Mold cleaning method and machining forming method of mold
Through the combination of hot-pressed vulcanized base glue, mold cleaning glue and silicone rubber mould glue, the thermosetting composite mold is thoroughly cleaned, solving the problems of incomplete cleaning and pollution in the existing technology, and achieving blind spot cleaning and cleaning The effect of omitting the release agent.
Patent Information
- Application Number
- CN202411214685.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the mold cleaning method of thermoset composite composite material complex structural parts product molds has problems such as incomplete dirt cleaning, easy to damage the surface of the mold and the toxicity of organic solvents. The mold after the mold is cleaned requires spraying a release agent to contaminate the environment and cannot Accurately control film thickness.
The hot-pressing vulcanization method of base glue, mold cleaning glue and silicone rubber mould glue is used to clean the hot-pressing mold at primary and intermediate level. The resin and foreign matter are brought out through the vulcanization process, and the mold release agent is dispersed under vacuum conditions. The spray release agent step is omitted.
The comprehensive and thorough cleaning of molds of complex structural parts is achieved, which avoids mold damage and contamination, and does not require spraying release agents, solving the problems of pollution and film thickness control.
Smart Images

Figure CN119078051A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material processing, and more specifically to a mold cleaning method and a processing and forming method of a mold. Background Art
[0002] With the development of VR / AR, weight reduction has become an inevitable trend of its development. As people have higher and higher requirements for light, thin and comfortable wearable products, thermosetting carbon fiber composite materials have become the preferred material for thinning and weight reduction of polymer materials due to their advantages such as high specific strength and high specific modulus. However, in the actual production process of thermosetting carbon fiber, components such as epoxy resin and release agent will adhere to the metal mold at high temperature. The mold surface is prone to adhesion of epoxy resin residues and volatiles of release agent. After repeated production, serious dirt will be generated on the mold surface, and these dirt will further oxidize at high temperature, causing mold corrosion, affecting the appearance quality of the product, and thus affecting production efficiency. Therefore, mold cleaning and surface demolding are problems that need to be solved urgently.
[0003] At present, thermosetting carbon fiber composite materials are mainly used in aerospace, automobile and other fields. They are mainly used in the electronic and electrical industry for flat-structured products such as notebook shells and mobile phone shells. The mold surface is generally cleaned by manual polishing. However, for complex structural parts of wearable products, the mold cavity is small and the structure is complex. Manual polishing easily leaves dead corners and is difficult to completely remove dirt. Existing mold cleaning methods generally include organic solvent cleaning, manual polishing and high-temperature pyrolysis.
[0004] Among them, the method of using organic solvent to clean the mold surface requires cleaning after the mold is removed. Since epoxy resin is difficult to dissolve, it is difficult to remove the residue on the mold surface without damaging the mold, and the organic solvent is volatile and toxic; the method of manual polishing, by using a metal brush or sandpaper to scrub and polish the dirt on the mold surface, the effect of this method of removing dirt is not ideal, and due to the complex structure of electronic products and the small mold cavity of the mold, manual polishing is easy to leave dead corners, it is difficult to completely remove the dirt, and it is easy to damage the mold surface after polishing, affecting the appearance and size of the product; there is also a high-temperature pyrolysis method, that is, heating in air or inert gas to degrade the residual dirt on the mold surface and then remove it, which has high requirements for the metal material of the mold. The cross-linked thermosetting resin is decomposed into organic substances (liquids and gases) with lower molecular weight, and there are also solid carbon char products. After the high-temperature treatment is completed, this method also requires annealing and tempering operations on the mold.
