d,J=12.8Hz),127.0(d,J=3.7Hz),121.9(d,J=5.1Hz),41.5(s),41.1(s),21.1(s). 31 P NMR (243MHz, CDCl3) δ46.75 (s).
[0077] Example 6
[0078] Synthesis of p-Methoxyphenylthiodiphenylphosphine Oxide
[0079]
[0080] 0.4 mm of diphenyl phosphine oxide, 0.2 mm of p-methoxythiophenol, 1.0 mol% of 5 wt% MoO3 / g-C3N4 catalyst after radio frequency were dissolved in 2 ml of DCE solvent and reacted at room temperature for 16 hours under 420 nm and 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent, with a yield of 80%.
[0081] NMR analysis of reaction products:
[0082] 1 H NMR (600MHz, CDCl3) δ7.84 (ddd, J=12.8, 5.1, 3.3Hz, 4H), 7.51 (td, J=7.3, 1.3Hz, 2 H),7.44(td,J=7.5,3.6Hz,4H),7.35–7.30(m,2H),6.75–6.71(m,2H),3.73(s,3H). 13C NMR(151MHz, CDCl3)δ160.5(d,J=2.2Hz),137.1(d,J=3.5Hz),133.0(s),132.6–132.1(m),1 31.6(d,J=10.2Hz), 128.5(d,J=13.1Hz), 116.0(d,J=5.2Hz), 114.8(d,J=1.7Hz), 55.28(s). 31 P NMR (243MHz, CDCl3) δ41.36 (s).
[0083] Example 7
[0084] Synthesis of m-Bromophenylthiodiphenylphosphine oxide
[0085]
[0086] 0.4 mm of diphenyl phosphine oxide, 0.2 mm of m-bromothiophenol, 1.0 mol% of 5 wt% MoO3 / g-C3N4 catalyst after radio frequency were dissolved in 2 ml of DCE solvent and reacted at room temperature for 16 hours under 420 nm and 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent. The yield was 72%.
[0087] NMR analysis of reaction products:
[0088] 1 H NMR (600MHz, CDCl3) δ7.88–7.80(m,4H),7.56–7.49(m,3H),7.48–7.42(m,5H),7.36(d,J=7.9Hz,1H),7.07(t,J=7.9Hz,1H). 13 C NMR(151MHz, CDCl3)δ137.6(d,J=3.9Hz),133.9(d,J=3.8Hz),132.7–132.4(m),132.1(d,J=2.0Hz),1 31.7(t,J=12.8Hz), 130.3(d,J=1.5Hz), 128.7(d,J=13.2Hz), 128.4(d,J=5.1Hz), 122.5(d,J=1.9Hz). 31 PNMR (243MHz,CDCl3)δ41.62(s).
[0089] Example 8
[0090] Synthesis of m-Tolylthiodiphenylphosphine Oxide
[0091]
[0092] 0.4 mm of diphenyl phosphine oxide, 0.2 mm of m-toluene thiophenol, 1.0 mol% of 5 wt% MoO3 / g-C3N4 catalyst after radio frequency were dissolved in 2 ml of DCE solvent and reacted at room temperature for 16 hours under 420 nm and 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent. The yield was 83%.
[0093] NMR analysis of reaction products:
[0094] 1 H NMR (600MHz, CDCl3) δ7.85 (ddd, J=12.9, 5.1, 3.3Hz, 4H), 7.53–7.48 (m, 2H), 7 .44(td,J=7.5,3.7Hz,4H),7.26–7.20(m,2H),7.09–7.03(m,2H),2.21(s,3H). 13 C NMR(151MHz, CDCl3)δ138.9(d,J=1.7Hz),136.0(d,J=3.8Hz),133.0(s),132.4–132.1(m),131.6(d,J =10.3Hz), 129.7(d,J=2.2Hz), 128.8(d,J=1.6Hz), 128.5(t,J=11.7Hz), 125.6(d,J=5.3Hz), 21.1(s). 31 P NMR(243MHz, CDCl3)δ41.23(s).
