Preparation method of gold nanosheet

By using polyvinylpyrrolidone and hydrogen peroxide at room temperature, gold nanosheets with good biocompatibility and adjustable optical absorption characteristics were prepared, solving the biotoxicity and cumbersome steps of surfactant in the prior art. The problem has achieved application in the biological field.

CN119076965APending Publication Date: 2024-12-06XUZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411209820.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing gold nanosheet preparation methods, the commonly used surfactant CTAB or CTAC is biotoxic and requires heating the solution or preparing the seed crystal solution in advance. The steps are cumbersome, which limits its application in the biological field.

Method used

Polyvinylpyrrolidone (PVP) is used as a stabilizer to prepare gold nanosheets through the reduction reaction of hydrogen peroxide and sodium hydroxide at room temperature, avoiding the need to prepare seed crystal solutions in advance and strictly control the reaction temperature, making it easy to operate.

Benefits of technology

The prepared gold nanosheets have good biocompatibility, the optical absorption peak position can be adjusted, and the size can reach 1 micron. They are suitable for surface-enhanced Raman scattering, plasma refractive index sensors, saturable absorbers, photothermal therapy and Organic degradation and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076965A_ABST
    Figure CN119076965A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of gold nanosheets. The preparation method comprises the following specific steps: preparing a polyvinylpyrrolidone solution, a chloroauric acid solution, a sodium borohydride solution and a sodium hydroxide solution; uniformly mixing polyvinylpyrrolidone and a chloroauric acid solution; then adding hydrogen peroxide, uniformly mixing and shaking, then adding a sodium borohydride solution or a sodium hydroxide solution, and standing at room temperature for 8-24 hours; the optical absorption peak position of the prepared gold nanosheet ranges from 790 nm to 970 nm, and the maximum size of the gold nanosheet can reach 1 micrometer. The invention provides a method for conveniently preparing a gold nanosheet with biocompatibility. In addition, the invention further provides a method for regulating and controlling the optical absorption peak position of the gold nanosheet in a large range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano material preparation, and particularly relates to a method for preparing a gold nano sheet. Background Art

[0002] Gold nanosheets show good anisotropy and excellent localized surface plasmon resonance performance because their lateral size is greater than their thickness. By controlling the raw material concentration, the lateral size of the gold nanosheets can be adjusted to obtain a tunable light absorption peak. Gold nanosheets play an important role in surface enhanced Raman scattering, plasma refractive index sensors, saturable absorbers, photothermal therapy, organic matter degradation and other fields.

[0003] At present, it has been reported that the method commonly used to prepare gold nanosheets is a wet chemical method based on reduction reaction. CTAB or CTAC is usually used as a surfactant to reduce gold ions in a solution. However, CTAB or CTAC surfactants usually have certain biological toxicity, which limits certain applications of gold nanosheets prepared using CTAB or CTAC in the biological field. According to reports, polyvinyl pyrrolidone (PVP) is used as a stabilizer to prepare metal nanoparticles, which have good biocompatibility. There are many related reports, such as Colloids and Surfaces A2020,594,124652; Journal of Materials Chemistry 2010,20,6176; and so on. At the same time, there are also reports on the use of PVP polymers to prepare gold nanosheets. However, in the process of preparing gold nanosheets using PVP, it is usually necessary to heat the solution, which makes the preparation steps more cumbersome. Recently, there have been reports on the preparation of gold nanosheets using PVP polymer at room temperature (Chem. Commun., 2016, 52, 398.). However, this method requires the preparation of a seed solution in advance, and the steps are relatively cumbersome. Summary of the invention

[0004] The invention aims to provide a method for preparing gold nanosheets, which method does not require the preparation of a seed solution in advance and does not require strict control of the reaction temperature, and is relatively convenient to operate.

[0005] To achieve the above object, the technical solution adopted by the present invention is as follows: a method for preparing gold nanosheets, the specific steps are:

[0006] Step 1: prepare polyvinyl pyrrolidone solution, chloroauric acid solution, sodium borohydride solution and sodium hydroxide solution respectively;

[0007] Step 2: Add polyvinyl pyrrolidone solution and chloroauric acid solution into a centrifuge tube and mix well;

[0008] Step 3: Add hydrogen peroxide solution to the mixed solution of step 2, mix and shake well, then quickly add sodium borohydride solution or sodium hydroxide solution; let stand at room temperature for 8-24 hours, and obtain gold nanosheets after centrifugation and washing.

