Bimetal oxide catalyst, preparation method and application
The preparation of benzaldehyde by catalyzing styrene oxidation under low concentration hydrogen peroxide conditions by bimetallic oxide catalysts, solving the problems of complex synthesis and safety risks in traditional methods, achieving efficient and safe benzaldehyde preparation, improving the safety of the process and Reaction efficiency.
Patent Information
- Application Number
- CN202411292101.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The traditional benzaldehyde preparation method has problems such as complex synthesis process, expensive raw materials, polluting the environment and poor reaction effect. High concentration of hydrogen peroxide has safety risks in transportation and production, and low concentration of hydrogen peroxide also has the possibility of explosion during purification and transportation.
Using bimetal oxide catalysts, including support and supported active component A (such as vanadium) and promote component B (such as molybdenum), catalyzing the selective oxidation of styrene under low concentrations of hydrogen peroxide, benzaldehyde is prepared by rotary evaporation, Catalysts were prepared by vacuum drying and muffle furnace calcining, etc., and the reaction was carried out at 50-80°C.
The efficient catalytic oxidation of styrene under low concentration hydrogen peroxide is achieved, which significantly improves the safety and reaction efficiency of the process, avoids the risks of transportation and use of high concentration hydrogen peroxide, and the reaction conditions are gentle and the process is simple.
Smart Images

Figure CN119075973A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalyst materials, and in particular relates to a bimetallic oxide catalyst and a preparation method and application thereof. Background Art
[0002] Benzaldehyde, as an important organic intermediate, has been widely used in the chemical industry, and has a wide range of applications in the fragrance, dye, medicine and agriculture industries. Traditional methods for preparing benzaldehyde include toluene chlorination and hydrolysis, toluene oxidation, benzyl alcohol oxidation, benzoic acid hydrogenation reduction and indirect electrooxidation, but these methods have many disadvantages, such as complex synthesis process, expensive raw materials, environmental pollution and poor reaction effect. In recent years, the method of preparing benzaldehyde by direct oxidation of styrene under the action of green oxidant hydrogen peroxide has attracted widespread attention.
[0003] As an environmentally friendly oxidant, hydrogen peroxide is highly valued by researchers around the world. It has low requirements for reaction conditions, a simple process and is harmless to the environment, and can effectively promote the oxidation reaction of carbon-carbon double bonds. Despite this, high-concentration hydrogen peroxide poses safety risks in transportation and production. For example, its irritation and corrosiveness to tissues may cause harm to personnel. At present, there are technical barriers to the direct production of high-concentration hydrogen peroxide, and low-concentration hydrogen peroxide also faces dangers during the purification process, and there is also the possibility of explosion during transportation and storage. Therefore, it is particularly important to explore how to safely and effectively use low-concentration hydrogen peroxide as an oxidant to synthesize fine chemicals.
[0004] At present, low-concentration hydrogen peroxide has been widely used in fields such as polysaccharide oxidation, gel and pulp bleaching, and medical disinfection. However, in the catalytic oxidation preparation of fine chemicals, such as the preparation of benzaldehyde from styrene, standard 30% concentration hydrogen peroxide is still commonly used. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to provide a bimetallic oxide catalyst and its preparation method and application, which can catalyze the selective oxidation of styrene to prepare benzaldehyde under the catalytic action of relatively low concentration of hydrogen peroxide; and has the characteristics of mild reaction conditions and simple preparation method.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solution:
[0007] A bimetallic oxide catalyst comprises a carrier and a metal oxide of an active component A and a metal oxide of a promoting component B loaded on the carrier; the carrier is one of Al2O3, TiO2, and SiO2; the active component A is at least any one of silver, vanadium, iron, and copper, preferably vanadium; the promoting component B is selected from at least any one of cobalt, cerium, tungsten, and molybdenum, preferably molybdenum.
[0008] Furthermore, the loading amount of the active component A is 0-20% of the carrier mass, preferably 8-12%; the loading amount of the promoting component B is 0-20% of the carrier mass, preferably 8-12%.
