Biological pretreatment method for preparing high-quality veneer and product

The logs are treated through lactic acid bacteria fermentation, and the chemical composition of wood are degraded by lactic acid bacteria, which solves the surface roughness and pollution of the veneer, improves the whiteness and flatness of the veneer, and achieves environmentally friendly and efficient veneer production.

CN119077876APending Publication Date: 2024-12-06NANJING FORESTRY UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411253864.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing wood processing technology, the lack of log pretreatment links leads to rough surfaces and easy burrs, which reduces the appearance quality and performance of veneers. In addition, traditional pretreatment methods have problems such as high cost, high energy consumption and environmental pollution.

Method used

The fermentation of lactic acid bacteria degrades the chemical components in the wood, soaks the log by mixing lactic acid bacteria solution to reduce the internal stress of the wood and improves the softening effect of the veneer. The mixed bacteria agent of Lactobacillus plantarum, Lactobacillus brucea or Streptococcus lactic acid is used. Anaerobic fermentation, spin cutting or slicing is performed for ultraviolet sterilization.

Benefits of technology

It significantly improves the whiteness and surface flatness of the veneer, reduces the surface roughness, and achieves environmentally friendly and pollution-free high-quality veneer production without affecting the mechanical properties of the veneer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077876A_ABST
    Figure CN119077876A_ABST
Patent Text Reader

Abstract

The invention discloses a biological pretreatment method for preparing a high-quality veneer and a product, and belongs to the technical field of wood processing. The biological pretreatment method disclosed by the invention comprises the step of soaking raw wood by using a mixed lactic acid bacteria solution, the mixed lactic acid bacteria solution is prepared by mixing lactobacillus plantarum with any one of lactobacillus buchneri, pediococcus acidilactici or lactic streptococci. According to the method, part of chemical components in wood are slightly degraded through lactobacillus fermentation, so that the growth stress and internal stress of the wood are reduced, the wood segment softening effect is achieved, the cutting resistance during rotary cutting or slicing is reduced, the roughness caused by cracks on the back face of the veneer is reduced or reduced, and the appearance quality and surface whiteness of the veneer are improved; and finally, the high-quality rotary-cut or sliced veneer is obtained. According to the scheme provided by the invention, the problems of higher cost, higher energy consumption, wastewater generation, environmental pollution and the like in the traditional treatment method can be effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wood processing, and in particular relates to a biological pretreatment method and product for preparing high-quality veneers. Background Art

[0002] At present, the construction and furniture industries mainly rely on various man-made panels made of fast-growing materials, such as plywood and laminated timber. As the unit material of plywood and laminated timber, veneer is a thin sheet of wood material produced by methods such as peeling, planing or sawing. In the process of peeling veneers from fast-growing materials, most veneer production factories have removed the log pretreatment link before peeling veneers in order to reduce the environmental burden. This measure has resulted in the logs not being effectively softened, thereby increasing the cutting resistance, making the surface of the veneer rough and prone to burrs, reducing the appearance quality and performance of the veneer, and is not conducive to the later processing of the veneer. The low-quality processing of the veneer has lowered the performance and appearance quality of plywood and various wood laminates. Therefore, there is an urgent need to improve the pretreatment level of log sections to improve the quality of processed veneers.

[0003] In the wood industry, the pretreatment of logs is a necessary process before veneer peeling or slicing. Traditional log pretreatment methods include hydrothermal pretreatment, microwave pretreatment and chemical pretreatment. Although these methods can soften the wood segments to a certain extent, they generally have problems such as high cost, high energy consumption, wastewater generation and environmental pollution. Therefore, it is of great significance to provide a simple, efficient and green non-polluting treatment method to prepare high-quality veneers. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a biological pretreatment method and product for preparing high-quality veneer. The method provided by the present invention utilizes lactic acid bacteria fermentation to degrade the chemical components in wood, thereby reducing the internal stress of the wood, achieving the effect of softening the wood, and finally obtaining high-quality veneer.

[0005] The present invention provides the following technical solutions:

[0006] Technical Solution 1: A biological pretreatment method for preparing high-quality veneer, comprising the step of soaking logs in a mixed lactic acid bacteria solution; the components of the mixed lactic acid bacteria solution include a mixture of Lactobacillus plantarum and any one of Lactobacillus buchneri, Pediococcus acidilactici or Streptococcus lactis.