[0009] Preferably, in step 1, the concentration of the polyvinyl pyrrolidone solution is 2 mM, the concentration of the chloroauric acid solution is 5 mM, the concentration of the sodium borohydride solution is 5 mM, and the concentration of the sodium hydroxide solution is 50 mM.

[0010] Preferably, in step 2, the molar ratio of polyvinyl pyrrolidone to chloroauric acid is (0.08-1):1.

[0011] More preferably, in step 2, the molar ratio of polyvinyl pyrrolidone to chloroauric acid is 0.4:1.

[0012] Preferably, in step three, the molar ratio of hydrogen peroxide, sodium borohydride and chloroauric acid is (12-60):(0.02-0.1):1.

[0013] Preferably, in step three, the molar ratio of hydrogen peroxide, sodium hydroxide and chloroauric acid is (12-60):(0.06-0.6):1.

[0014] In the present invention, hydrogen peroxide reduces trivalent gold ions to obtain monovalent gold ions, and sodium borohydride reduces trivalent gold ions to obtain smaller gold particles. Monovalent gold ions continue to deposit on the surface of smaller gold particles, and PVP polymer plays a role in regulating the growth of atoms along special crystal planes and preventing particle aggregation, thereby obtaining gold nanosheets with better dispersibility. In the process of preparing micron sheets, smaller gold particles are generated in the solution after sodium hydroxide is added, and monovalent gold ions obtained by reducing trivalent gold ions with hydrogen peroxide continue to deposit on the surface of smaller gold particles, and PVP polymer plays a role in regulating the growth of atoms along special crystal planes and preventing particle aggregation, thereby obtaining gold micron sheets. Using sodium hydroxide instead of sodium borohydride slows down the reaction rate and prolongs the reaction time, thereby obtaining nanosheets with larger side lengths, and the side length size can reach 1 micron.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. The present invention adopts PVP to prepare gold nanosheets, and the prepared gold nanosheets have good biocompatibility.

[0017] 2. The present invention does not require the preparation of seed solution in advance, and does not require strict control of the growth temperature, and the operation is simpler.

[0018] 3. The present invention can regulate the optical absorption peak position by the content of hydrogen peroxide solution in the system, and the optical absorption peak position of the prepared gold nanosheet is located at 790-970nm. The size of the gold nanosheet can reach up to 1 micron. The gold nanosheet prepared by the present invention can be used in the fields of surface enhanced Raman scattering, plasma refractive index sensor, saturable absorber, photothermal therapy, organic degradation, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a scanning electron microscope image of the gold nanosheets prepared in Example 1 of the present invention.

[0020] Figure 2 This is the optical absorption spectrum of the gold nanosheets prepared in Example 1 of the present invention.

[0021] Figure 3 This is the optical absorption spectrum of the gold nanosheets prepared in Example 2 of the present invention.

[0022] Figure 4 This is the optical absorption spectrum of the gold nanosheets prepared in Example 3 of the present invention.

[0023] Figure 5 This is the optical absorption spectrum of the gold nanosheets prepared in Example 4 of the present invention.

[0024] Figure 6 This is a scanning electron microscope image of the gold nanosheets prepared in Example 6 of the present invention.

[0025] Figure 7 This is the optical absorption spectrum of the gold nanosheets prepared in Example 6 of the present invention.

[0026] Figure 8 This is the optical absorption spectrum of the gold nanosheets prepared in Example 7 of the present invention. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0028] The hydrogen peroxide solution used in the following examples is a commercially available product with a mass concentration of 30%.

[0029] Example 1

[0030] Step 1: prepare 2 mM polyvinyl pyrrolidone solution, 5 mM chloroauric acid solution and 5 mM sodium borohydride solution respectively;

[0031] Step 2: Add 4.7 mL of pure water, 0.5 mL of polyvinyl pyrrolidone solution, and 0.5 mL of chloroauric acid solution into a centrifuge tube; the molar ratio between the polyvinyl pyrrolidone and chloroauric acid is 0.4:1;

[0032] Step 3: Add 3 μL of hydrogen peroxide solution to the mixture in step 2, shake gently to mix, and quickly add 10 μL of sodium borohydride; after standing at room temperature for 8-24 hours, centrifuge and wash to obtain gold nanosheets, and evenly disperse them in a pure water solution for storage.