[0009] The present invention provides a method for preparing the above-mentioned bimetallic oxide catalyst, comprising the following steps:
[0010] The ammonium salts corresponding to the active component A and the promoting component B are dissolved in an aqueous solution, added to the carrier for impregnation, and after rotary evaporation, the obtained powder is dried in a vacuum drying oven and calcined in a muffle furnace to obtain the bimetallic oxide catalyst AB / carrier.
[0011] Furthermore, the loading conditions of the active component A and the promoting component B are mixing and stirring at 60-80° C. and immersing for 9-12 hours.
[0012] Furthermore, the rotary evaporation temperature is 70-80°C, the calcination temperature is 400-600°C, preferably 550°C, and the calcination time is 4-5h.
[0013] In the preparation of the bimetallic oxide catalyst, the molar ratio of the active component A to the promoting component B is 1:3 to 3:1.
[0014] The present invention also proposes the use of the above-mentioned bimetallic oxide catalyst in the in-situ oxidation of styrene using low-concentration hydrogen peroxide to prepare benzaldehyde. Specifically, under the action of the above-mentioned bimetallic oxide catalyst, low-concentration hydrogen peroxide is used as an oxidant to selectively oxidize styrene to prepare benzaldehyde.
[0015] The present invention provides a method for preparing benzaldehyde by in-situ oxidation of styrene using low-concentration hydrogen peroxide. Under the action of the bimetallic oxide catalyst as described above, low-concentration hydrogen peroxide is used as an oxidant to selectively oxidize styrene to prepare benzaldehyde.
[0016] Furthermore, in the above method, the concentration of the low-concentration hydrogen peroxide is 5-10%.
[0017] Furthermore, in the above method, the oxidation temperature of styrene oxidation by low concentration hydrogen peroxide is 50-80°C; and the molar ratio of styrene to hydrogen peroxide is 1:2 to 1:3.
[0018] Furthermore, the dosage of the bimetallic oxide catalyst is 6.33 mg per mole of styrene through orthogonal experiment screening.
[0019] The principle of the catalytic reaction of the bimetallic oxide catalyst of the present invention (taking the Mo-V combination as an example): the vanadium catalyst contains active sites and can react with hydrogen peroxide (H2O2) to form highly active peroxy species, which can undergo selective oxidation reaction with styrene to generate benzaldehyde. According to existing literature records, there is a strong synergistic effect between vanadium and molybdenum. In the preparation process of the catalyst, the interaction between the active species and the carrier can be adjusted by controlling the synthesis method, and the surface state of the catalyst can be optimized, thereby obtaining a mesostructure catalyst system with superior performance. It is speculated that it is this strong synergistic effect that can greatly improve the generation efficiency of peroxy species, so that styrene can also achieve a higher catalytic oxidation efficiency under low concentration hydrogen peroxide conditions.
[0020] Compared with the prior art, the present invention has the following beneficial effects: the present invention relates to a solid bimetallic oxide catalyst, and the process of selectively oxidizing styrene to prepare benzaldehyde in low-concentration hydrogen peroxide is in the form of liquid-solid phase reaction, styrene is in liquid under reaction conditions, and the styrene liquid undergoes oxidation reaction on the surface of the multiphase catalyst without the risk of polymerization blockage, and low-concentration hydrogen peroxide is used as an oxidant in the reaction situ, which effectively solves a series of problems existing in the transportation and use of high-concentration hydrogen peroxide, and significantly improves the intrinsic safety of the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the catalytic performance evaluation results of the catalysts prepared in Examples 1-5 of the present invention;
[0022] Figure 2 This is a schematic diagram of the catalytic performance evaluation results of the catalysts prepared in Examples 6-10 of the present invention;
[0023] Figure 3 Schematic diagram of the catalytic performance evaluation results of the catalysts prepared in Examples 11-14 of the present invention. DETAILED DESCRIPTION
[0024] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0025] Example 1
[0026] (1) Preparation of bimetallic oxide catalysts
[0027] 0.4086g (NH4)2MoO4 and 0.4592g NH4(VO)3 were added to a beaker (wherein the molar ratio Mo:V = 10:10), 30ml of deionized water was added, and 2g of commercial SiO2 (500nm) was added after washing in an ultrasonic bath for 5min. After rotary evaporation at 70-80℃, the obtained powder was dried overnight at 70℃ in a vacuum drying oven and calcined in a muffle furnace at 400℃ for 4 hours. Catalyst Mo was obtained. 10 V 10 / SiO2-400, grind to 40-60 mesh for later use.
