Preparation method of ruthenium cluster modified titanium oxide coated titanium nitride material for photocatalytic methane dry reforming
The titanium oxide-coated titanium nitride material is modified through ruthenium clusters, which solves the problem of low dry reforming efficiency of photocatalytic methane, achieves efficient and stable adsorption and catalysis of methane and carbon dioxide, and improves the production efficiency of synthesis gas and catalysts. stability.
Patent Information
- Application Number
- CN202411287023.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing photocatalytic methane dry reforming technology is inefficient and the material has weak adsorption capacity to methane and carbon dioxide, making it difficult to achieve efficient synthesis gas production.
The titanium oxide-coated titanium nitride material is modified by ruthenium clusters, and the ruthenium clusters are loaded on the partially oxidized titanium nitride material through photodeposition method to enhance its adsorption ability to methane and carbon dioxide, and improve the material through titanium oxide coating. stability and electron transfer efficiency.
Highly efficient and highly stable photocatalytic dry reforming of methane under mild conditions is achieved, which significantly improves the activation ability of methane and carbon dioxide and the cycling stability of the catalyst.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to a ruthenium cluster-modified titanium oxide-coated titanium nitride material for photocatalytic methane dry reforming, belonging to the field of nanomaterials and photocatalytic technology. Background Art
[0002] Combined conversion of two greenhouse gases, methane and carbon dioxide, into synthesis gas (H 2 and CO), namely the methane dry reforming (DRM) reaction, has recently attracted widespread attention in the field of catalysis. The methane dry reforming reaction is highly endothermic and must be carried out at high temperatures above 1073 K. In addition, carbon deposition is also a serious problem in the DRM reaction. Compared with traditional thermal catalytic methane dry reforming, photocatalysis can enable the reaction to proceed under relatively mild conditions, which is a green, environmentally friendly, non-toxic and low-energy way to prepare synthesis gas. However, the efficiency of photocatalytic methane dry reforming is still far below the requirements of practical applications, so it is necessary to develop efficient and stable methane dry reforming photocatalysts.
[0003] TiN is an ideal photocatalytic material with the advantages of strong light absorption, non-toxicity, no secondary pollution, low cost, and long-term stability. However, it lacks catalytic active sites and has poor activity in the photocatalytic methane dry reforming reaction. In addition, TiN has a weak adsorption capacity for carbon dioxide and methane molecules, and photogenerated carriers are prone to recombination, making it difficult to achieve efficient production of syngas. Currently, there is little research on photocatalytic transition metal nitride materials, and the use of TiN for photocatalytic methane dry reforming reactions remains to be explored.
[0004] Therefore, based on the above research background, from the perspective of constructing active sites and improving stability, the present invention prepared a titanium nitride material coated with titanium oxide modified by ruthenium clusters, and simultaneously combined the material with other metal-loaded titanium oxide-coated titanium nitride materials and unmodified TiN and TiO 2 The materials were systematically compared. On the one hand, the modified ruthenium clusters can enhance the adsorption capacity of methane and carbon dioxide and promote the activation of methane and carbon dioxide. On the other hand, TiO 2 The coating of materials can enhance the electron transfer between TiN and Ru, while stabilizing the Ru clusters deposited on the surface, thereby improving the stability.
[0005] The ruthenium cluster modified titanium oxide coated titanium nitride material prepared by the present invention realizes efficient and highly stable photocatalytic methane dry reforming under mild conditions. Summary of the invention
[0006] The present invention uses a photodeposition method to load ruthenium in the form of clusters in a partially oxidized titanium nitride material. First, commercial titanium nitride is rinsed with a mixed solution of hydrogen peroxide and ammonia to remove surface antioxidants, and then the titanium nitride powder is subjected to programmed temperature oxidation, and then cooled to room temperature to prepare a partially oxidized titanium nitride material. The partially oxidized titanium nitride material is then added to a 1:1 ethanol mixture of ruthenium chloride and stirred for 30 minutes, and then 2000 mW / cm -2 After irradiation with high intensity light for 30 min and multiple centrifugal drying, the ruthenium cluster-modified titanium oxide-coated titanium nitride material can be obtained.
[0007] The method for preparing titanium nitride used in the present invention is as follows: 200 mg of commercial nano-TiN is soaked in 10 ml of a 1:1 mixed solution of hydrogen peroxide and ammonia for 10 min, then rinsed with deionized water and ethanol for multiple times, and dried by an infrared lamp under an argon atmosphere to obtain TiN powder.