[0033] Figure 1 The scanning electron microscope image of the gold nanosheet prepared in Example 1 is shown, and it can be seen that the size of the gold nanosheet is about 80-160 nm and the thickness is about 8 nm.

[0034] Figure 2 The figure shows the optical absorption spectrum of the gold nanosheets prepared in Example 1. It can be seen that the optical absorption peak of the gold nanosheets prepared in this example is around 970 nm.

[0035] Example 2

[0036] Step 1: prepare 2 mM polyvinyl pyrrolidone solution, 5 mM chloroauric acid solution and 5 mM sodium borohydride solution respectively;

[0037] Step 2: Add 4.7 mL of pure water, 0.5 mL of polyvinyl pyrrolidone solution, and 0.5 mL of chloroauric acid solution into a centrifuge tube; the molar ratio between the polyvinyl pyrrolidone and chloroauric acid is 0.4:1;

[0038] Step 3: Add 11 μL of hydrogen peroxide solution to the mixture in step 2, shake gently to mix, and quickly add 10 μL of sodium borohydride; after standing at room temperature for 8-24 hours, centrifuge and wash to obtain gold nanosheets, and evenly disperse them in a pure water solution for storage.

[0039] Figure 3 The figure shows the optical absorption spectrum of the gold nanosheets prepared in Example 2. It can be seen that the optical absorption peak of the gold nanosheets prepared in this example is around 850nm.

[0040] Example 3

[0041] Step 1: prepare 2 mM polyvinyl pyrrolidone solution, 5 mM chloroauric acid solution and 5 mM sodium borohydride solution respectively;

[0042] Step 2: Add 4.7 mL of pure water, 0.5 mL of polyvinyl pyrrolidone solution, and 0.5 mL of chloroauric acid solution into a centrifuge tube; the molar ratio between the polyvinyl pyrrolidone and chloroauric acid is 0.4:1;

[0043] Step 3: Add 20 μL of hydrogen peroxide solution to the mixture in step 2, shake gently to mix, and quickly add 10 μL of sodium borohydride; after standing at room temperature for 8-24 hours, centrifuge and wash to obtain gold nanosheets, and evenly disperse them in a pure water solution for storage.

[0044] Figure 4 The figure shows the optical absorption spectrum of the gold nanosheets prepared in Example 3. It can be seen that the optical absorption peak of the gold nanosheets prepared in this example is around 790 nm.

[0045] Comparing Examples 1-3, as the amount of hydrogen peroxide solution in the system increases, the optical absorption peak of the gold nanosheets blue-shifts, which may be due to the reduction in their size.

[0046] Example 4

[0047] Step 1: prepare 2 mM polyvinyl pyrrolidone solution, 5 mM chloroauric acid solution and 5 mM sodium borohydride solution respectively;

[0048] Step 2: Add 4.7 mL of pure water, 0.5 mL of polyvinyl pyrrolidone solution, and 0.5 mL of chloroauric acid solution into a centrifuge tube; the molar ratio between the polyvinyl pyrrolidone and chloroauric acid is 0.4:1;

[0049] Step 3: Add 5 μL of hydrogen peroxide solution to the mixture in step 2, shake gently to mix, and quickly add 20 μL of sodium borohydride. After standing at room temperature for 8-24 hours, centrifuge and wash to obtain gold nanosheets, which are evenly dispersed in a pure water solution for storage.

[0050] Figure 5 The figure shows the optical absorption spectrum of the gold nanosheets prepared in Example 4. It can be seen that the optical absorption peak of the gold nanosheets prepared in this example is around 890 nm.

[0051] Example 5

[0052] Step 1: prepare 2 mM polyvinyl pyrrolidone solution, 5 mM chloroauric acid solution and 5 mM sodium borohydride solution respectively;

[0053] Step 2: Add 4.7 mL of pure water, 0.5 mL of polyvinyl pyrrolidone solution, and 0.5 mL of chloroauric acid solution into a centrifuge tube; the molar ratio between the polyvinyl pyrrolidone and chloroauric acid is 0.4:1;

[0054] Step 3: Add 5 μL of hydrogen peroxide solution to the mixture in step 2, shake gently to mix, and quickly add 30 μL of sodium borohydride. After standing at room temperature for 8-24 hours, centrifuge and wash to obtain gold nanosheets, which are evenly dispersed in a pure water solution for storage.