[0005] Taking into account the shortcomings of the above methods, the current mold cleaning method for complex structural parts of thermosetting composite materials mainly adopts a combination of manual polishing and solvent cleaning. Although the effect is better than the above single mold cleaning method, it still has defects such as incomplete dirt cleaning, easy damage to the mold surface, affecting the size of the product appearance, and the toxicity of organic solvents. In addition, during the product production process, a release agent needs to be applied to the mold surface after organic solvent cleaning to facilitate demolding after the subsequent finished product is formed. Due to the complex structure of the product, the mold is generally demolded by spraying a release agent, which pollutes the environment and cannot accurately control the film thickness. Summary of the invention
[0006] In view of the above problems, the purpose of the present invention is to provide a mold cleaning method and a processing and molding method, so as to solve the problems in the prior art that when cleaning the mold of a complex structural part product made of thermosetting composite materials, due to the small mold cavity and complex structure, a combination of manual polishing and solvent cleaning is used, which has the disadvantages of incomplete dirt cleaning, easy damage to the mold surface, affecting the size of the product appearance, and toxicity of organic solvents; and in the product production process, the mold after mold cleaning needs to be demolded by spraying a release agent on the mold surface after cleaning with an organic solvent, which pollutes the environment and the film thickness cannot be accurately controlled.
[0007] The present invention provides a mold cleaning method, comprising the following steps:
[0008] Adding primer into the hot pressing mold to be cleaned, softening the resin remaining on the inner wall of the hot pressing mold by hot pressing and vulcanizing the primer in the hot pressing mold, tearing off the hot pressing and vulcanized primer from the cavity surface of the hot pressing mold to take out part of the softened resin in the hot pressing mold, and completing the primary mold cleaning of the hot pressing mold;
[0009] Adding mold clearing glue into the hot pressing mold that has completed the primary mold clearing, allowing the mold clearing glue to be hot-pressed and vulcanized in the hot pressing mold, tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold to remove the remaining softened resin and other residual foreign matter in the hot pressing mold, and completing the intermediate mold clearing of the hot pressing mold;
[0010] Add silicone rubber mold lubricating glue containing a release agent component into the hot pressing mold that has completed the intermediate mold cleaning, and vulcanize the silicone rubber mold lubricating glue in the hot pressing mold under vacuum conditions, so that the release agent component precipitated by the vulcanization of the silicone rubber mold lubricating glue is dispersed on the surface of the mold cavity, and the vulcanized silicone rubber mold lubricating glue is taken out from the hot pressing mold to complete the mold cleaning of the hot pressing mold.
[0011] In addition, a preferred solution is that the step of adding a primer into the hot pressing mold to be cleaned and allowing the primer to be hot-pressed and vulcanized in the hot pressing mold to soften the resin remaining on the inner wall of the hot pressing mold comprises:
[0012] The hot pressing mold for taking out the hot pressing molded product is used as the hot pressing mold to be cleaned;
[0013] Adding a primer into the hot pressing mold to be cleaned, placing the hot pressing mold with the primer added at a first vulcanization temperature, and hot pressing and vulcanizing the primer in the pressing mold for a first vulcanization time to soften the resin remaining on the inner wall of the pressing mold;
[0014] Wherein, the first vulcanization temperature is the same as the product molding temperature when the hot pressing mold is used to process the product; the first vulcanization temperature ranges from 140°C to 180°C;
[0015] The first vulcanization time ranges from 3 min to 10 min.
[0016] In addition, a preferred solution is that the ingredients of the primer include unvulcanized rubber, detergent, filler, vulcanizer, and softener; wherein,
[0017] The unvulcanized rubber is a base rubber compounded with natural rubber and butadiene rubber in any proportion;
[0018] The cleaning agent is a high boiling point compound containing an amino group and / or a high boiling point compound containing an amine group;
[0019] The filler is any one of white carbon black, titanium dioxide, calcium carbonate, clay, talcum powder, or a mixture of several of them in any proportion;
[0020] The vulcanizing agent is one of sulfur, sulfur donor, peroxide, amine or a mixture of several of them in any proportion;
[0021] The softener is any one of aromatic oils, naphthenic oils and vaseline.