[0008] The method for partially oxidizing titanium nitride used in the present invention is as follows: 400 mg of commercial titanium nitride is placed in a porcelain ark, calcined at 350 ° C for 1 h in a muffle furnace at a heating rate of 5 ° C / min, and then cooled to room temperature to collect the powder, which is recorded as TiN@TiO 2 .
[0009] The method for constructing a ruthenium cluster-modified titanium oxide-coated titanium nitride material according to the present invention is as follows: 200 mgTiN@TiO 2 Dispersed in a mixture of 15 mL ethanol and 15 mL water, then added with ruthenium chloride solution, stirred for 30 min, and then used 2000 mW / cm -2 The solution was irradiated with strong light for 30 min. The sample was then washed three times with a mixed solution of ethanol and water at a ratio of 1:1, and then placed in a 70 °C oven for 8 h to obtain the finished product TiN@TiO 2 -Ru.
[0010] The method for preparing partially oxidized titanium nitride materials loaded with different metals involved in the present invention is as follows: porous titanium silicon materials loaded with other metals are prepared according to the method for loading ruthenium clusters, and ruthenium trichloride is replaced with chloroplatinic acid and chloroauric acid respectively.
[0011] The method for preparing different carrier materials loaded with ruthenium clusters according to the present invention is as follows: 200 mg of metal oxide is dispersed in 30 mL of water, and then a ruthenium trichloride solution is added and stirred for 4 h. Then, it is washed three times with deionized water, dried, calcined in a muffle furnace at 400 ° C for 1 h, and the heating rate is 5 ° C / min. Then, it is cooled to room temperature and the powder is collected to obtain different carriers loaded with ruthenium clusters.
[0012] Titanium nitride, a typical metal nitride, is used as a photocatalytic semiconductor. It has similar optical properties to precious metals such as Au and Ag in the optical range, and exhibits a unique localized plasma resonance effect (LSPR) and absorption capacity of the entire solar spectrum. At the same time, titanium nitride also has a strong photothermal effect, which can convert infrared light that is difficult to use with traditional semiconductor materials into thermal energy, increase the temperature of the catalytic site, and facilitate the photocatalytic methane dry reforming reaction.
[0013] The partially oxidized titanium nitride forms a titanium nitride core-titanium oxide shell structure, that is, the titanium oxide coating is conducive to the stability of titanium nitride under high temperature and oxidizing atmosphere, thereby maintaining the structure of the catalyst unchanged and improving the stability of the photothermal methane dry reforming reaction.
[0014] Loading ruthenium in the form of clusters on titanium oxide-coated titanium nitride can improve the material's adsorption capacity for methane and carbon dioxide, thereby promoting activation.
[0015] By designing this structure, the titanium oxide intermediate layer and Ru clusters can enhance the absorption of light through a synergistic effect, promote the separation and migration of photogenerated carriers, and increase the lifetime of photogenerated carriers. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 a is a TEM image of titanium nitride in Example 1, and its diameter is about 30-80 nm. Figure 1 b is the TEM image of partially oxidized titanium nitride in Example 2. It can be seen that there is an obvious oxide layer on the surface of the oxidized sample, which belongs to anatase TiO 2 . Figure 1 c is TiN@TiO in Example 3 2 -Ru(1%) sample, it can be clearly seen that the morphology of the sample has no obvious change after loading Ru, and the Ru clusters are evenly dispersed in the TiO 2 surface, and its size is 0.95nm. Figure 1 d is the XRD pattern of the Ru cluster modified TiN samples with different oxidation degrees in Example 3. The peaks at 36.6°, 42.59°, 61.81°, 74.07°, and 93.17° correspond to the (111), (200), (220), (311), and (222) crystal planes of titanium nitride (JCPDS No. 98-000-0339), respectively. The peak at 25.3° corresponds to the (101) crystal plane of anatase titanium oxide (JCPDS No. 98-000-0081). No peaks of Ru clusters were observed, confirming the high dispersion of Ru. Figure 1e is the BET diagram of the Ru cluster-modified TiN samples with different oxidation degrees in Example 3. It can be seen that the H1-type hysteresis loop confirms that the material is a particle aggregate with relatively uniform size.
