TRB door ring production method and TRB door ring

By using TRB material in the door ring to divide multiple intensity areas and perform laser welding, the problem of difficult to reduce the weight of the door ring in the prior art is solved, and the door ring strength and light weight are achieved, improving performance and reducing production costs.

CN119077286APending Publication Date: 2024-12-06CHONGQING ZHIXIN IND CO LTD

Patent Information

Application Number
CN202411039541.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to improve the strength and durability of the door ring while meeting the automotive lightweight demand. Due to the insufficient strength of the weld area, the door ring weight is difficult to further reduce, and it is impossible to meet the higher lightweight requirements.

Method used

The door ring structure is divided into multiple continuous strength areas using TRB material, and the material sheets of different thicknesses are designed according to the strength requirements of different locations, and the annular joints are formed through laser welding to reduce the length and number of joints, and the overall weight is reduced. and performance improvement.

Benefits of technology

It achieves the meeting of the strength requirements of the door ring while reducing the overall weight, reducing the risk of the strength impact of the weld, improving part performance and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077286A_ABST
    Figure CN119077286A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of door ring production, and discloses a TRB door ring production method and a TRB door ring, and the TRB door ring production method comprises the following steps: step 1, dividing a door ring structure into four sections, and respectively obtaining an A section structure, a B section structure, a C section structure and a D section structure; 2, performing strength demand analysis on different positions of each section of structure, and correspondingly marking out a corresponding strength area on each section of structure according to the analysis; 3, calculating a corresponding material thickness value according to the strength requirement of each strength area, and respectively preparing four sections of material sheets with continuously changing thicknesses by adopting a TRB material according to the material thickness values; fourthly, the four sections of material pieces are sequentially subjected to end-to-end laser tailor-welding to form an annular shape, and four tailor-welded seams are formed; and fifthly, the material pieces obtained after tailor welding are subjected to hot stamping forming for follow-up machining operation. According to the invention, the TRB material is made into the material sheets with continuously changing thicknesses, so that the number of the material sheets is effectively reduced, the laser tailored blank welding length and the number of patch plates are reduced, the overall weight of the door ring is reduced, and the overall performance of the door ring is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vehicle door ring production, and in particular to a TRB door ring production method and a TRB door ring. Background Art

[0002] In the field of door knocker design and manufacturing, the door knocker is a key component that connects the door body and the door frame. The mechanical loads borne by different positions of the door knocker are different. Therefore, the strength requirements of different parts of the door knocker are different due to functional differences. This requires the door knocker to have corresponding strength and durability. With the introduction of the concept of lightweight automobiles, and in order to meet the strength requirements of door knockers, the prior art often uses patches to locally strengthen weak areas to form door knockers that meet the overall strength requirements. However, with the continuous increase in the demand for lightweight automobiles, although this method of local increase can reduce the weight of the door knocker as a whole, it is still necessary to add patch plates, and in order to ensure the strength of the door knocker, the number and thickness of the patch plates cannot be reduced. Therefore, the weight of the door knocker will still increase, making it difficult for the door knocker to meet better lightweight requirements.

[0003] And because the patch plate is set on the sheet material by welding, it will increase more welds accordingly, making the strength of the weld area weaker, which in turn affects the overall strength of the door knocker. Therefore, it is necessary to further increase the length or thickness of the patch plate to compensate for this deficiency, resulting in the door knocker weight is always difficult to further reduce, and it is difficult to meet higher lightweight requirements.

[0004] In order to overcome this technical difficulty, an integrated door ring structure is proposed in the prior art, such as the invention patent "A hot-formed laser-welded integrated door ring structure and processing method" with publication number CN118004284 A, which uses 6 sheets of different thicknesses to be welded in sequence and then stamped into an integrated structure. Although this method effectively reduces the use of patch plates and optimizes the cost and weight of the vehicle while meeting performance requirements, it is mainly made of CR950 / 1300HS material, that is, conventional aluminum-silicon-plated material, which combines the advantages of aluminum and silicon and is currently a commonly used production material.

[0005] In order to ensure performance, when setting the material thickness, due to the performance and processing limitations of the materials used, the entire sheet can only be set to a unified material thickness. In order to reduce the weight as much as possible, the sheet can only be divided into multiple pieces. Although the overall weight is effectively reduced, it will increase more welds, thereby increasing the strength risk of the weld area. In order to reduce the risk brought by welds, the welds can only be reduced as much as possible, which will lead to an expansion of the sheet range. In order to meet the highest strength requirements, the entire sheet must be unified to the highest material thickness, resulting in an increase in the weight of the door ring, and it is still difficult to meet the high requirements of lightweight. In the existing technology, it is always difficult to break through this technical difficulty. Summary of the invention

[0006] The present invention aims to provide a TRB door knocker production method and a TRB door knocker, which use TRB materials to be divided into multiple continuous strength areas according to the door knocker strength requirements, and meet the door knocker strength requirements without the need for additional patch plates. At the same time, through laser welding, the laser welding length and the number of welds are reduced, the risks at the welds are reduced, the overall weight of the door knocker is reduced, the overall performance of the parts is improved, and the cost of the parts is reduced.