[0007] Furthermore, the steps include first peeling the logs and removing surface impurities, soaking them in the mixed lactic acid bacteria solution, performing anaerobic fermentation in a fermentation device, then rotary cutting or slicing the logs after anaerobic fermentation, and finally performing ultraviolet sterilization.

[0008] Furthermore, in the mixed lactic acid bacteria solution, based on the number of live bacteria of the Lactobacillus plantarum as the calculation base, the mixing ratio of any one of the Lactobacillus buchneri, the Pediococcus acidilactici or the Streptococcus lactis to the Lactobacillus plantarum is 1:(1-10).

[0009] Furthermore, the logs are completely immersed in the mixed lactic acid bacteria solution, and the liquid level of the mixed lactic acid bacteria solution is greater than 20 cm of the log stack height.

[0010] Furthermore, the conditions of the anaerobic fermentation are: fermentation at 10-35°C for 5-30 days, and regular exhaust of the fermentation device.

[0011] Furthermore, the thickness of the peeled or sliced ​​logs is 0.5-12 mm.

[0012] Furthermore, the wavelength of ultraviolet sterilization is 200-275nm, and the sterilization time is 15-200s.

[0013] Technical Solution 2: A high-quality veneer prepared using the biological pretreatment method.

[0014] Furthermore, the average whiteness of the high-quality veneer is 90±3.

[0015] Technical Solution Three: A method for preparing a high-quality veneer product, comprising subjecting the high-quality veneer to air-dry storage or wet storage to obtain the high-quality veneer product.

[0016] Compared with the prior art, the present invention has the following advantages and technical effects:

[0017] The present invention adopts biological pretreatment to log wood segments, that is, the log wood segments are treated by lactic acid bacteria fermentation, which consumes nutrients such as sugar in the growth of trees, slightly degrades some chemical components such as cellulose, hemicellulose and lignin in the logs, destroys the structure of the pit membrane, and improves the permeability between wood cells to a certain extent. The log wood segments are fermented to destroy the connection between lignin and carbohydrates, so that the lignin itself produces a softening effect, reduces the internal stress of the wood under certain conditions, and achieves the effect of softening the wood. Compared with physical and chemical treatment methods, the method adopted by the present invention is simple and easy to operate, and the lactic acid bacteria fermentation liquid can be circulated for the pretreatment of log wood segments to achieve the recycling of the treatment liquid. No harmful substances are generated during the fermentation process, no wastewater pollution, and no environmental pollution. It is a green log pretreatment method and a method for producing high-quality veneers. After the mixed bacterial agent composed of plant lactobacillus and other lactic acid bacteria is used to ferment the log wood segments, the quality of the obtained veneer is significantly improved, the whiteness of the veneer is increased by 10.77±2%, and the Ra value of the surface roughness is reduced by 48.97±5%. During the fermentation process, some chemical components are slightly degraded, but the basic mechanical properties of the veneer are not affected. The surface of the obtained veneer is flat and not prone to burrs, and the surface of the veneer is more delicate and has higher whiteness. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 It is the process flow chart of Example 1;

[0020] Figure 2 The microscopic morphology of the rotary cut veneer in Comparative Example 1;

[0021] Figure 3 The microscopic morphology of the rotary cut veneer in Example 2;

[0022] Figure 4 ] are the infrared spectra of the single plates in Example 2 and Comparative Example 1. DETAILED DESCRIPTION

[0023] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0024] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0025] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0026] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0027] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0028] The poplar logs used in the following examples were from Lianyungang Zhiwei Wood Industry Co., Ltd., Jiangsu Province; the bacterial powders of Lactobacillus plantarum, Lactobacillus buchneri, Pediococcus acidilactici and Streptococcus lactis were all purchased from Shandong Zhongke Jiayi Bioengineering Co., Ltd.