[0055] Example 6

[0056] Step 1: prepare 2 mM polyvinyl pyrrolidone solution, 5 mM chloroauric acid solution and 50 mM sodium hydroxide solution respectively;

[0057] Step 2: Add 4.7 mL of pure water, 0.5 mL of polyvinyl pyrrolidone solution, and 0.5 mL of chloroauric acid solution into a centrifuge tube; the molar ratio between the polyvinyl pyrrolidone and chloroauric acid is 0.4:1;

[0058] Step 3: Add 3 μL of hydrogen peroxide solution to the mixture in step 2, shake gently to mix, and quickly add 30 μL of sodium hydroxide. After standing at room temperature for 8-24 hours, centrifuge and wash to obtain gold nanosheets, which are evenly dispersed in a pure water solution for storage.

[0059] Figure 6 The figure shows a scanning electron microscope image of the gold nanosheets prepared in Example 6 of the present invention. It can be seen that the maximum side length of the gold nanosheets can reach 1 micron.

[0060] Figure 7 The optical absorption spectrum of the gold nanosheets prepared in Example 6 is shown, and the spectrum is similar to the absorption spectrum of gold sheets with a size of micrometer in the literature.

[0061] Example 7

[0062] Step 1: prepare 2 mM polyvinyl pyrrolidone solution, 5 mM chloroauric acid solution and 50 mM sodium hydroxide solution respectively;

[0063] Step 2: Add 4.7 mL of pure water, 0.5 mL of polyvinyl pyrrolidone solution, and 0.5 mL of chloroauric acid solution into a centrifuge tube; the molar ratio between the polyvinyl pyrrolidone and chloroauric acid is 0.4:1;

[0064] Step 3: Add 3 μL of hydrogen peroxide solution to the mixture in step 2, shake gently to mix, and quickly add 20 μL of sodium hydroxide. After standing at room temperature for 8-24 hours, centrifuge and wash to obtain gold nanosheets, which are evenly dispersed in a pure water solution for storage.

[0065] Figure 8 The optical absorption spectrum of the gold nanosheets prepared in Example 7 is shown, and the spectrum is similar to the absorption spectrum of gold sheets with a size of micrometer in the literature.

[0066] The nanosheet synthesized by the invention is applied in the fields of surface enhanced Raman scattering spectroscopy, saturable absorber, photothermal, plasma refractive index sensor, organic matter degradation, etc.

[0067] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing gold nanosheets, characterized in that: The specific steps are: Step 1: prepare polyvinyl pyrrolidone solution, chloroauric acid solution, sodium borohydride solution and sodium hydroxide solution respectively; Step 2: Add polyvinyl pyrrolidone solution and chloroauric acid solution into a centrifuge tube and mix well; Step 3: Add hydrogen peroxide solution to the mixed solution of step 2, mix and shake well, then quickly add sodium borohydride solution or sodium hydroxide solution; let stand at room temperature for 8-24 hours, and obtain gold nanosheets after centrifugation and washing.

2. The method for preparing a gold nanosheet according to claim 1, characterized in that: In step 1, the concentration of the polyvinyl pyrrolidone solution is 2 mM, the concentration of the chloroauric acid solution is 5 mM, the concentration of the sodium borohydride solution is 5 mM, and the concentration of the sodium hydroxide solution is 50 mM.

3. The method for preparing a gold nanosheet according to claim 1, characterized in that: In step 2, the molar ratio of polyvinyl pyrrolidone to chloroauric acid is (0.08-1):

1.

4. The method for preparing a gold nanosheet according to claim 3, characterized in that: In step 2, the molar ratio of polyvinyl pyrrolidone to chloroauric acid is 0.4:

1.

5. The method for preparing a gold nanosheet according to claim 1, characterized in that: In step 3, the molar ratio of hydrogen peroxide, sodium borohydride and chloroauric acid is (12-60):(0.02-0.1):

1.

6. The method for preparing a gold nanosheet according to claim 1, characterized in that: In step 3, the molar ratio of hydrogen peroxide, sodium hydroxide and chloroauric acid is (12-60):(0.06-0.6):1.