[0007] To achieve the above object, the present invention adopts the following technical solution, a TRB door ring production method, comprising the following steps:

[0008] Step 1: Divide the door ring structure into four sections, namely, section A structure, section B structure, section C structure and section D structure;

[0009] Step 2: Perform strength requirement analysis on different positions of each structure section, and draw corresponding strength areas on each structure section according to the analysis results;

[0010] Step 3: Calculate the corresponding material thickness value according to the strength requirements of each strength area, and use TRB material to make four sections of continuously changing thickness sheets according to the material thickness values, namely, section A sheet, section B sheet, section C sheet, and section D sheet;

[0011] Step 4: Laser weld the four sections of the sheet end to end in sequence to form a ring, forming four welded seams;

[0012] Step 5: hot stamping the welded pieces for subsequent processing.

[0013] At the same time, the present invention also provides a TRB door ring, which is produced by using the above-mentioned TRB door ring production method.

[0014] The principles and advantages of this solution are:

[0015] Traditional door knockers are generally manufactured by combining TWB (Tailor Welded Blanks) with patch plates. In order to ensure the strength requirements of the door knockers, patch plates have become an effective production method to reduce the weight of the door knockers. Even if patch plates are not used, the thickness of the patch plates needs to be directly converted into the blanks. Therefore, adding patch plates has become an inherent production model. At the same time, due to the limitations of the commonly used production materials of door knockers, the weight of the door knockers is difficult to meet higher requirements.

[0016] This solution breaks the conventional production thinking and the inherent technical barriers in this field. It uses TRB materials to replace the original patch plate production method. Different strength areas are designed according to the strength requirements of different positions of the door ring, and correspondingly, different continuous material thicknesses are set on the same sheet, thereby ensuring that the strength requirements of different positions of the door ring are met and the overall weight of the door ring can be reduced. At the same time, due to the design of a whole piece of material with continuously changing material thickness, the strength of the corresponding area can be strengthened while reducing the number of sheets and corresponding welds, reducing the risk of strength impact of welds and improving the overall performance of the door ring. At the same time, the use of this solution can reduce the length of laser welding and subsequent patch welding processes, directly form an integrated product, shorten the production cycle, and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The figure is a schematic flow chart of a method for producing a TRB door knocker according to the present invention.

[0018] Figure 2 It is a schematic structural diagram of a TRB door ring of the present invention. DETAILED DESCRIPTION

[0019] The following is further described in detail through specific implementation methods:

[0020] The figure marks in the drawings of the specification include: A section structure 1, B section structure 2, C section structure 3, D section structure 4, A1 strength area 5, A2 strength area 6, A3 strength area 7, B1 strength area 8, B2 strength area 9, B3 strength area 10, C1 strength area 11, C2 strength area 12, C3 strength area 13, D1 strength area 14, D2 strength area 15, D3 strength area 16, D4 strength area 17, A12 transition area 18, A23 transition area 19, B12 transition area 20, B23 transition area 21, C12 transition area 22, C23 transition area 23, D12 transition area 24, D23 transition area 25, D34 transition area 26, first tailored weld 27, second tailored weld 28, third tailored weld 29, fourth tailored weld 30.

[0021] Embodiment 1

[0022] A TRB door knocker production method in this embodiment uses TRB material to directly make continuous sheets of different thicknesses, and then uses laser welding to reduce the laser welding length and the number of patch plates while meeting the door knocker strength requirements, effectively reducing the overall weight of the door knocker, and at the same time reducing the number of welds to improve the overall performance of the door knocker.

[0023] Details are as attached Figure 1 As shown, the production method comprises the following steps:

[0024] S1, as attached Figure 2As shown, the door ring structure is divided into four sections, namely, section A structure 1, section B structure 2, section C structure 3 and section D structure 4.

[0025] Among them, the A-section structure 1 corresponds to the upper side beam position of the door ring, ensuring the integrity of the overall structure of the upper side beam and improving the strength of the upper side beam position. The B-section structure 2 corresponds to the door ring A-pillar, the corner between the A-pillar and the upper side beam, and the front end of the door sill. The B-section structure 2 directly forms the corners at both ends in one piece. Due to the structure of the corners themselves, their strength is lower than that of other positions. The corners at both ends are directly merged into one piece to reduce the welding lines at the corners and improve the strength performance of the corners.