[0095] Example 9
[0096] Synthesis of Naphthylthiodiphenylphosphine Oxide
[0097]
[0098] 0.4 mm of diphenyl phosphine oxide, 0.2 mm of naphthiophenol, 1.0 mol% of 5 wt% MoO3 / g-C3N4 catalyst after radio frequency were dissolved in 2 ml of DCE solvent and reacted at room temperature for 16 hours under 420 nm and 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent. The yield was 78%.
[0099] NMR analysis of reaction products:
[0100] 1H NMR (600MHz, CDCl3) δ8.91–8.85(m,2H),8.09–8.03(m,2H),8.00(d,J=8.3Hz,2H),7.91–
[0101] 7.85(m,2H),7.51(td,J=6.2,3.4Hz,4H),7.46–7.41(m,2H),7.37(dd,J=8.0,1.4Hz,2H),6.97(d,J=8.0Hz,2H),2.23(s,3H). 13 C NMR (151MHz, CDCl3) δ 139.0 (d, J = 2.3Hz), 135.3 (d, J = 3.8Hz), 133.9 (d, J = 10.1Hz), 133.6 (d, J = 3.2Hz), 133.4 (d, J = 11.6Hz), 133.2 (d, J = 9.3Hz), 129.80 (d, J = 1.7Hz), 129.4 (s), 128.9–128.6 (m), 127.4–127.1 (m), 126.4 (s), 124.3 (d, J = 15.4Hz), 123.0 (d, J = 5.3Hz), 21.1 (s). 31 P NMR (243MHz, CDCl3) δ45.29 (s).
[0102] Example 10
[0103] Synthesis of Propylthiodiphenylphosphine Oxide
[0104]
[0105] 0.4 mm diphenyl phosphine oxide, 0.2 mm propyl mercaptan, 1.0 mol% RF 5 wt% MoO3 / g-C3N4 catalyst were dissolved in 2 ml DCE solvent and reacted at room temperature for 16 hours under 420 nm, 8 W light. After the reaction, the organic phase was concentrated and the product was obtained by column chromatography using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as eluent. The yield was 79%.
[0106] NMR analysis of reaction products:
[0107] 1H NMR(600MHz, CDCl3) δ7.87(ddd,J=12.9,8.2,1.2Hz,4H),7.51(dd,J=7.5,1.7Hz,2H),7.46(tdd,J =7.2,3.5,2.0Hz,4H),2.77(dt,J=10.4,7.3Hz,2H),1.64(h,J=7.3Hz,2H),0.92(t,J=7.3Hz,3H). 13 C NMR (151MHz, CDCl3) δ133.8 (s), 133.1 (s), 132.2 (d, J = 3.0Hz), 131.4 (d, J = 1 0.4Hz), 128.6 (d, J = 13.0Hz), 31.2 (d, J = 2.3Hz), 24.0 (d, J = 5.0Hz), 13.2 (s). 31 PNMR (243MHz,CDCl3)δ43.12(s).
[0108] The present invention utilizes a plasma-treated MoO3 / g-C3N4 heterojunction catalyst to generate phosphine free radicals and sulfur free radicals from a reaction substrate under light, and finally generates a target product in a one-pot method by means of free radical coupling.
[0109] Compared with the prior art, the advantages of the present invention are as follows:
[0110] 1. The present invention utilizes radio frequency plasma technology to manufacture a novel MoO3 / g-C3N4 heterojunction catalyst, thereby improving the photocatalytic activity.
[0111] 2. The reagents used in the present invention are green, environmentally friendly, cheap, highly economical, and suitable for large-scale production.
[0112] 3. The substrate used in the present invention is simple, easy to obtain and has a wide range.
[0113] 4. The reaction conditions of the present invention are mild, carried out at room temperature, no special gas is required, the equipment is simple, and it is easy to operate.