[0017] Figure 2 a is the photocatalytic DRM activity diagram of TiN materials with different proportions of Ru loaded under a 300 W xenon lamp. The TiN sample showed no catalytic activity, CO and H 2 The generation rate of CO shows a volcanic trend with the increase of Ru loading, and the activity is optimal when the Ru loading is 1%, indicating that Ru is a CO 2 and CH 4 The main active sites of activation. 2 The increase in CO and H 2 The generation rate also shows a volcanic trend, which means that only suitable TiN and TiO 2 The ratio can further promote the methane dry reforming reaction ( Figure 2 b). Figure 2 c is TiN@TiO under different light intensities 2 -Ru(1%) photocatalytic DRM activity diagram. It can be seen that with the increase of light intensity, its H 2 The CO production rate increased synchronously, confirming the light-driven nature of the reaction. To confirm the importance of metal Ru and TiN materials, Figure 2 d shows the photocatalytic DRM activity results of TiN materials loaded with different metal elements and other oxide materials loaded with Ru. Compared with the Ru-loaded sample, the Pt-loaded TiN material only showed weak DRM activity. 2 and Al 2 O 3 The above activity tests prove that Ru loading and titanium nitride support synergistically improve the photocatalytic DRM reaction performance. Compared with other metals, Ru loading can 2 and CH 4 In order to explore the stability of the catalyst, TiN-Ru (1%) and TiN@TiO 2 -Ru(1%) for photocatalytic methane dry reforming cycle stability test ( Figure 2 e and Figure 2 f). The results show that after 20 h, the catalytic rate only decreased by 6%, compared with TiN@TiO 2 -Ru (1%) and TiN-Ru (1%) decreased significantly (25%), indicating that TiN@TiO 2 -Ru(1%) catalyst has good cycling stability.
[0018] Figure 3 a and Figure 3 b TiN, TiN-Ru (1%) and TiN@TiO 2 CO of -Ru(1%) sample 2 -TPD and CH 4 -TPD spectrum. It can be seen that the Ru cluster is CO 2 and CH 4 The main adsorption site of TiO 2 Played a role in CH 4 Supplementary adsorption effect. Figure 3 cf is TiN@TiO 2 -Ru (1%) in situ XPS test, we can see that after illumination, N, Ti, and O have obvious positive shifts, and the negative shift of Ru is more obvious, because the content of Ru is much smaller than that of N, Ti, and O. The above results confirm that electrons will migrate from TiN to TiO 2 Finally, the Ru sites are enriched, and the titanium oxide intermediate layer plays an important role in electron transport, thereby improving the photocatalytic activity.
[0019] Figure 4 a is TiN, TiO 2 and TiN@TiO 2 -Ru(1%) UV-visible diffuse reflectance spectrum shows that TiN has very strong light absorption ability, which not only has strong absorption in the visible region, but also can absorb in the near-infrared region. Although partial oxidation and loading of Ru reduce the partial light absorption of the sample, the sample still maintains the absorption ability of a wide spectrum. Figure 4 b is TiN, TiO 2 and TiN@TiO 2 -Ru(1%) material transient photocurrent spectrum, TiN@TiO 2 -Ru(1%) has a strong photocurrent response, which indicates that Ru loading and TiO 2 Modifying the sample can facilitate the separation of photogenerated charges. Figure 4 cf is TiN, TiO 2 and TiN@TiO 2 -Electrochemical impedance spectroscopy of Ru(1%) materials, Ru loading and TiO 2 The modified samples showed lower electrochemical impedance, which means that the Ru clusters and TiO 2 The intermediate layer reduces the material's electron transfer barrier and helps to improve the mobility of photogenerated carriers. Figure 4 g and Figure 4 h is TiN, TiO 2 and TiN@TiO 2-Ru(1%) material fluorescence emission and time-resolved fluorescence lifetime diagram. The lower fluorescence intensity means that TiN@TiO 2 -Ru(1%) sample's photogenerated electrons and holes are not easy to recombine; TiN@TiO 2 The longer fluorescence lifetime of the -Ru(1%) sample indicates that its photogenerated carriers have a longer lifetime. This indicates that the Ru loading and TiO 2 Modifying samples can promote the separation and migration of photogenerated charges, thereby improving catalytic activity.
[0020] The above experimental results prove that the Ru cluster-loaded titanium oxide-modified titanium nitride material we synthesized has excellent photocatalytic DRM performance and stability.
