Rivet mounting method based on thin product in progressive die
The rivet installation method for thin-material products in progressive dies addresses the force deficiencies by creating an inclined rivet hole with a chamfer or arc, improving torque and force consistency while facilitating easy rivet insertion and adaptability.
Patent Information
- Application Number
- CN202411201985.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
Existing progressive dies struggle to meet the push-out force, pull-out force, and torque requirements during riveting of thin-material products due to shallow interference fits, necessitating frequent adjustments of rivet bottom hole diameters, which is inefficient and resource-intensive.
A rivet installation method involving punching a smaller rivet bottom hole, forming an inclined hole with a chamfer or arc, and pressing the rivet downward to ensure a secure fit, increasing torque, push-out force, and pull-out force while allowing easy rivet insertion.
Enhances torque, push-out force, and pull-out force, ensuring stable rivet installation with reduced manual effort and adaptability to different rivet specifications, thus optimizing the riveting process for thin-material products.
Smart Images

Figure CN119076873A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stamping dies, and in particular to a rivet installation method based on a thin material product in a progressive die. Background Art
[0002] At present, during the riveting process of the product, the progressive die has high requirements for the push-out force, pull-out force and torque after the product is riveted. When the raw material of the product is relatively thin, the above three forces are difficult to meet.
[0003] like Figure 1-Figure 2 As shown in the figure, the principle of the punch riveting process is to use the pattern under the rivet cap to make an interference fit with the process hole on the thin product. First, punch out the rivet bottom hole on the product to place the rivet, use the machine tool and the stamping die to squeeze the rivet into the rivet bottom hole, and bite the pattern on the rivet and the stamped product together to complete the punch riveting process. However, when the raw material of the stamped product is relatively thin, the pattern under the rivet cap and the product bite shallowly, resulting in the punch riveting related forces (push-out force, pull-out force, torque) not meeting the requirements.
[0004] When the force related to punching and riveting cannot meet the requirements, the usual adjustment method is to adjust the diameter of the rivet bottom hole of the stamped product, reducing its diameter to reduce the gap between the rivet and the bottom hole, but usually the amount that can be adjusted is very small, because too small a bottom hole will make it difficult for workers to put the rivet into the bottom hole during operation. In addition, different products require different rivet models. Every time a new product is developed, the diameter of the rivet bottom hole needs to be re-adjusted, which wastes manpower and material resources. Summary of the invention
[0005] In order to solve the deficiencies of the above technical solutions, the object of the present invention is to provide a rivet installation method for thin-material products in a progressive die.
[0006] The purpose of the present invention is achieved through the following technical solutions.
[0007] A rivet installation method for thin-material products in a progressive die comprises the following steps:
[0008] Step 1, punching a rivet bottom hole from top to bottom on a thin product with a first punch, wherein the diameter of the rivet bottom hole is smaller than the diameter of the rivet to be installed on the product;
[0009] Step 2, placing a second punch just below the rivet bottom hole, placing a die just above the rivet bottom hole, the groove of the die facing the rivet bottom hole, a chamfer or arc is provided at the connection between the inner wall of the groove and the bottom surface of the die, and punching the rivet bottom hole from bottom to top with the second punch, the outer edge of the rivet bottom hole is tilted upward to form an inclined rivet bottom hole, wherein the diameter of the second punch is larger than the diameter of the rivet and smaller than the inner diameter of the die;
[0010] Step 3, placing the rivet above the bottom hole of the inclined rivet, and pressing the rivet downward with the progressive die. Under the action of the pressure, the material at the edge of the bottom hole of the inclined rivet flows and becomes flat, and the rivet is bitten.
[0011] In the above technical solution, in step 1, the thickness of the thin product is 0.5 to 1.5 mm.
[0012] In the above technical solution, in step 1, the difference between the diameter of the rivet bottom hole and the diameter of the rivet is 0.7 to 1.3 mm.
[0013] In the above technical solution, in step 2, the difference between the diameter of the second punch and the diameter of the rivet is 0.1 to 0.3 mm.
[0014] In the above technical solution, in step 2, the difference between the diameter of the second punch and the inner diameter of the die is 0.6 to 1.60 mm.