[0029] Example 1

[0030] A method for preparing high-quality veneer products:

[0031] (1) cutting the felled poplar logs according to the size of the fermentation device, and peeling the cut wood segments;

[0032] (2) Preparation of mixed lactic acid bacteria solution: Based on the number of live bacteria of Lactobacillus plantarum as the calculation base, Lactobacillus buchneri powder and Lactobacillus plantarum powder were mixed at a ratio of 1:1 to obtain mixed bacterial powder, and the mixed bacterial powder and water were mixed at a mass ratio of 1:10. 3 Prepare a mixed lactic acid bacteria solution;

[0033] (3) Soaking the peeled wood pieces in a mixed lactic acid bacteria solution with the liquid level being 30 cm higher than the height of the wood piece stack, and fermenting them under anaerobic conditions at 25°C for 14 days;

[0034] (4) The fermentation device needs to be deflated every 24 hours for 7 days before fermentation and every 48 hours for 7 days after fermentation. The pH of the lactic acid bacteria mixed solution is measured with pH test paper every 48 hours;

[0035] (5) Rinse the fermented wood segments with clean water to complete the wood segment pretreatment;

[0036] (6) The wood segments are peeled, and the peeled veneer thickness is 0.8 mm. The peeled veneer is sterilized for 15 seconds under short-wave sterilizing ultraviolet UVC with a wavelength of 200 nm, and then the veneer is air-dried to a moisture content of 12% to obtain a high-quality veneer.

[0037] A method for preparing a high-quality veneer product, wherein the prepared high-quality veneer is subjected to air-drying storage or wet storage to obtain a high-quality veneer product. Air-dry storage refers to the dry storage of high-quality veneers with a moisture content of 10-15% after air-drying; wet storage refers to the direct vacuum sealing storage of veneers with a moisture content of more than 50% after sterilization. See the process flow chart Figure 1 .

[0038] Example 2

[0039] A method for preparing high-quality veneer products:

[0040] (1) cutting the felled poplar logs according to the size of the fermentation device, and peeling the cut wood segments;

[0041] (2) Preparation of mixed lactic acid bacteria solution: Based on the number of live bacteria of Lactobacillus plantarum as the calculation base, the powders of Pediococcus acidilactici and Lactobacillus plantarum were mixed at a ratio of 1:5 to obtain a mixed bacterial powder, and the mixed bacterial powder and water were mixed at a mass ratio of 1:10. 2 Prepare a mixed lactic acid bacteria solution;

[0042] (3) Soaking the peeled wood pieces in a mixed lactic acid bacteria solution with the liquid level being 35 cm higher than the height of the wood piece stack, and fermenting them under anaerobic conditions at 25°C for 7 days;

[0043] (4) The fermentation device needs to be deflated every 24 hours for 3 days before fermentation, and every 48 hours for 4 days after fermentation. The pH of the lactic acid bacteria mixed solution is measured with pH test paper every 48 hours;

[0044] (5) Rinse the fermented wood segments with clean water to complete the wood segment pretreatment;

[0045] (6) The wood segments are peeled, and the peeled veneer thickness is 0.8 mm. The peeled veneer is sterilized for 150 seconds under short-wave sterilizing ultraviolet UVC with a wavelength of 275 nm, and then the veneer is air-dried to a moisture content of 15% to obtain high-quality veneer.

[0046] Example 3

[0047] A method for preparing high-quality veneer products:

[0048] (1) cutting the felled poplar logs according to the size of the fermentation device, and peeling the cut wood segments;

[0049] (2) Preparation of mixed lactic acid bacteria solution: Based on the number of live bacteria of Lactobacillus plantarum as the calculation base, Streptococcus lactis and Lactobacillus plantarum powders were mixed at a ratio of 1:10 to obtain mixed bacterial powder, and the mixed bacterial powder and water were mixed at a mass ratio of 1:10. 2 Prepare a mixed lactic acid bacteria solution;

[0050] (3) Soaking the peeled wood pieces in a mixed lactic acid bacteria solution with the liquid level being 25 cm higher than the height of the wood piece stack, and mixed fermenting at 10° C. under anaerobic conditions for 30 days;

[0051] (4) The fermentation device needs to be deflated every 24 hours for 3 days before fermentation, and every 48 hours for 4 days after fermentation. The pH of the lactic acid bacteria mixed solution is measured with pH test paper every 48 hours;

[0052] (5) Rinse the fermented wood segments with clean water to complete the wood segment pretreatment.

