Stripping agent of zinc oxide concentrate surface flotation reagent as well as preparation method and application of stripping agent
By using surfactant stripping agent composed of dodecyl ammonium sulfate, butylene glycol, propylene oxide, and neopentyl glycol dioctyl ester, the foaming and blistering of low-grade oxidation mixed lead-zinc ore during acidic leaching is solved and The problem of TOC exceeding the standard has achieved effective removal of ore surface reagents and improved the stability of the smelting process.
Patent Information
- Application Number
- CN202411072582.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Low-grade oxidation sulfur mixed lead-zinc ore is difficult to enter the existing smelting process, and the oxidized ore is wrapped and vulcanized by flotation reagent after mixed flotation, resulting in bubble generation during acid leaching and TOC exceeding the standard, affecting the problem of rough surface of zinc sheets and difficult to peel off .
Using a release agent composed of dodecyl ammonium sulfate, butylene glycol, propylene oxide, and neopentyl glycol dioctyl ester, a surfactant is formed through specific proportions and process preparation methods, and the flotation of the surface of the adsorbent ore particles is fed Reagents and improve bubbles during acidic leaching to reduce the TOC content in the leaching solution.
Effectively remove the flotation agent remaining on the surface of zinc oxide concentrate, improve the bubble phenomenon during acidic leaching, and reduce the TOC content in the leaching solution, improve the flatness of the surface of zinc sheets and the stability of the smelting process.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lead-zinc ore dressing, and in particular relates to a stripping agent for zinc oxide concentrate surface flotation reagent, and a preparation method and application thereof. Background Art
[0002] Ping lead-zinc mine has the largest single lead-zinc mineral resources in China and the fifth largest in the world. After years of "mining the rich and abandoning the poor", the mining area has accumulated 40 million tons of low-grade oxygen-sulfur mixed lead-zinc ore (grade Zn6.5%, Pb1.58%, zinc metal content 2.1356 million tons, lead metal content 492,000 tons), accounting for one-third of the current geological reserves. Due to the difficulty of processing and low grade, this mineral has never been effectively developed.
[0003] Based on many years of previous research, low-grade oxygen-sulfur mixed stockpiles can be mixed with oxygen-sulfur mixed concentrates through mixed flotation, which has good economic efficiency and process stability. There are two key technical difficulties in the smelting application of this mixed concentrate: (1) Because it is a mixture of oxygen and sulfur, it is difficult to enter the existing smelting process; (2) After mixed flotation, the oxidized ore is coated and sulfided by the flotation reagents (xanthate, No. 2 oil, sodium lignin sulfonate, octadecylamine, etc.), and the existing mineral processing technology is difficult to separate oxygen and sulfur.
[0004] When the oxide ore obtained after the oxygen-sulfur separation process is directly subjected to acid leaching, bubbles will be generated and the TOC in the leachate will exceed the standard. When TOC exceeds the standard, the zinc flake surface will be rough and difficult to peel off during the electrolysis stage. In order to solve the above problems, the flotation reagents remaining on the surface of the zinc oxide concentrate are stripped in advance, which can improve the foaming phenomenon during acid leaching and reduce the TOC content in the leachate. Summary of the invention
[0005] The first object of the present invention is to provide a stripping agent for flotation reagents remaining on the surface of zinc oxide concentrate; the second object of the present invention is to provide a method for preparing the stripping agent; the third object of the present invention is to provide the use of the stripping agent in removing flotation reagents remaining on the surface of zinc oxide concentrate.
[0006] The first object of the present invention is achieved as follows: the stripping agent comprises, by mass, 30 to 40 parts of ammonium lauryl sulfate, 10 to 20 parts of butanediol, 20 to 25 parts of propylene oxide, 30 to 35 parts of neopentyl glycol dicaprylate, and 40 to 46 parts of water.
[0007] The second object of the present invention is achieved by: the preparation method of the stripping agent comprises the following steps: Step 1: 40-46 parts of water, 30-40 parts of ammonium dodecyl sulfate, and 10-20 parts of butanediol are added to a reaction kettle in sequence, and heated while stirring until the temperature of the reactants in the kettle rises to 35-45° C. to obtain solution a.