[0028] (2) Evaluation of catalyst
[0029] The catalytic reaction was carried out in a round-necked flask equipped with a condenser. The reaction conditions were as follows: 17.398 mmol of styrene, 10 ml of acetonitrile and 110 mg of catalyst were stirred at 70°C for about 10 min, and then 49.017 mmol of H2O2 (10%) was added. After heating and stirring for more than 9 h on a heating device equipped with a magnetic stirrer, the collected samples were qualitatively and quantitatively analyzed by GC-MS for the reaction products. The results are as follows: Figure 1 shown.
[0030] Embodiment 2-5
[0031] (1) Preparation of bimetallic oxide catalysts
[0032] 0.4086g (NH4)2MoO4 and 0.4592g NH4(VO)3 were added into a beaker (wherein the molar ratio Mo:V=10:10), 30ml deionized water was added, and 2g commercial SiO2 (500nm) was added after washing in an ultrasonic bath for 5min. After rotary evaporation at 70-80℃, the obtained powder was dried overnight at 70℃ in a vacuum drying oven and calcined in a muffle furnace at 450, 500, 550, and 600℃ for 4 hours, respectively. Catalyst Mo was obtained, respectively. 10 V 10 / SiO2-450、Mo 10 V 10 / SiO2-500、Mo 10 V 10 / SiO2-550、Mo 10 V 10 / SiO2-600, grind to 40-60 mesh for later use.
[0033] (2) Evaluation of catalyst
[0034] The catalyst evaluation method of Examples 2-5 is the same as that of Example 1, and the results are as follows: Figure 1 Example 6
[0035] (1) Preparation of bimetallic oxide catalysts
[0036] 0.8172g (NH4)2MoO4 was added to a beaker (wherein the molar ratio Mo:V = 20:0), 30ml of deionized water was added, and 2g of commercial SiO2 (500nm) was added after washing in an ultrasonic bath for 5min. After rotary evaporation at 70-80℃, the obtained powder was dried overnight at 70℃ in a vacuum drying oven and calcined in a muffle furnace at 550℃ for 4 hours. Catalyst Mo was obtained. 20 / SiO2-550, grind to 40-60 mesh for later use.
[0037] (2) Evaluation of catalyst
[0038] The catalyst evaluation method of Example 6 is the same as that of Example 1, and the results are as follows: Figure 2 shown.
[0039] Example 7
[0040] (1) Preparation of bimetallic oxide catalysts
[0041] 0.6129g (NH4)2MoO4 and 0.2296g NH4(VO)3 were added to a beaker (wherein the molar ratio Mo:V = 15:5), 30ml of deionized water was added, and 2g of commercial SiO2 (500nm) was added after washing in an ultrasonic bath for 5min. After rotary evaporation at 70-80℃, the obtained powder was dried overnight at 70℃ in a vacuum drying oven and calcined in a muffle furnace at 550℃ for 4 hours. Catalyst Mo was obtained. 15 V5 / SiO2-550, grind to 40-60 mesh for later use.