[0022] In addition, a preferred solution is that the mold clearing glue is added into the hot pressing mold that has completed the primary mold clearing, the mold clearing glue is hot-pressed and vulcanized in the hot pressing mold, and the vulcanized mold clearing glue is torn off from the mold cavity surface of the hot pressing mold to remove the remaining softened resin and other residual foreign matter in the hot pressing mold, thereby completing the intermediate mold clearing of the hot pressing mold, including:
[0023] Adding mold clearing glue into the hot pressing mold after the primary mold clearing, placing the hot pressing mold with the mold clearing glue at a second vulcanization temperature, allowing the mold clearing glue to be hot-pressed and vulcanized in the hot pressing mold for a second vulcanization time, and then tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold;
[0024] If after tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold, the mold cavity surface of the hot pressing mold is smooth and free of residual foreign matter, the intermediate mold clearing of the hot pressing mold is completed; otherwise, repeat the step of adding mold clearing glue into the hot pressing mold for hot pressing vulcanization until the mold cavity surface of the hot pressing mold is smooth and free of residual foreign matter, and the intermediate mold clearing of the hot pressing mold is completed; wherein,
[0025] The second vulcanization temperature is the same as the product molding temperature when the hot pressing mold is used to process the product; the second vulcanization temperature ranges from 140°C to 180°C;
[0026] The second vulcanization time ranges from 3 min to 10 min.
[0027] In addition, a preferred solution is that the components of the mold cleaning glue include unvulcanized rubber, a cleaning agent, a main filler, an auxiliary filler and a vulcanizing agent; wherein,
[0028] The unvulcanized rubber is a base rubber compounded with natural rubber and butadiene rubber in any proportion;
[0029] The cleaning agent is a high boiling point compound containing an amino group and / or a high boiling point compound containing an amine group;
[0030] The main filler is any one of white carbon black, titanium dioxide, calcium carbonate, clay, talcum powder, or a mixture of several of them in any proportion;
[0031] The auxiliary filler is zeolite powder with a porous structure
[0032] The vulcanizing agent is any one of sulfur, sulfur donor, peroxide and amine.
[0033] In addition, a preferred solution is that the hot pressing vulcanization temperature of the silicone rubber mold lubricant is the same as the product molding temperature when the hot pressing mold is used to process the product, and the hot pressing vulcanization temperature of the silicone rubber mold lubricant ranges from 100°C to 200°C; the hot pressing vulcanization time of the silicone rubber mold lubricant is 1min-10min.
[0034] In addition, a preferred solution is that the silicone rubber mold lubricant includes silicone rubber raw rubber, pre-treated filler, internal demoulding aid, self-lubricating aid, cross-linking agent and catalyst.
[0035] In addition, a preferred solution is that the silicone rubber is solid silicone rubber or liquid silicone rubber.
[0036] In addition, a preferred solution is that the pressure inside the hot pressing mold is the same during the hot pressing and vulcanization of the primer in the hot pressing mold, the hot pressing and vulcanization of the mold clearing glue in the hot pressing mold, and the hot pressing and vulcanization of the silicone rubber mold lubricating glue in the hot pressing mold.
[0037] The present invention provides a processing and molding method for a thermosetting composite material, which uses the mold cleaning method as described above to perform mold cleaning on a hot pressing mold, and during the product processing and molding process, the step of spraying a mold release agent is omitted.
[0038] It can be seen from the above technical scheme that the mold cleaning method and processing molding method provided by the present invention do not affect the mold cavity surface of the hot pressing mold by sequentially adding primer, mold cleaning glue and silicone rubber mold lubricating glue into the hot pressing mold for hot pressing and vulcanization, and cleaning the mold cavity surface of the hot pressing mold; first, the residual resin in the hot pressing mold is softened by the hot pressing and vulcanized primer, so that the adhesion of the softened resin to the metal surface of the mold cavity is reduced, and when the vulcanized primer is torn off from the mold cavity surface, part of the softened resin is taken out; then, the mold cleaning glue is bonded to the mold cavity by the hot pressing and vulcanized When the hot-pressed vulcanized mold clearing glue is torn off, the foreign matter precipitated from the surface of the mold cavity and the remaining softened resin are separated and removed together. Without unloading the mold, the complex mold cavity surface of the material mold used to produce electronic products can be thoroughly cleaned in all directions without dead ends; finally, the release agent component precipitated from the hot-pressed vulcanized silicone rubber mold lubricating glue is dispersed to the surface of the mold cavity, so that the hot-pressed mold after mold cleaning does not need to be sprayed with a release agent when producing thermosetting composite materials products, which effectively solves the problems of polluting the environment and being unable to accurately control the film thickness when demolding by spraying a release agent in the prior art.