[0015] The advantages and beneficial effects of the present invention are:
[0016] After the rivet is manually placed in the bottom hole of the inclined rivet, the material at the edge of the bottom hole of the inclined rivet flows and becomes flat under the action of pressure, and the rivet is bitten, and the values of the related torque, push-out force and pull-out force are increased, and the stability of the product is very good. Based on this, while ensuring the related torque, push-out force and pull-out force after the rivet is finally installed, a hole with a larger diameter can be punched, so that it is convenient to put the rivet in during manual punching and riveting, and the method is applicable to installing rivets of different specifications on different products. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a thin product after punching by the rivet process in the background technology.
[0018] Figure 2 It is a thin product after rivets are installed using the rivet process in the background technology.
[0019] Figure 3 FIG. 1 is a process diagram of step 1 in the embodiment.
[0020] Figure 4 This is a process diagram of step 2 in Example 1.
[0021] Figure 5 This is a process diagram of step 2 in Example 2.
[0022] Figure 6 3 is a process diagram of step 3 in the embodiment.
[0023] Among them, 1: thin product, 2: rivet bottom hole, 3: first punch, 4: die, 5: inclined rivet bottom hole, 6: rivet, 7: second punch, 8: chamfer, 9: guide arc, 10: groove. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0025] The diameter of the rivet required for the thin product described below is 5mm.
[0026] Example 1 (the diameter of the rivet required in this example is 5 mm)
[0027] like Figure 2-Figure 6 As shown, a rivet installation method based on a thin product 1 in a progressive die comprises the following steps:
[0028] Step 1, use a 4.0 mm first punch 3 to punch a rivet bottom hole 2 with a diameter of 4.0 mm from top to bottom on a 1.0 mm thick thin product 1.
[0029] Step 2, place a second punch 7 with a diameter of 5.10 mm just below the rivet bottom hole 2, and place a die 4 with an inner diameter of 6.2 mm just above the rivet bottom hole 2, the groove 10 of the die 4 is opposite to the rivet bottom hole 2, and a chamfer 8 is set at the connection between the inner wall of the groove 10 and the bottom surface of the die 4 (i.e., the contact surface between the die 4 and the thin product 1), and use the second punch 7 to punch the rivet bottom hole 2 from bottom to top, and the edge of the rivet bottom hole 2 is tilted upward to form an inclined rivet bottom hole 5 with an inner diameter of 5.10 mm.
[0030] Step 3, the rivet 6 is placed above the inclined rivet bottom hole 5, and the progressive die presses the rivet downward. Under the action of pressure, the material at the edge of the inclined rivet bottom hole 5 flows and becomes flat, and the rivet is bitten.
[0031] After testing, the torque of the rivet of this embodiment is greater than 7.6Nm, the push-out force is greater than 600N, and the pull-out force is greater than 4.5kN, which meets the product processing requirements.
[0032] Example 2 (the diameter of the rivet required in this example is 5 mm)
[0033] like Figure 2-Figure 6 As shown, a rivet installation method based on a thin product 1 in a progressive die comprises the following steps:
[0034] Step 1, use a 4.0 mm first punch 3 to punch a rivet bottom hole 2 with a diameter of 4.0 mm from top to bottom on a 1.0 mm thick thin product 1.
[0035] Step 2, place a second punch 7 with a diameter of 5.10 mm just below the rivet bottom hole 2, and place a die 4 with an inner diameter of 6.2 mm just above the rivet bottom hole 2, the groove 10 of the die 4 is opposite to the rivet bottom hole 2, and a chamfer 8 is set at the connection between the inner wall of the groove 10 and the bottom surface of the die 4 (i.e., the contact surface between the die 4 and the thin product 1), and use the second punch 7 to punch the rivet bottom hole 2 from bottom to top, and the edge of the rivet bottom hole 2 is tilted upward to form an inclined rivet bottom hole 5 with an inner diameter of 5.10 mm.
[0036] Step 3, the rivet 6 is placed above the inclined rivet bottom hole 5, and the progressive die presses the rivet downward. Under the action of pressure, the material at the edge of the inclined rivet bottom hole 5 flows and becomes flat, and the rivet is bitten.