[0008] Step 2: Add 20 to 25 parts of propylene oxide to solution a, and stir the reaction at room temperature for 1.5 to 2.5 hours to obtain solution b.
[0009] Step 3: Add 30-35 parts of neopentyl glycol dicaprylate to solution b, stir and react at room temperature for 3-5 hours to obtain solution c.
[0010] Step 4: The pH value of solution c is adjusted to 4-5, and then solution c is ultrasonically emulsified at 40-45° C. for 20-40 min, and then cooled to room temperature to obtain the target stripping agent.
[0011] The third object of the present invention is achieved by: using the stripping agent to remove the flotation agent remaining on the surface of the zinc oxide concentrate, adding the stripping agent in an amount of 2-5 to the zinc oxide concentrate slurry and stirring for 40-45 minutes.
[0012] Compared with the prior art, the technical solution of the present invention has outstanding substantial features and significant progress in the following aspects: the stripping agent is formed by compounding ammonium dodecyl sulfate, butanediol, propylene oxide, and neopentyl glycol dioctanoate. The stripping agent is added to the zinc oxide concentrate slurry. The stripping agent has good surface activity, and the flotation reagents remaining on the surface of the ore particles will be adsorbed and enter the groups of the stripping agent. After filter pressing, the stripping agent carries the mineral processing reagents on the surface of the ore particles and separates them from the oxide ore with the aqueous solution. The stripping agent can improve the foaming phenomenon of the slurry during acid leaching, and at the same time reduce the TOC content in the leachate. DETAILED DESCRIPTION
[0013] The present invention is further described below, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.
[0014] The stripping agent of the zinc oxide concentrate surface flotation reagent of the present invention comprises, by mass, 30-40 parts of dodecyl ammonium sulfate, 10-20 parts of butanediol, 20-25 parts of propylene oxide, 30-35 parts of neopentyl glycol dicaprylate, and 40-46 parts of water.
[0015] The stripping agent preferably comprises, by mass, 32 parts of ammonium lauryl sulfate, 16 parts of butanediol, 23 parts of propylene oxide, 32 parts of neopentyl glycol dicaprylate, and 43 parts of water.
[0016] The pH value of the stripping agent is 4-5, preferably 4.5.
[0017] The preparation method of the stripping agent comprises the following steps: Step 1: 40-46 parts of water, 30-40 parts of ammonium dodecyl sulfate, and 10-20 parts of butanediol are added to a reaction kettle in sequence, and heated while stirring until the temperature of the reactants in the kettle rises to 35-45° C. to obtain solution a.
[0018] Step 2: Add 20 to 25 parts of propylene oxide to solution a, and stir the reaction at room temperature for 1.5 to 2.5 hours to obtain solution b.
[0019] Step 3: Add 30-35 parts of neopentyl glycol dicaprylate to solution b, stir and react at room temperature for 3-5 hours to obtain solution c.
[0020] Step 4: The pH value of solution c is adjusted to 4-5, and then solution c is ultrasonically emulsified at 40-45° C. for 20-40 min, and then cooled to room temperature to obtain the target stripping agent.
[0021] The heating rate in step 1 is 3-6°C / min.
[0022] The reaction time in step 2 is preferably 2 h.
[0023] The reaction time in step 3 is preferably 4 h.
[0024] The ultrasonic emulsification time in step 4 is preferably 30 minutes.
[0025] The stripping agent is used in removing the flotation reagent on the surface of zinc oxide concentrate. In the sorting stage, the stripping agent is added into the zinc oxide concentrate pulp in an amount of 2-5, and stirred at 20-30° C. for 40-45 minutes.
[0026] Example 1 The stripping agent of the zinc oxide concentrate surface flotation reagent comprises 35 g of dodecyl ammonium sulfate, 15 g of butanediol, 22 g of propylene oxide, 35 g of neopentyl glycol dioctanoate, and 43 g of water, and the pH value is 4.5.