[0039] In order to achieve the above and related purposes, one or more aspects of the present invention include the features that will be described in detail later. The following description and the accompanying drawings describe some exemplary aspects of the present invention in detail. However, these aspects indicate only some of the various ways in which the principles of the present invention can be used. In addition, the present invention is intended to include all these aspects and their equivalents. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] By referring to the following description in conjunction with the accompanying drawings, and with a more complete understanding of the present invention, other objects and results of the present invention will become more apparent and easily understood.
[0041] Figure 1 The present invention is a flowchart of a mold cleaning method according to an embodiment of the present invention. DETAILED DESCRIPTION
[0042] In the following description, for the purpose of explanation, numerous specific details are set forth in order to provide a thorough understanding of one or more embodiments. However, it is apparent that these embodiments may also be implemented without these specific details.
[0043] In view of the above-mentioned prior art, when cleaning the mold of a complex structural part product made of thermosetting composite materials, due to the small mold cavity and complex structure, a combination of manual polishing and solvent cleaning is used, which has the disadvantages of incomplete dirt cleaning, easy damage to the mold surface, affecting the size of the product appearance, and toxicity of organic solvents; and in the product production process, the mold after cleaning needs to be demolded by spraying a release agent on the mold surface after cleaning with an organic solvent, which pollutes the environment and cannot accurately control the film thickness. A mold cleaning method and a processing and molding method are proposed.
[0044] It should be noted that the mold in this solution is a mold in a hot pressing environment, particularly a thermosetting composite material mold, but the specific type of the mold is not specifically limited.
[0045] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0046] In order to illustrate the mold cleaning method and processing method of the thermosetting composite material mold provided by the present invention, Figure 1 The flowchart of the method for clearing a thermosetting composite material mold according to an embodiment of the present invention is shown.
[0047] like Figure 1 As shown, the mold cleaning method of the thermosetting composite material mold provided by the present invention comprises the following steps:
[0048] Step S1, add primer into the hot pressing mold to be cleared, soften the resin remaining on the inner wall of the hot pressing mold by hot pressing and vulcanizing the primer in the hot pressing mold, tear off the hot pressing and vulcanizing primer from the cavity surface of the hot pressing mold, take out the partially softened resin in the hot pressing mold, and complete the primary mold clearing of the hot pressing mold. Specifically, the hot pressing mold is generally attached with a certain resin and other foreign matter including fiber, release agent, etc. on its cavity surface after completing a product molding process. Add primer into the hot pressing mold to be cleared, the hot pressing mold to which the primer is added is under a high temperature environment, soften the residual resin in the hot pressing mold, and reduce the adhesion of resin on the metal mold cavity surface. When the primer is torn off from the cavity surface, the adhesion of the softened primer on the cavity is reduced, and the vulcanized primer is taken out, and at this time, the primary mold clearing of the hot pressing mold is completed.
[0049] As a preferred embodiment of the present invention, a primer is added into the hot pressing mold to be cleaned, and the resin remaining on the inner wall of the hot pressing mold is softened by hot pressing and vulcanizing the primer in the hot pressing mold, comprising:
[0050] The hot pressing mold for taking out the hot pressing molded product is used as the hot pressing mold to be cleaned;
[0051] Adding primer into the hot pressing mold to be cleaned, placing the hot pressing mold with the primer added at a first vulcanization temperature, and hot pressing and vulcanizing the primer in the hot pressing mold for a first vulcanization time to soften the resin remaining on the inner wall of the pressing mold;
[0052] The first vulcanization temperature is the same as the product molding temperature when the product is processed by the hot pressing mold; the first vulcanization temperature ranges from 140° C. to 180° C.; and the first vulcanization time ranges from 3 min to 10 min.