[0053] (6) The wood segments are peeled, and the peeled veneer thickness is 0.8 mm. The peeled veneer is sterilized for 200 seconds under short-wave sterilizing ultraviolet UVC with a wavelength of 240 nm, and then the veneer is air-dried to a moisture content of 10% to obtain a high-quality veneer.

[0054] Comparative Example 1

[0055] The poplar veneer that has not been processed with the mixed lactic acid bacteria solution has a thickness of 0.8 mm and a moisture content of 12% (the felled poplar logs are peeled, rinsed with clean water, and the wood sections are peeled. The peeled veneer has a thickness of 0.8 mm. The peeled veneer is sterilized for 15 seconds under short-wave sterilizing ultraviolet light UVC with a wavelength of 200 nm, and then the veneer is air-dried to a moisture content of 12% to obtain a veneer).

[0056] Comparative Example 2

[0057] A method for preparing a single board product:

[0058] (1) cutting the felled poplar logs according to the size of the fermentation device, and peeling the cut wood segments;

[0059] (2) Preparation of plant lactic acid bacteria solution: plant lactobacillus powder and water in a mass ratio of 1:10 2 Prepare a plant lactic acid bacteria solution;

[0060] (3) Soaking the peeled wood pieces in a mixed lactic acid bacteria solution with the liquid level being 35 cm higher than the height of the wood piece stack, and fermenting them under anaerobic conditions at 25°C for 7 days;

[0061] (4) The fermentation device needs to be deflated every 24 hours for 3 days before fermentation, and every 48 hours for 4 days after fermentation. The pH of the lactic acid bacteria mixed solution is measured with pH test paper every 48 hours;

[0062] (5) Rinse the fermented wood segments with clean water to complete the wood segment pretreatment;

[0063] (6) The wood segments are peeled, and the peeled veneer thickness is 0.8 mm. The peeled veneer is sterilized for 150 seconds under short-wave sterilizing ultraviolet UVC with a wavelength of 275 nm, and then the veneer is air-dried to a moisture content of 15%, thereby obtaining other veneers.

[0064] In order to compare the effects of the present invention, the pH value, surface roughness analysis, surface color difference and mechanical properties of the above embodiments and comparative examples were respectively carried out; and the optimal implementation and comparative example single board were characterized by SEM and FTIR. The specific detection methods are as follows:

[0065] (1) pH value: A PHS-25 pH meter was calibrated with a pH buffer solution. The poplar veneers prepared in the three examples and two comparative examples and the veneers prepared in the comparative examples were crushed into powders that could pass through a 40-mesh sieve. 3.0 g of the sieved poplar powder was weighed in a 50 mL beaker, and 30.0 mL of cooled distilled water was poured into it. The pH value of the poplar powder was measured with a pH meter, and each group was measured three times in parallel.

[0066] (2) Surface roughness: The surface of the specimen was sanded with 400-grit sandpaper. The stylus diameter of the surface roughness tester was 80 μm, the sampling length was L = 2.50 mm, and the specimen size was 100 mm × 100 mm × 0.8 mm (length × width × height). The measured Ra (arithmetic mean deviation of the profile) was used to evaluate the surface roughness of the poplar veneer before and after fermentation, and each group was measured 5 times in parallel.

[0067] (3) Surface color difference: The surface color of the single board was measured at five random positions using a colorimeter (Shanghai Zhansheng Electromechanical Equipment Co., Ltd.) in the CIELAB color space. The L* value represents the darkness and lightness of the color, that is, whiteness, and the value range is 0-100; the larger the L* value, the higher the brightness and the greater the whiteness. Each group was measured three times in parallel.

[0068] (4) Mechanical properties: A universal mechanical testing machine was used to determine the tensile properties of artificial boards. The specimen was fixed between the two clamps of the tensile testing machine with a spacing of 120 mm. The specimen was destroyed within 60 ± 30 s. The tensile strength of the veneer was tested and calculated. Each group was measured 5 times in parallel. The tensile strength of the fermented poplar veneer was calculated according to Formula 1.