[0042] (2) Evaluation of catalyst
[0043] The catalyst evaluation method of Example 7 is the same as that of Example 1, and the results are as follows: Figure 2 Shown
[0044] Example 8
[0045] (1) Preparation of bimetallic oxide catalysts
[0046] 0.4086g (NH4)2MoO4 and 0.4592g NH4(VO)3 were added into a beaker (wherein the molar ratio Mo:V=10:10), 30ml deionized water was added, and 2g commercial SiO2 (500nm) was added after washing in an ultrasonic bath for 5min. After rotary evaporation at 70-80℃, the obtained powder was dried overnight at 70℃ in a vacuum drying oven and calcined in a muffle furnace at 550℃ for 4 hours. Catalyst Mo was obtained. 10 V 10 / SiO2-550, grind to 40-60 mesh for later use.
[0047] (2) Evaluation of catalyst
[0048] The catalyst evaluation method of Example 8 is the same as that of Example 1, and the results are as follows: Figure 2 shown.
[0049] Example 9
[0050] (1) Preparation of bimetallic oxide catalysts
[0051] 0.2043g (NH4)2MoO4 and 0.6888g NH4(VO)3 were added to a beaker (wherein the molar ratio Mo:V = 5:15), 30ml of deionized water was added, and 2g of commercial SiO2 (500nm) was added after washing in an ultrasonic bath for 5min. After rotary evaporation at 70-80℃, the obtained powder was dried overnight at 70℃ in a vacuum drying oven and calcined in a muffle furnace at 550℃ for 4 hours. The catalyst Mo5V 15 / SiO2-550, grind to 40-60 mesh for later use.
[0052] (2) Evaluation of catalyst
[0053] The catalyst evaluation method of Example 9 is the same as that of Example 1, and the results are as follows: Figure 2 Shown
[0054] Example 10
[0055] (1) Preparation of bimetallic oxide catalysts
[0056] 0.9184 g NH4(VO)3 was added to a beaker (wherein the molar ratio Mo:V=0:20), 30 ml of deionized water was added, and 2 g of commercial SiO2 (500 nm) was added after washing in an ultrasonic bath for 5 min. After rotary evaporation at 70-80°C, the obtained powder was dried overnight at 70°C in a vacuum drying oven and calcined in a muffle furnace at 550°C for 4 hours. Catalyst V was obtained. 20 / SiO2-550, grind to 40-60 mesh for later use.
[0057] (2) Evaluation of catalyst
[0058] The catalyst evaluation method of Example 10 is the same as that of Example 1, and the results are as follows: Figure 2 Shown
[0059] Examples 11-14
[0060] (1) Preparation of bimetallic oxide catalysts
[0061] The catalyst preparation method of Examples 11-14 is the same as that of Example 8.
[0062] 2) Evaluation of catalyst
[0063] The catalytic reaction was carried out in a round-necked flask equipped with a condenser. The reaction conditions were as follows: 17.398 mmol of styrene, 10 ml of acetonitrile and 110 mg of catalyst were stirred at 50, 60, 70 and 80 °C for about 10 min, then 49.017 mmol of H2O2 (10%) was added, and after heating and stirring for more than 9 h on a heating device equipped with a magnetic stirrer, the collected samples were qualitatively and quantitatively analyzed by GC-MS for the reaction products. The results are as follows: Figure 3 shown.
[0064] Examples 15-23
[0065] The substrate range is expanded to include a variety of aromatic olefins. Under the conditions of the catalyst and low concentration of hydrogen peroxide, they can all be oxidized to carbonyl-containing compounds, as shown in Table 1 below, where the catalyst used and the reaction conditions are similar to those in Example 8.
[0066] Table 1 Conversion rate and carbonyl compound selectivity of extended substrates in Examples 15-23
[0067]
[0068]
[0069] From the above Figure 1-3 It can be seen that the method for preparing benzaldehyde by oxidizing styrene with low-concentration hydrogen peroxide in situ of the present invention achieves efficient conversion of styrene in a laboratory round-necked flask, with a conversion rate of more than 70% and a benzaldehyde selectivity of more than 80%. The conversion rate of styrene and the selectivity of benzaldehyde can be optimized by adjusting the composition of the catalyst active components or adjusting the calcination temperature of the catalyst and the oxidation reaction temperature parameters as needed. Comparing Examples 1-14, it can be seen that Example 8 is the best catalyst preparation method and the best reaction parameters, with a styrene conversion rate of 96.11% and a benzaldehyde selectivity of 87.82%. In addition, it can be seen from the above table that the catalyst prepared by the present invention is also applicable to some other aromatic olefins.