[0021] Although the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Specific implementation plan
[0022] The present invention will be described in more detail below through specific embodiments, but the protection scope of the present invention is not limited to these embodiments. Example 1
[0023] Synthesis of Titanium Nitride
[0024] Commercial nano-TiN was soaked in a mixed solution of hydrogen peroxide and ammonia for 10 min, then rinsed with deionized water and ethanol for multiple times, and dried by an infrared lamp under an argon atmosphere to obtain TiN powder. Example 2
[0025] Synthesis of Partially Oxidized Titanium Nitride
[0026] 400 mg TiN was placed in a porcelain ark and calcined at 350 °C for 1 h in a muffle furnace with a heating rate of 5 °C / min. The powder was then cooled to room temperature and collected, which was recorded as TiN@TiO 2 . Example 3
[0027] Synthesis of Ruthenium Cluster-supported Titanium Oxide-coated Titanium Nitride Materials
[0028] 200 mg TiN@TiO 2 Disperse in 15 mL of ethanol and 15 mL of water, stir for 30 min, then add ruthenium chloride solution, continue to stir the mixed solution for 30 min, and then use 300 W xenon lamp to irradiate the solution for 1 h (2000 mW / cm -2The sample was then washed three times with a mixed solution of ethanol and water in a ratio of 1:1, and then placed in a 70 °C oven for 8 h to obtain the finished product TiN@TiO 2 -Ru. Comparative Example 1
[0029] Synthesis of Titanium Dioxide Materials
[0030] 400 mg TiN was placed in a porcelain ark and calcined at 500 °C for 4 h in a muffle furnace with a heating rate of 5 °C / min. The powder was then cooled to room temperature and recorded as TiO 2 . Comparative Example 2
[0031] Synthesis of Ruthenium-supported Titanium Dioxide Materials
[0032] 200 mg TiO 2 Disperse in 15 mL of ethanol and 15 mL of water, stir for 30 min, then add ruthenium chloride solution, continue to stir the mixed solution for 30 min, and then use 300 W xenon lamp to irradiate the solution for 1 h (2000 mW / cm -2 The sample was then washed three times with a mixed solution of ethanol and water (1:1), and then placed in a 70 °C oven for 8 h to obtain the finished TiO 2 -Ru. Comparative Example 3
[0033] Synthesis of Ruthenium-supported Titanium Nitride Materials
[0034] 200 mg of commercial TiN was dispersed in 15 mL of ethanol and 15 mL of water and stirred for 30 min. Then, ruthenium chloride solution was added. The mixed solution was stirred for another 30 min and then illuminated with a 300 W xenon lamp for 1 h (2000 mW / cm -2 ). The reacted sample was then washed three times with a mixed solution of ethanol: water = 1:1, and then placed in a 70 °C oven for 8 h to obtain the finished product TiN-Ru. Comparative Example 4
[0035] Synthesis of Ruthenium-supported Metal Oxide Materials
[0036] 200 mg Al 2 O 3 and SiO 2 Disperse in 30 mL of water, then add ruthenium trichloride solution and stir for 4 h. Then wash it three times with deionized water, dry it, place it in a muffle furnace and calcine it at 400 °C for 1 h, with a heating rate of 5 °C / min, then cool it to room temperature and collect the powder to obtain the finished Al2 O 3 -Ru、SiO 2 -Ru. Comparative Example 5
[0037] Titanium nitride coated with titanium oxide (TiN@TiO 2 -M) Synthesis of Materials
[0038] 200 mg TiN@TiO 2 The mixture was dispersed in 15 mL of ethanol and 15 mL of water and stirred for 30 min. Then, chloroplatinic acid and chloroauric acid solutions were added respectively. The mixed solution was stirred for another 30 min and then illuminated with a 300 W xenon lamp for 1 h (2000 mW / cm -2 The sample was then washed three times with a mixed solution of ethanol and water (1:1), and then placed in a 70 °C oven for 8 h to obtain the finished product TiN@TiO 2 -M (M=Pt, Au). Experiments and data
[0039] The activity investigation method of photocatalytic methane dry reforming provided by the present invention is as follows:
[0040] 10 mg of catalyst was placed in a flow photothermal catalytic reaction device (PLR-PTSR II) and heated at 10 mL min -1 The flow rate of CH 4 : CO 2 A mixed gas of Ar: Ar (volume ratio of 5:5:90) was introduced into the reaction device. The adsorption saturation was maintained for 30 minutes under dark conditions, and then the activity test was carried out under simulated light of a 300 W xenon lamp. The photothermal reaction temperature during illumination was kept constant at 300 °C by the temperature control component, and the pressure was kept constant at 0.3 MPa. The outlet of the reaction device was connected to a gas chromatograph, and the reaction products were detected in automatic injection mode. A flame ionization detector was used to detect CO, and a flame ionization detector was used to detect H 2 The detection was carried out using a thermal conductivity detector.