[0069]

[0070] Where:

[0071] σ1——tensile strength of specimen, in megapascals (MPa);

[0072] F max ——The maximum load when the specimen is destroyed, in Newton (N);

[0073] b——average width of the tensile fracture surface of the specimen, in millimeters (mm);

[0074] t is the average thickness of the tensile fracture surface of the specimen, in millimeters (mm).

[0075] (5) SEM: The poplar veneer of Comparative Example 1 and the optimal embodiment selected after fermentation was cut into test samples with a flat surface and a size of approximately 5 mm×5 mm×0.8 mm using a slicer. The microscopic morphology of the samples was observed using an environmental scanning electron microscope (Quanta 200, FEI, USA) at a test voltage of 20 KV.

[0076] (6) FTIR: The poplar veneer of Comparative Example 1 and the selected optimal embodiment after fermentation was crushed at room temperature and passed through a 200-mesh sieve. The samples were tested by infrared spectroscopy (VERTEX 80V, Bruker, Germany). The scanning range was 450-2200 cm -1 , scan times is 64 times, set resolution to 4cm -1 .

[0077] The test results are as follows:

[0078] (1) pH value: The pH value of comparative example 1 was neutral, at 6.8±0.2; the pH value of comparative example 2 showed a downward trend in the first 3 days, dropping to 5.5±0.2, and began to rise on the 4th day, with the final pH value being 5.3±0.2. The pH value of Example 1 showed a downward trend in the first 9 days, dropping to a minimum of 5.2±0.2, and began to rise on the 10th day, with the final pH value being 6.1±0.2. The pH values ​​of Examples 2 and 3 showed a downward trend in the first 3 days, dropping to 5.1±0.2, and began to rise on the 4th day, with the final pH value being 6.0±0.2. This indicates that the lactic acid bacteria degraded some of the chemical components of the veneer in the early stage and produced a large amount of lactic acid, but the lactic acid began to inhibit fermentation after reaching a certain concentration, so the pH value began to rise, and the degradation rate of some of the chemical components of the veneer slowed down until the fermentation stopped.

[0079] (2) Surface roughness: The surface roughness of the high-quality veneers obtained in the three groups of examples is significantly lower than that of Comparative Examples 1 and 2. The surface roughness of the tight edge along the grain and the transverse grain is 7.5-8.1 μm and 9.3-10.6 μm respectively, and the surface roughness of the loose edge along the grain and the transverse grain is 6.7-8.5 μm and 9.2-10.7 μm respectively, which is far below the international requirements. The roughness of the tight edge and the loose edge of Comparative Example 1 is higher than 10 μm, and that of Comparative Example 2 is higher than 9 μm. This is because the fermentation of lactic acid bacteria makes the wood segments fully softened, so the surface of the veneers peeled out in Examples 1-3 is smoother and flatter, with fewer burrs and lower surface roughness.

[0080] (3) Surface color difference: The surface brightness of the veneers of the three groups of embodiments and the two groups of comparative examples are shown in Table 1. The surface brightness L* values ​​of the embodiments are all higher than those of the comparative examples, with the highest increase of 10.77%. It can be seen that the surface whiteness of the high-quality veneers after the biological pretreatment of the present invention is significantly improved, thereby improving the appearance quality and use value of the veneers.

[0081] Table 1

[0082]

[0083] (4) Mechanical properties: The tensile strengths of the three groups of embodiments and the two groups of comparative examples are shown in Table 2. The mechanical properties of the embodiments and the comparative examples are not much different. Due to the instability of the wood structure, the tensile strengths are within a reasonable range. This indicates that although the lactic acid bacteria solution of the present invention degrades the main chemical components of cellulose, hemicellulose and lignin in the veneer during the fermentation process, it does not have an adverse effect on the mechanical strength of the veneer.