[0026] The C-section structure 3 corresponds to the middle part of the threshold. Since the threshold has a relatively low strength requirement, the traditional threshold structure includes two corners, which are mainly used for splicing, resulting in a high strength requirement at both ends, and thus the strength requirement of the entire threshold is raised. This solution separates the two ends and only retains the middle position, which can effectively reduce the overall weight while meeting the local strength requirements. The D-section structure 4 corresponds to the door knocker B-pillar, the rear end of the threshold, and the corner between the B-pillar and the side beam. The connecting corner is directly formed into one piece to improve the strength performance of the corner, while reducing the need for welding lines and patches, reducing the number of sheets as a whole, and meeting the strength requirements at the same time, effectively reducing the number of welds, improving performance while reducing weight.

[0027] S2, conduct strength demand analysis on different positions of each section of the structure, and according to the analysis results, draw corresponding strength areas on each section of the structure.

[0028] In this embodiment, the A segment structure 1 is divided into sequentially connected A1 strength area 5, A2 strength area 6 and A3 strength area 7 according to strength requirements. The B segment structure 2 is divided into sequentially connected B1 strength area 8, B2 strength area 9 and B3 strength area 10 according to strength requirements. The C segment structure 3 is divided into sequentially connected C1 strength area 11, C2 strength area 12 and C3 strength area 13 according to strength requirements. The D segment structure 4 is divided into sequentially connected D1 strength area 14, D2 strength area 15, D3 strength area 16 and D4 strength area 17 according to strength requirements.

[0029] S3, according to the strength requirements of each strength area, the corresponding material thickness value is calculated, and TRB material is used to make four sections of material sheets with continuously changing thickness according to the material thickness value, which correspond to section A sheet, section B sheet, section C sheet and section D sheet respectively.

[0030] In this embodiment, according to the strength requirements of each strength area, the material thickness of the A1 strength area 5 and the A3 strength area 7 are set to be the same, both 2.3 mm. The material thickness of the A2 strength area 6 is set to 2.1 mm. The material thickness of the B1 strength area 8 is set to 1.8 mm, the material thickness of the B2 strength area 9 is set to 1.5 mm, and the material thickness of the B3 strength area 10 is set to 1.9 mm.

[0031] The material thickness of the C1 strength area 11 and the C3 strength area 13 is set to be the same, both 1.4mm. The material thickness of the C2 strength area 12 is set to be 1.7mm. The material thickness of the D1 strength area 14 and the D3 strength area 16 is set to be the same, both 2.1mm. The material thickness of the D2 strength area 15 is set to be 2.4mm, and the material thickness of the D4 strength area 17 is set to be 1.6mm. This ensures that the strength of each strength area on each sheet meets the requirements, while effectively reducing the thickness of each sheet, thereby reducing the overall weight of the door knocker. At the same time, there is no need to add patch plates, reduce weld seams, and improve the overall performance of the door knocker.

[0032] At the same time, on each section of the sheet, a transition area is provided between each strength area, and the thickness of the transition area is between the thicknesses of two adjacent strength areas, so that the two strength areas can transition smoothly and ensure stable connection between the two strength areas. In this embodiment, the width of the transition area W = E*(50-100) mm, where E is the material thickness difference between adjacent strength areas.

[0033] As attached Figure 2 As shown, an A12 transition region 18 is provided between the A1 strength region 5 and the A2 strength region 6, and an A23 transition region 19 is provided between the A2 strength region 6 and the A3 strength region 7. A B12 transition region 20 is provided between the B1 strength region 8 and the B2 strength region 9, and a B23 transition region 21 is provided between the B2 strength region 9 and the B3 strength region 10. A C12 transition region 22 is provided between the C1 strength region 11 and the C2 strength region 12, and a C23 transition region 23 is provided between the C2 strength region 12 and the C3 strength region 13. A D12 transition region 24 is provided between the D1 strength region 14 and the D2 strength region 15, a D23 transition region 25 is provided between the D2 strength region 15 and the D3 strength region 16, and a D34 transition region 26 is provided between the D3 strength region 16 and the D4 strength region 17. This ensures that different strength areas on each sheet can meet the strength requirements according to different positions, while achieving the production of one-piece continuous thickness-changing sheets without connecting them by welding, ensuring the stability of the sheet while reducing the number of welds and improving overall performance.

[0034] In this embodiment, the length of the strength area on each section of the structure can be adjusted according to the strength requirements to meet the strength requirements of each vehicle model.

[0035] S4, the four sections of the sheet are sequentially welded end to end by laser to form a ring, so as to form four welding seams.

[0036] In this embodiment, the front end of the A1 strength region 5 and the upper end of the B1 strength region 8 are laser welded to form a first weld 27. The rear end of the B3 strength region 10 and the front end of the C1 strength region 11 are laser welded to form a second weld 28. The rear end of the C3 strength region 13 and the lower end of the D4 strength region 17 are laser welded to form a third weld 29. The front end of the D1 strength region 14 and the rear end of the A3 strength region 7 are laser welded to form a fourth weld 30. Therefore, this solution only needs four welds to complete the splicing of the entire door ring, thereby reducing the number of welds. At the same time, the selected weld position can effectively reduce the length of the weld, thereby reducing the risk of strength impact caused by the weld, and also reducing the area of ​​the weld area, thereby reducing the overall weight, further shortening the production cycle, and reducing production costs.