[0053] Specifically, after the hot pressing mold completes the hot pressing molding of the product and takes out the molded product, it is necessary to perform mold cleaning on the inside of the mold. The hot pressing mold after each use is used as the hot pressing mold to be cleaned, and primer is added to the inside. The hot pressing mold with primer added is placed at the first vulcanization temperature, so that the primer in the hot pressing mold is hot-pressed and vulcanized in the mold at the first vulcanization temperature until the first vulcanization time is reached. The higher the first vulcanization temperature, the shorter the first vulcanization time. The first vulcanization temperature is the same as the product molding temperature when the hot pressing mold is used to process the product, so as to ensure that the hot pressing and vulcanization of the primer in the hot pressing mold can soften the resin remaining in the mold. The specific first vulcanization temperature needs to be determined according to the product molding temperature. When the first vulcanization temperature ranges from 140℃ to 180℃, the primary mold cleaning effect of the primer is the best. If the temperature is too low, the primer vulcanization is easy to be incomplete, affecting the softening effect on the resin. If the temperature is too high, the tear strength of the vulcanized primer is too low, and when it is torn off from the surface of the mold cavity, debris will be left. However, it should be noted that the limitation of the first vulcanization temperature in the present invention does not mean that the mold cleaning solution provided by the present invention cannot be used outside this temperature range. The first vulcanization temperature and the first vulcanization time specified in the present invention are merely a preferred embodiment of the present invention.
[0054] As a preferred embodiment of the present invention, the ingredients of the primer include unvulcanized rubber, detergent, filler, vulcanizer, and softener; wherein,
[0055] Unvulcanized rubber is a base rubber compounded with natural rubber and butadiene rubber in any proportion;
[0056] The cleaning agent is a high boiling point compound containing an amino group and / or a high boiling point compound containing an amine group;
[0057] The filler is any one of white carbon black, titanium dioxide, calcium carbonate, clay, talcum powder, or a mixture of several of them in any proportion;
[0058] The vulcanizing agent is one of sulfur, sulfur donor, peroxide, amine or a mixture of the above in any proportion;
[0059] The softener is any one of aromatic oils, naphthenic oils and vaseline.
[0060] Specifically, the ingredients of the primer used in the present invention include but are not limited to unvulcanized rubber, detergent, filler, vulcanizer, softener, and may also include vulcanization auxiliaries and other auxiliaries.
[0061] Wherein, the unvulcanized rubber is a base rubber compounded with natural rubber and cis-1,4-dibutyl rubber in any proportion. For example, the unvulcanized rubber is a base rubber compounded with natural rubber and cis-1,4-dibutyl rubber in a ratio of 1:1. The cleaning agent is a high-boiling compound containing amino and / or amine groups, such as ethanolamine, diethanolamine and triethanolamine, etc.; it can also be an ether compound or alcohol ether compound containing an ether bond, such as ethylene glycol methyl ether, diethylene glycol butyl ether, ethylene glycol phenyl ether and dipropylene glycol, etc., and can also be a high-boiling organic small molecule compound, such as benzyl alcohol, N-methyl pyrrolidone, etc.; the filler is any one of white carbon black, titanium dioxide, calcium carbonate, clay, talc or several mixed in any proportion; the vulcanizing agent can be sulfur, sulfur donor, peroxide, amines and other substances for vulcanization, but because the sulfur vulcanization process has a large odor, the present invention preferably uses a peroxide vulcanization system. There are many varieties of peroxides in the peroxide vulcanization system, generally including diisopropylbenzene peroxide (DCP), di-tert-butyl peroxide isopropylbenzene (BIPB), di-tert-butyl peroxide (DPBP) and benzoyl peroxide (BPO), etc. The ingredients of the primer may also include a co-crosslinking agent, such as tripropylene isocyanurate (TAIC); the softener may be selected from aromatic oils, naphthenic oils, vaseline, etc. Other additives such as antioxidants, anti-aging agents, stabilizers, and release agents may also be included. The present invention does not specifically limit the specific formula of the primer.