[0084] Table 2

[0085]

[0086] (5) SEM: Figure 2The figure shows the microscopic morphology of the veneer in comparative example 1. It can be seen that the tear marks of the fiber of the rotary cut veneer are relatively obvious, the tear edges are uneven, the cell walls are not completely peeled off, the rupture of the ducts is not obvious, and the resistance during the rotary cutting process is relatively large. Therefore, the surface of the veneer in the comparative example is very easy to burr and the surface roughness is relatively high. Figure 3 This is the microscopic morphology of the veneer in Example 2 of the optimal group. The fiber tearing marks of the rotary cut veneer in Example 2 are not obvious, the tearing edges are relatively smooth, the cell walls are mostly peeled off in one piece, and the duct rupture is more obvious, indicating that the cell wall is softened to a certain extent by lactic acid bacteria, which reduces the resistance during the rotary cutting process, so that the surface roughness of the finally obtained veneer is lower and it is not easy to pilling.

[0087] (6) FTIR: The FTIR of the single board of the best group Example 2 and Comparative Example 1 in the embodiment is as follows Figure 4 The main stretching vibration point of Example 2 in the spectrum is basically the same as that of Comparative Example 1, but Example 2 has a main stretching vibration point at 1736 cm -1 The characteristic absorption peaks of hemicellulose acetyl group at 1593 and 1505 cm -1 The characteristic absorption peak intensity of lignin at 1034 cm is greatly reduced. This is because the hydrogen bonds and ether bonds between lignin and hemicellulose are destroyed during the fermentation process, which causes some lignin and hemicellulose to dissolve and be removed. At the same time, compared with Comparative Example 1, the 1034 cm corresponding to the cellulose of the fermented wood in Example 2 is -1 The characteristic absorption peak at (C—O stretching vibration in cellulose ether bond) also showed a significant decrease, indicating that the wood not only lost part of the lignin and hemicellulose, but also part of the cellulose during the lactic acid bacteria fermentation.

[0088] In summary, the lactic acid bacteria fermentation wood segment scheme provided by the present invention is a low-cost, simple-to-operate biological pretreatment method, which provides a solution to the environmental pollution problems existing in the current traditional log treatment methods. It can improve the appearance quality of the veneer on the basis of environmental protection, reduce its surface roughness, and increase the brightness of the veneer without destroying the mechanical properties of the wood itself. It is a feasible and effective biological pretreatment method.

[0089] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A biological pretreatment method for preparing high-quality veneer, characterized in that: The method comprises the steps of soaking the logs with a mixed lactic acid bacteria solution; the components of the mixed lactic acid bacteria solution include a mixture of plant lactobacillus and any one of Lactobacillus buchneri, Pediococcus acidilactici or Streptococcus lactis.

2. The biological pretreatment method according to claim 1, characterized in that: The steps include peeling the logs and removing surface impurities, soaking them in the mixed lactic acid bacteria solution, performing anaerobic fermentation in a fermentation device, peeling or slicing the logs after anaerobic fermentation, and finally performing ultraviolet sterilization.

3. The biological pretreatment method according to claim 1, characterized in that: In the mixed lactic acid bacteria solution, based on the number of live bacteria of the plant lactobacillus as a calculation base, the mixing ratio of any one of the Lactobacillus buchneri, the Pediococcus acidilactici or the Streptococcus lactis to the plant lactobacillus is 1:(1-10).

4. The biological pretreatment method according to claim 2, characterized in that: The logs are completely immersed in the mixed lactic acid bacteria solution, and the liquid level of the mixed lactic acid bacteria solution is greater than 20 cm of the stacking height of the logs.

5. The biological pretreatment method according to claim 2, characterized in that: The conditions of the anaerobic fermentation are: fermentation at 10-35° C. for 5-30 days, and regular exhaust of the fermentation device.

6. The biological pretreatment method according to claim 2, characterized in that: The thickness of the peeled or sliced ​​logs is 0.5-12 mm.

7. The biological pretreatment method according to claim 2, characterized in that: The wavelength of ultraviolet sterilization is 200-275nm, and the sterilization time is 15-200s.

8. A high-quality veneer prepared by the biological pretreatment method according to any one of claims 1 to 7.

9. The high-quality single board according to claim 8, characterized in that: The average whiteness of the high-quality veneer is 90±3.

10. A method for preparing a high-quality single-board product, characterized in that: The method comprises subjecting the high-quality veneer described in claim 8 or 9 to air-dry storage or wet storage to obtain the high-quality veneer product.

Citation Information

Cited By

  • Anti-corrosion mildew-proof environment-friendly plywood and preparation method thereof

    CN120839891A