[0037] In this embodiment, laser welding is to directly weld the two ends together without adding additional reserved materials, thereby reducing material loss and improving material utilization. At the same time, the strength of the weld is improved through laser welding.

[0038] S5, hot stamping is performed on the welded pieces for subsequent processing.

[0039] Correspondingly, in this embodiment, a TRB door ring is also provided, which is a TRB door ring manufactured using the above-mentioned TRB door ring production method.

[0040] In this embodiment, TRB material is used for laser welding. According to the strength requirements of different positions of the door knocker, strength areas of different thicknesses are set accordingly. The TRB material is integrated into a sheet with continuously changing thickness, which effectively reduces the number of sheets. At the same time, the laser welding length and the number of patch plates are reduced. While ensuring the overall strength requirements of the door knocker, the overall weight of the door knocker is effectively reduced, thereby improving the overall performance of the door knocker and reducing production costs.

[0041] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for producing a TRB door ring, characterized in that: The following steps are involved: Step 1: Divide the door ring structure into four sections, namely, section A structure, section B structure, section C structure and section D structure; Step 2: Perform strength requirement analysis on different positions of each structure section, and draw corresponding strength areas on each structure section according to the analysis results; Step 3: Calculate the corresponding material thickness value according to the strength requirements of each strength area, and use TRB material to make four sections of continuously changing thickness sheets according to the material thickness values, namely, section A sheet, section B sheet, section C sheet, and section D sheet; Step 4: Laser weld the four sections of the sheet end to end in sequence to form a ring, forming four welded seams; Step 5: hot stamping the welded pieces for subsequent processing.

2. A TRB door knocker production method according to claim 1, characterized in that: The section A structure corresponds to the side beam position above the door ring; the section B structure corresponds to the door ring A-pillar, the corner between the A-pillar and the side beam, and the front end of the door sill; the section C structure corresponds to the middle of the door sill; the section D structure corresponds to the door ring B-pillar, the rear end of the door sill, and the corner between the B-pillar and the side beam.

3. A TRB door knocker production method according to claim 1, characterized in that: On each section of the sheet, a transition area is provided between each strength area; the width of the transition area is W=E*(50-100) mm, wherein E is the difference in material thickness between adjacent strength areas.

4. A TRB door knocker production method according to claim 1, characterized in that: The A section structure is divided into A1 strength area, A2 strength area and A3 strength area connected in sequence according to strength requirements; the B section structure is divided into B1 strength area, B2 strength area and B3 strength area connected in sequence according to strength requirements; the C section structure is divided into C1 strength area, C2 strength area and C3 strength area connected in sequence according to strength requirements; the D section structure is divided into D1 strength area, D2 strength area, D3 strength area and D4 strength area connected in sequence according to strength requirements.

5. A TRB door knocker production method according to claim 4, characterized in that: The front end of the A1 strength region and the upper end of the B1 strength region are laser welded to form a first weld; the rear end of the B3 strength region and the front end of the C1 strength region are laser welded to form a second weld; the rear end of the C3 strength region and the lower end of the D4 strength region are laser welded to form a third weld; the front end of the D1 strength region and the rear end of the A3 strength region are laser welded to form a fourth weld.

6. A TRB door knocker production method according to claim 4, characterized in that: The material thickness of the A1 strength area is the same as that of the A3 strength area, which is 2.3 mm; the material thickness of the A2 strength area is 2.1 mm; the material thickness of the B1 strength area is 1.8 mm, the material thickness of the B2 strength area is 1.5 mm, and the material thickness of the B3 strength area is 1.9 mm.

7. A method for producing a TRB door knocker according to claim 4, characterized in that: The material thickness of the C1 strength zone and the C3 strength zone is the same, both are 1.4 mm; the material thickness of the C2 strength zone is 1.7 mm; the material thickness of the D1 strength zone and the D3 strength zone is the same, both are 2.1 mm; the material thickness of the D2 strength zone is 2.4 mm; and the material thickness of the D4 strength zone is 1.6 mm.

8. A method for producing a TRB door knocker according to claim 4, characterized in that: The length of the strength area on each section of the structure is adjusted according to the strength requirements.

9. A method for producing a TRB door knocker according to claim 5, characterized in that: The laser welding is direct butt welding.

10. A TRB door knocker, characterized in that: A door knocker produced by a TRB door knocker production method as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Integrated forming method and die for automobile door ring

    CN115401429A

  • Variable-thickness automobile door ring and preparation method thereof