[0037] Example 3 (the diameter of the rivet required in this example is 7 mm)
[0038] A rivet installation method based on a thin product 1 in a progressive die comprises the following steps:
[0039] Step 1, use a 6.0 mm first punch 3 to punch a rivet bottom hole 2 with a diameter of 6.0 mm from top to bottom on a 1.0 mm thick thin product 1.
[0040] Step 2, place a second punch 7 with a diameter of 7.10 mm just below the rivet bottom hole 2, and place a die 4 with an inner diameter of 8.2 mm just above the rivet bottom hole 2, the groove 10 of the die 4 is opposite to the rivet bottom hole 2, and an arc guide 9 is provided at the connection between the inner wall of the groove 10 and the bottom surface of the die 4 (i.e., the contact surface between the die 4 and the thin product 1), and use the second punch 7 to punch the rivet bottom hole 2 from bottom to top, and the edge of the rivet bottom hole 2 is tilted upward to form a bevel rivet bottom hole 5 with an inner diameter of 7.10 mm.
[0041] Step 3, the rivet 6 is placed above the inclined rivet bottom hole 5, and the progressive die presses the rivet downward. Under the action of pressure, the material at the edge of the inclined rivet bottom hole 5 flows and becomes flat, and the rivet is bitten.
[0042] For ease of explanation, spatial relative terms such as "upper", "lower", "left", "right" and the like are used in the embodiments to illustrate the relationship of one element or feature shown in the figure relative to another element or feature. It should be understood that, in addition to the orientation shown in the figure, the spatial terms are intended to include different orientations of the device in use or operation. For example, if the device in the figure is inverted, the element described as being "under" other elements or features will be positioned "on" other elements or features. Therefore, the exemplary term "under" can include both upper and lower orientations. The device can be positioned in other ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here can be interpreted accordingly.
[0043] Furthermore, relational terms such as “first” and “second” and the like are merely used to distinguish one component from another having the same name, but do not necessarily require or imply any such actual relationship or order between these components.
[0044] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.
Claims
1. A rivet installation method for thin products in a progressive die, characterized in that: The following steps are involved: Step 1, punching a rivet bottom hole from top to bottom on a thin product with a first punch, wherein the diameter of the rivet bottom hole is smaller than the diameter of the rivet to be installed on the product; Step 2, placing a second punch just below the rivet bottom hole, placing a die just above the rivet bottom hole, the groove of the die facing the rivet bottom hole, a chamfer or arc is provided at the connection between the inner wall of the groove and the bottom surface of the die, and punching the rivet bottom hole from bottom to top with the second punch, the outer edge of the rivet bottom hole is tilted upward to form an inclined rivet bottom hole, wherein the diameter of the second punch is larger than the diameter of the rivet and smaller than the inner diameter of the die; Step 3, placing the rivet above the bottom hole of the inclined rivet, and pressing the rivet downward with the progressive die. Under the action of the pressure, the material at the edge of the bottom hole of the inclined rivet flows and becomes flat, and the rivet is bitten.
2. The installation method according to claim 1, characterized in that: In the step 1, the thickness of the thin product is 0.5 to 1.5 mm.
3. The installation method according to claim 1, characterized in that: In step 1, the difference between the diameter of the rivet bottom hole and the diameter of the rivet is 0.7 to 1.3 mm.
4. The installation method according to claim 1, characterized in that: In step 2, the difference between the diameter of the second punch and the diameter of the rivet is 0.1 to 0.3 mm.
5. The installation method according to claim 1, characterized in that: In step 2, the difference between the diameter of the second punch and the inner diameter of the die is 0.6 to 1.60 mm.
Citation Information
Patent Citations
Full-automatic punching riveting system and working process thereof
CN108838316A
Moving plate machining method and moving plate machined through moving plate machining method
CN112974639A
Novel riveting and stamping structure
CN215908845U
Apparatus designed to make openings for driven rivets in thin sheet metal.
FR855374A
Method for joining metal component and method for manufacturing joint component
JP2022115534A