[0070] Although the present invention is described in detail through the above preferred embodiments, these descriptions should not be regarded as constraints on the present invention. Under the guidance of this specification, those skilled in the art should be able to identify the possibility of making appropriate modifications or adjustments to the present invention. These potential modifications or adjustments, as long as they do not exceed the definition of the claims of the present invention, should be regarded as reasonable extensions of the present invention.
Claims
1. A bimetallic oxide catalyst, It is characterized in that The invention comprises a carrier and a metal oxide of an active component A and a metal oxide of a promoting component B loaded on the carrier; the carrier is Al 2 O 3 、TiO 2 、SiO 2 The active component A is at least one of silver, vanadium, iron and copper; the promoting component B is at least one of cobalt, cerium, tungsten and molybdenum.
2. A bimetallic oxide catalyst according to claim 1, It is characterized in that The loading amount of the active component A is 8-12% of the carrier mass; the loading amount of the promoting component B is 8-12% of the carrier mass.
3. The method for preparing the bimetallic oxide catalyst according to claim 1 or 2, It is characterized in that The steps include: The ammonium salts corresponding to the active component A and the promoting component B are dissolved in an aqueous solution, added to the carrier for impregnation, and after rotary evaporation, the obtained powder is dried in a vacuum drying oven and calcined in a muffle furnace to obtain the bimetallic oxide catalyst AB / carrier.
4. The method for preparing the bimetallic oxide catalyst according to claim 3, It is characterized in that The loading conditions of the active component A and the promoting component B are mixing and stirring at 60-80° C. and immersing for 9-12 hours.
5. The method for preparing the bimetallic oxide catalyst according to claim 3, It is characterized in that The rotary evaporation temperature is 70-80°C, the calcination temperature is 400-600°C, and the calcination time is 4-5h.
6. The method for preparing the bimetallic oxide catalyst according to claim 3, It is characterized in that The molar ratio of the active component A to the promoting component B is 1:3 to 3:
1.
7. Use of the bimetallic oxide catalyst as claimed in claim 1 or 2 in the in-situ oxidation of styrene using low concentration hydrogen peroxide to prepare benzaldehyde, It is characterized in that Under the action of the bimetallic oxide catalyst described in claim 1 or 2, low-concentration hydrogen peroxide is used as an oxidant to selectively oxidize styrene to prepare benzaldehyde.
8. A method for preparing benzaldehyde by in-situ oxidation of styrene using low concentration hydrogen peroxide. It is characterized in that Under the action of the bimetallic oxide catalyst described in claim 1 or 2, low-concentration hydrogen peroxide is used as an oxidant to selectively oxidize styrene to prepare benzaldehyde.
9. The method for preparing benzaldehyde by in-situ oxidation of styrene using low-concentration hydrogen peroxide according to claim 8, It is characterized in that The concentration of the low-concentration hydrogen peroxide is 5-10%.
10. The method for preparing benzaldehyde by in-situ oxidation of styrene using low-concentration hydrogen peroxide according to claim 8, It is characterized in that The oxidation temperature of styrene oxidized by low-concentration hydrogen peroxide is 50-80° C.; the molar ratio of styrene to hydrogen peroxide is 1:2 to 1:3.
Citation Information
Patent Citations
Process for preparing benzaldehyde by catalytic oxidation of phenylethene
CN101306986A
Method for oxidizing styrene
CN102850207A
Molybdenum-vanadium double-metal oxide catalyst and application of same to chemical-chain dehydrogenation of light alkanes
CN109382090A
Process for one step preparation of benzaldehyde by selective oxidation of toluene
CN1827575A
Method of preparing formaldehyde by catalytic selection oxidation of ethylene
CN1948254A