[0062] Step S2, adding mold clearing glue into the hot pressing mold that has completed the primary mold clearing, allowing the mold clearing glue to be hot-pressed and vulcanized in the hot pressing mold, tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold to remove the remaining softened resin and other residual foreign matter in the hot pressing mold, and completing the intermediate mold clearing of the hot pressing mold.
[0063] Specifically, mold clearing glue is added to the hot pressing mold that has completed the primary mold clearing, and the hot pressing mold with the mold clearing glue is placed at high temperature to vulcanize the mold clearing glue in the hot pressing mold. When the vulcanized mold clearing glue is torn off from the mold cavity surface of the mold, the fibers, mold release agents, precipitated dirt and other foreign matters remaining on the mold cavity surface are removed together with the remaining softened resin. Ensure that the mold cavity surface of the hot pressing mold is smooth and clean, and the intermediate mold clearing of the hot pressing mold is completed.
[0064] The mechanism of action of mold cleaning glue on the cavity surface of hot pressing mold is:
[0065] Physical bonding: The rubber component in the mold cleaning glue is sticky, and the dirt on the surface of the mold cavity is adhered and removed;
[0066] Chemical bonding: The highly active functional groups in the mold cleaning glue react with the dirt to remove the dirt from the mold cavity surface.
[0067] Mechanical grinding: The abrasive in the mold cleaning glue is used to grind, scrub and flush the dirt on the surface of the mold cavity so that the dirt falls off the surface of the mold cavity;
[0068] Decomposition: The solvent in the mold cleaning glue component is used to decompose the dirt to thoroughly clean the bottom layer of dirt on the surface of the mold cavity.
[0069] As a preferred embodiment of the present invention, mold clearing glue is added into the hot pressing mold after primary mold clearing, the mold clearing glue is hot-pressed and vulcanized in the hot pressing mold, and the vulcanized mold clearing glue is torn off from the mold cavity surface of the hot pressing mold to remove the remaining softened resin and other residual foreign matter in the hot pressing mold, thereby completing the intermediate mold clearing of the hot pressing mold, including:
[0070] Adding mold clearing glue into the hot pressing mold after primary mold clearing, placing the hot pressing mold with the mold clearing glue at a second vulcanization temperature, allowing the mold clearing glue to be hot-pressed and vulcanized in the pressing mold for a second vulcanization time, and then tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold;
[0071] If the mold cavity surface of the hot pressing mold is smooth and free of residual foreign matter after the vulcanized mold clearing glue is torn off from the mold cavity surface of the hot pressing mold, the intermediate mold clearing of the hot pressing mold is completed; otherwise, the steps of adding mold clearing glue to the hot pressing mold for hot pressing vulcanization are repeated until the mold cavity surface of the hot pressing mold is smooth and free of residual foreign matter, and the intermediate mold clearing of the hot pressing mold is completed; wherein,
[0072] The second vulcanization temperature is the same as the product molding temperature when the product is processed by the hot pressing mold; the second vulcanization temperature ranges from 140°C to 180°C; and the second vulcanization time ranges from 3min to 10min.