[0114] The principles and implementation methods of the present invention are described in this article using individual examples. The above implementation cases are used to help understand the methods and applications of the present invention, and also enable any technician in the field to practice the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A method for preparing a sulfur-containing phosphonate, characterized in that: The specific steps include: Adding a sulfur-containing compound, a phosphorus-containing compound and a photocatalyst MoO3 / g-C3N4 heterojunction into a solvent; The general structural formula of the phosphorus-containing compound is as follows: Wherein, R1 and R2 are independently selected from substituted or unsubstituted alkyl, substituted or unsubstituted aryl, substituted or unsubstituted heteroaryl, substituted or unsubstituted alkoxy; The general structural formula of the sulfur-containing compound is as follows: R -SH (II) Wherein, R is selected from substituted or unsubstituted alkyl, substituted or unsubstituted aryl, substituted or unsubstituted heteroaryl, substituted or unsubstituted alkoxy; The photocatalyst MoO3 / g-C3N4 heterojunction preparation method is as follows: MoO3 is subjected to radio frequency treatment in a radio frequency plasma device under an inert gas environment for 10 to 90 minutes, with the power set to 10 to 200 W, and then the treated MoO3 and g-C3N4 are dispersed together in an alcohol solution and fully dispersed, and the alcohol solution is removed by heating, and finally the mixture is calcined at 200 to 400° C. for 2 to 6 hours to obtain a radio frequency MoO3 / g-C3N4 catalyst; Under the light with a wavelength of 400 to 440 nm and a light intensity of 5 to 10 W, the reaction is fully carried out in a solvent to obtain a sulfur-containing phosphonate product, and the reaction formula is as follows:
2. The method for preparing a sulfur-containing phosphonate according to claim 1, characterized in that: The mass ratio of MoO3 to g-C3N4 in the MoO3 / g-C3N4 heterojunction is 1:49 to 1:
10.
3. The method for preparing a sulfur-containing phosphonate according to claim 1, characterized in that: In the reaction system, the molar proportions of the sulfur-containing compound, the phosphorus-containing compound and the photocatalyst MoO3 / g-C3N4 heterojunction are 50-150 molar proportions, 150-250 molar proportions and 0.5-2 molar proportions respectively.
4. The method for preparing a sulfur-containing phosphonate according to claim 1, characterized in that: The solvent is DCE solvent.
5. The method for preparing a sulfur-containing phosphonate according to claim 1, characterized in that: The reaction was carried out at room temperature under 420 nm, 8 W light for 16 hours.
6. The method for preparing a sulfur-containing phosphonate according to claim 1, characterized in that: The phosphorus-containing compounds include diphenylphosphine, di(4-methylphenyl)phosphine, di(4-methoxyphenyl)phosphine, di(4-tert-butylphenyl)phosphine, di(3,5-dimethylphenyl)phosphine, dimethyl phosphite, diethyl phosphite, diisopropyl phosphite, dibutyl phosphite, diphenyl phosphite, DOPO-(9-,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide), ethyl phenyl phosphate, and phenyl n-butylphosphine.
7. The method for preparing a sulfur-containing phosphonate according to claim 1, characterized in that: The sulfur-containing compound includes n-butyl mercaptan, cyclohexyl mercaptan, benzyl mercaptan, 2-naphthalenethiol, 4-methylthiophenol, 4-tert-butylthiophenol, 4-methoxythiophenol, 4-fluorothiophenol, 4-chlorothiophenol, 4-bromothiophenol, 2-methylthiophenol, and 3-chlorothiophenol.
8. The method for preparing a sulfur-containing phosphonate according to claim 1, characterized in that: After the reaction is completed, the solvent is removed by rotary evaporation, and the purified product is obtained by column chromatography.
9. The method for preparing a sulfur-containing phosphonate according to claim 8, characterized in that: The column chromatography uses a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1 as an eluent.
10. A MoO3 / g-C3N4 heterojunction for phosphonylation reaction after radio frequency photocatalysis, characterized in that: The preparation method is as follows: MoO3 is radio-frequency treated in a radio-frequency plasma device under an inert gas environment for 10 to 90 minutes, with the power set to 10 to 200 W. The treated MoO3 and g-C3N4 are then dispersed together in an alcohol solution and fully dispersed. The alcohol solution is removed by heating, and finally the mixture is calcined at 200 to 400°C for 2 to 6 hours to obtain a radio-frequency MoO3 / g-C3N4 catalyst.