Claims
1. A method for preparing a ruthenium cluster-modified titanium oxide-coated titanium nitride material for photocatalytic methane dry reforming, characterized in that For commercial titanium nitride materials, a surface titanium oxide coating layer is prepared by temperature-controlled calcination to achieve partial oxidation of titanium nitride, and then Ru clusters are deposited in an ethanol solution containing ruthenium trichloride by controlling the light intensity, and finally washed and dried to obtain a ruthenium cluster-modified titanium oxide-coated titanium nitride material; The prepared material has excellent light energy utilization and methane and carbon dioxide adsorption capabilities, and can show good photocatalytic methane dry reforming performance; The specific steps include: Step 1: 200 mg of commercial nano-TiN was soaked in 10 ml of a 1:1 mixture of hydrogen peroxide and ammonia for 10 min, then rinsed with deionized water and ethanol several times, and dried with an infrared lamp under an argon atmosphere to obtain TiN powder; Step 2: 400 mg of TiN powder treated in the first step was placed in a porcelain ark and calcined at 350 °C for 1 h in a muffle furnace at a heating rate of 5 °C / min. The powder was then cooled to room temperature and collected, which was recorded as TiN@TiO2. Step 3: Disperse 200 mg TiN@TiO2 in 15 ml ethanol and 15 ml water, stir for 30 min, then add ruthenium chloride solution, stir the mixed solution for 30 min, and illuminate the solution with 300 W xenon lamp for 1 h (2000 mW / cm -2 ); then the sample after the reaction was washed three times with a mixed solution of ethanol: water = 1:1, and then placed in a 70 °C oven for 8 h to obtain the finished product TiN@TiO2-Ru; Step 4: Prepare other metal-loaded TiN@TiO2 according to the methods of the first two steps, and replace ruthenium trichloride with chloroplatinic acid and chloroauric acid respectively.
2. The method for preparing the ruthenium cluster modified titanium oxide coated titanium nitride material according to claim 1, characterized in that: In the first step, a 1:1 hydrogen peroxide:ammonia solution mixture is used to remove the anti-oxidation protective agent on the surface of commercial nano-TiN.
3. The method for preparing the ruthenium cluster modified titanium oxide coated titanium nitride material according to claim 1, characterized in that: In the second step, the calcination temperature is 350°C, the purpose of which is to control the crystal form of the surface oxide layer to be anatase titanium oxide.
4. The method for preparing the ruthenium cluster modified titanium oxide coated titanium nitride material according to claim 1, characterized in that: In the second step, the calcination holding time is 1 h and the heating rate is 5 °C / min. The purpose is to control the calcination time to obtain titanium oxide-coated titanium nitride material with suitable oxidation thickness.
5. The method for preparing the ruthenium cluster modified titanium oxide coated titanium nitride material according to claim 1, characterized in that: In the third step, a 1:1 ethanol: water mixed solution is used to ensure the successful dispersion of TiN@TiO2 material. Different alcohol-water ratios will affect the subsequent Ru deposition.
6. The method for preparing the ruthenium cluster modified titanium oxide coated titanium nitride material according to claim 1, characterized in that: In the third step, a light intensity of 2000 mW / cm -2 Xenon lamp irradiation is used to ensure that the deposited Ru is a cluster structure.
Citation Information
Patent Citations
Preparation method and application of Au-Pt co-modified carbon nitride for efficient photocatalysis of methane non-oxidative coupling reaction
CN113649041A
Ru-based photocatalyst for carbon dioxide hydrogenation methanation reaction as well as preparation method and application thereof
CN113713808A
Platinum-cluster-loaded mesoporous black titanium dioxide nanosheet photocatalyst and preparation method thereof
CN115254097A