[0073] Specifically, mold clearing glue is added to the hot pressing mold that has completed the primary mold clearing, and the hot pressing mold with the mold clearing glue is placed at a second vulcanization temperature, so that the mold clearing glue is hot-pressed and vulcanized in the hot pressing mold to the second vulcanization time, and the vulcanized mold clearing glue is attached to the cavity surface of the hot pressing mold. When the vulcanized mold clearing glue is torn off from the cavity surface of the hot pressing mold, the fibers, release agents, precipitated dirt and other foreign matter remaining on the cavity surface and the remaining softened resin can be removed at the same time. However, it is possible that the cavity surface cannot be smooth and free of residue after one mold clearing glue vulcanization operation. Therefore, it is necessary to determine whether the intermediate mold clearing is completed by observation. If the cavity surface of the hot pressing mold is smooth and free of residual foreign matter after the vulcanized mold clearing glue is torn off from the cavity surface of the hot pressing mold, the intermediate mold clearing of the hot pressing mold is completed. Otherwise, it is necessary to repeat the steps of adding mold clearing glue to the hot pressing mold, hot-pressing and vulcanizing, and then tearing it off until the cavity surface of the hot pressing mold is smooth and free of residual foreign matter, and the intermediate mold clearing of the hot pressing mold is completed.
[0074] The higher the second vulcanization temperature, the shorter the second vulcanization time. The second vulcanization temperature is the same as the product molding temperature when the hot pressing mold is used to process the product. The preferred range is 140°C-180°C. The intermediate mold clearing effect of the mold clearing glue is the best. If the temperature is too low, the mold clearing glue will be incompletely vulcanized, affecting the adsorption effect on the softened resin and other residual foreign matter. If the temperature is too high, the tear strength of the vulcanized mold clearing glue will be too low, leaving debris when it is torn off from the mold cavity surface. However, it should be noted that the limitation of the second vulcanization temperature in the present invention does not mean that the mold clearing scheme provided by the present invention cannot be adopted outside this temperature range. The first vulcanization temperature and the first vulcanization time defined in the present invention are only used as a preferred embodiment of the present invention.
[0075] As a preferred embodiment of the present invention, the components of the mold cleaning rubber include unvulcanized rubber, a cleaning agent, a main filler, an auxiliary filler and a vulcanizing agent; wherein,
[0076] Unvulcanized rubber is a base rubber compounded with natural rubber and butadiene rubber in any proportion;
[0077] The cleaning agent is a high boiling point compound containing an amino group and / or a high boiling point compound containing an amine group;
[0078] The main filler is any one of white carbon black, titanium dioxide, calcium carbonate, clay, talcum powder, or a mixture of several of them in any proportion;
[0079] The auxiliary filler is a zeolite powder with a porous "molecular sieve" structure.
[0080] The vulcanizing agent is any one of sulfur, a sulfur donor, a peroxide, and an amine.
[0081] Specifically, the components of the mold cleaning glue include, but are not limited to, unvulcanized rubber, detergent, filler, and vulcanizing agent. For example, it may also include vulcanizing auxiliaries and other auxiliaries.
[0082] Unvulcanized rubber is a base rubber compounded with natural rubber and cis-1,4-dibutyl rubber in any proportion, for example, a base rubber compounded with natural rubber and cis-1,4-dibutyl rubber in a ratio of 1:1. Cleaning agent is a high boiling point compound containing amino and / or amine groups, such as ethanolamine, diethanolamine and triethanolamine, etc.; or an ether compound or alcohol ether compound containing an ether bond, such as ethylene glycol methyl ether, diethylene glycol butyl ether, ethylene glycol phenyl ether and dipropylene glycol, etc., or a high boiling point organic small molecule compound, such as any one of benzyl alcohol, N-methyl pyrrolidone, etc. or several mixed in any proportion; the main filler is any one of white carbon black, titanium dioxide, calcium carbonate, clay, talc or several mixed in any proportion, which can be used as the main reinforcing filler, and the auxiliary filler is a zeolite powder of a molecular sieve structure. Vulcanizing agent can be selected from sulfur, sulfur donor, peroxide, amines and other substances for vulcanization, but due to the large smell during sulfur vulcanization, the present invention preferably uses a peroxide vulcanization system. There are many varieties of peroxides, including diisopropylbenzene peroxide (DCP), di-tert-butyl peroxide isopropylbenzene (BIPB), di-tert-butyl peroxide (DPBP) and benzoyl peroxide (BPO); the mold clearing glue may also include a cross-linking agent, such as tripropylene isocyanurate (TAIC); and may also include antioxidants, anti-aging agents, stabilizers, release agents and other auxiliary agents. The present invention does not specifically limit the specific composition formula of the mold clearing glue.