[0027] The preparation method of the stripping agent is: Step 1: Add 43 g of water, 35 g of ammonium dodecyl sulfate and 15 g of butanediol into a reaction kettle in sequence, heat with stirring at a rate of 5°C / min until the temperature of the reactants in the kettle reaches 40°C to obtain a uniform solution a.
[0028] Step 2: Slowly drop 22 g of propylene oxide into solution a, and stir the reaction at room temperature for 2 h to obtain solution b.
[0029] Step 3: Slowly drop 35 g of neopentyl glycol dicaprylate into solution b, and stir the reaction at room temperature for 4 h to obtain solution c.
[0030] Step 4: The pH value of solution c was adjusted to 4.5, and then solution c was ultrasonically emulsified at 42° C. for 30 min, and then cooled to room temperature to obtain the target stripping agent.
[0031] The application method of the stripping agent is: The prepared stripping agent was added into the zinc oxide concentrate slurry in an amount of 4 and stirred at 25°C for 40 minutes.
[0032] Example 2 The stripping agent of the zinc oxide concentrate surface flotation reagent comprises 30 g of dodecyl ammonium sulfate, 12 g of butanediol, 25 g of propylene oxide, 33 g of neopentyl glycol dioctanoate, and 40 g of water, and the pH value is 4.
[0033] The preparation method of the stripping agent is: Step 1: Add 40 g of water, 30 g of ammonium dodecyl sulfate and 12 g of butanediol into a reaction kettle in sequence, heat with stirring at a rate of 4°C / min until the temperature of the reactants in the kettle reaches 45°C to obtain a uniform solution a.
[0034] Step 2: Slowly drop 25 g of propylene oxide into solution a, and stir the reaction at room temperature for 2.5 h to obtain solution b.
[0035] Step 3: Slowly drop 33 g of neopentyl glycol dicaprylate into solution b, and stir the reaction at room temperature for 5 h to obtain solution c.
[0036] Step 4: The pH value of solution c was adjusted to 4, and then solution c was ultrasonically emulsified at 45° C. for 20 min, and then cooled to room temperature to obtain the target stripping agent.
[0037] The application method of the stripping agent is: In the sorting stage, the prepared stripping agent was added into the zinc oxide concentrate slurry in an amount of 3 and stirred at 28°C for 45 minutes.
[0038] Example 3 The stripping agent of the zinc oxide concentrate surface flotation reagent comprises 40 g of dodecyl ammonium sulfate, 20 g of butanediol, 20 g of propylene oxide, 30 g of neopentyl glycol dioctanoate, and 40 g of water, and the pH value is 5.
[0039] The preparation method of the stripping agent is: Step 1: Add 40 g of water, 40 g of ammonium dodecyl sulfate and 20 parts of butanediol into a reaction kettle in sequence, heat with stirring at a rate of 4°C / min until the temperature of the reactants in the kettle reaches 35°C to obtain a uniform solution a.
[0040] Step 2: Slowly drop 20 g of propylene oxide into solution a, and stir the reaction at room temperature for 1.5 h to obtain solution b.
[0041] Step 3: Slowly drop 30 g of neopentyl glycol dicaprylate into solution b, and stir the reaction at room temperature for 3 h to obtain solution c.
[0042] Step 4: The pH value of solution c was adjusted to 5, and then solution c was ultrasonically emulsified at 40° C. for 40 min, and then cooled to room temperature to obtain the target stripping agent.
[0043] The application method of the stripping agent is: In the sorting stage, the prepared stripping agent was added into the zinc oxide concentrate slurry in an amount of 2 and stirred at 30°C for 42 minutes.
[0044] Example 4 ——Comparison example
[0045] The stripping agent used as a control example contains 25 g of ammonium dodecyl sulfate, 25 g of butanediol, 30 g of propylene oxide, 25 g of neopentyl glycol dicaprylate, and 55 g of water, and has a pH value of 4.5.
[0046] The preparation method of the stripping agent is: Step 1: Add 55 g of water, 25 g of ammonium dodecyl sulfate and 25 g of butanediol into a reaction kettle in sequence, and heat while stirring. The heating rate is the same as in Example 1, until the temperature of the reactants in the kettle rises to 40° C. to obtain a uniform solution a.
[0047] Step 2: Slowly drop 30 g of propylene oxide into solution a, and stir the reaction at room temperature for 2 h to obtain solution b.
[0048] Step 3: Slowly drop 25 g of neopentyl glycol dicaprylate into solution b, and stir the reaction at room temperature for 4 h to obtain solution c.
[0049] Step 4: The pH value of solution c was adjusted to 4.5, and then solution c was ultrasonically emulsified at 42° C. for 30 min, and then cooled to room temperature to obtain a peeling agent as a control example.
[0050] The application method of the stripping agent is the same as that of Example 1.
[0051] Example 5 ——Comparison of the application effects of the stripping agents prepared in Examples 1, 2, 3 and the control example
[0052] The application method of the stripping agent uniformly adopts the values in Example 1. The TOC content in the leachate is determined using the HJ501-2009 (Determination of total organic carbon in water quality - combustion oxidation-non-dispersive infrared absorption method) standard. The results are shown in the following table: .
Claims
1. A stripping agent for zinc oxide concentrate surface flotation reagent, characterized in that: The stripping agent comprises, by mass, 30-40 parts of ammonium lauryl sulfate, 10-20 parts of butanediol, 20-25 parts of propylene oxide, 30-35 parts of neopentyl glycol dicaprylate, and 40-46 parts of water.
2. The stripping agent according to claim 1, characterized in that The stripping agent comprises, by mass, 30-40 parts of ammonium lauryl sulfate, 10-20 parts of butanediol, 20-25 parts of propylene oxide, 30-35 parts of neopentyl glycol dicaprylate, and 40-46 parts of water.
3. The stripping agent according to claim 1, characterized in that The pH value of the stripping agent is 4-5.
4. A method for preparing the stripping agent according to claim 1, characterized in that The following steps are involved: Step 1: 40-46 parts of water, 30-40 parts of ammonium dodecyl sulfate, and 10-20 parts of butanediol are added to a reaction kettle in sequence, and heated while stirring until the temperature of the reactants in the kettle rises to 35-45° C. to obtain solution a; Step 2: Add 20-25 parts of propylene oxide to solution a, and stir the reaction at room temperature for 1.5-2.5 hours to obtain solution b; Step 3: Add 30-35 parts of neopentyl glycol dicaprylate to solution b, and stir the mixture at room temperature for 3-5 hours to obtain solution c; Step 4: The pH value of solution c is adjusted to 4-5, and then solution c is ultrasonically emulsified at 40-45° C. for 20-40 min, and then cooled to room temperature to obtain the target stripping agent.
5. The preparation method according to claim 4, characterized in that: The heating rate in step 1 is 3-6°C / min.
6. The preparation method according to claim 4, characterized in that: The reaction time in step 2 is 2 h.
7. The preparation method according to claim 4, characterized in that: The reaction time in step 3 is 4 h.
8. The preparation method according to claim 4, characterized in that: The ultrasonic emulsification time in step 4 is 30 minutes.
9. Use of the stripping agent according to claim 1 in removing flotation reagents from the surface of zinc oxide concentrate, characterized in that: During the sorting stage, add 2-5% of the stripping agent into the zinc oxide concentrate slurry and stir at 20-30℃ for 40-45min.
Citation Information
Patent Citations
method FOR TREATMENT OF ZINC ORE LEACH RESIDUES
BE829988A
Selection method of high mud lead zinc oxide sulfur mixed ores
CN105013601A
Beneficiation method of micro-fine particle zinc oxide ore
CN106540815A
Method for recovering zinc sulfide through flotation of zinc oxide and leaching residues in acid leaching oxygen-sulfur mixed zinc concentrate
CN116555565A
Method for producing high-purity nanometer zinc oxide from low-grade zinc oxide ore by ammonia decarburization
WO2014047762A1