[0083] Step S3, adding silicone rubber mold lubricating glue containing a release agent component into the hot pressing mold that has completed the intermediate mold cleaning, and vulcanizing the silicone rubber mold lubricating glue in the hot pressing mold under vacuum conditions, so that the release agent component precipitated by the vulcanization of the silicone rubber mold lubricating glue is dispersed onto the surface of the mold cavity, and the vulcanized silicone rubber mold lubricating glue is taken out from the hot pressing mold to complete the mold cleaning of the hot pressing mold.
[0084] Specifically, silicone rubber mold lubrication glue has good fluidity and is especially suitable for complex structural parts. It does not break during demoulding and there is no residual glue in the mold after cleaning. It can be completely cleaned in one mold, and demoulding can be achieved without spraying a release agent when producing products.
[0085] As a preferred embodiment of the present invention, the hot pressing vulcanization temperature of the silicone rubber mold lubricant is the same as the product molding temperature when the hot pressing mold is used to process the product, and the hot pressing vulcanization temperature of the silicone rubber mold lubricant ranges from 100°C to 200°C; the hot pressing vulcanization time of the silicone rubber mold lubricant is 1min to 10min.
[0086] Specifically, the higher the hot press vulcanization temperature, the shorter the hot press vulcanization time. The specific hot press vulcanization temperature needs to be determined according to the product molding temperature. Silicone rubber has a large vulcanization temperature gradient and can be used at low temperatures. Generally, rubber vulcanization requires a higher temperature, generally > 140°C, and a long vulcanization time.
[0087] As a preferred embodiment of the present invention, the silicone rubber mold lubricant comprises silicone rubber raw rubber, pre-treated filler, internal demoulding aid, self-lubricating aid, cross-linking agent and catalyst.
[0088] Specifically, the components of the silicone rubber mold lubricant used in the present invention include but are not limited to silicone rubber raw rubber, pre-treated filler, internal mold release agent, self-lubricating agent, cross-linking agent and catalyst. The silicone rubber mold lubricant in the scheme of the present invention can be added to the silicone rubber raw rubber. The mold release agent component (internal mold release agent) that does not participate in the chemical reaction is compounded with a fluorine mold release agent, a silicone oil mold release agent and a paraffin mold release agent to achieve the effect of mold lubrication and demolding. The mold release agent precipitates during the vulcanization of the silicone rubber and disperses on the surface of the mold cavity. When producing thermosetting carbon fiber composites, there is no need to apply a mold release agent. Most of the mold lubricants on the market are rubbers, and the operating temperature is high. The general vulcanization temperature is 140-180°C, and the mold lubrication effect is achieved by using the precipitation of the mold release agent after the vulcanization of the rubber, but the demolding effect cannot be achieved. The mold release agent needs to be applied when producing products.
[0089] As a preferred embodiment of the present invention, the silicone rubber is solid silicone rubber or liquid silicone rubber.
[0090] As a preferred embodiment of the present invention, the thermosetting composite material is a thermosetting carbon fiber composite material.
[0091] As a preferred embodiment of the present invention, the pressure inside the hot pressing mold is the same during the hot pressing and vulcanization of the primer glue in the hot pressing mold, the hot pressing and vulcanization of the mold clearing glue in the hot pressing mold, and the hot pressing and vulcanization of the silicone rubber mold lubricating glue in the hot pressing mold.
[0092] Specifically, during the hot pressing and vulcanization of the primer, during the hot pressing and vulcanization of the mold cleaning glue, and during the hot pressing and vulcanization of the silicone rubber mold lubricating glue, the pressure value in the hot pressing mold can be any pressure value, and the present invention does not make any special restrictions on this. Preferably, but not limited to, 30-50 kgf / cm2.
[0093] The processing and molding method of the thermosetting composite material provided by the present invention adopts the mold cleaning method of the thermosetting composite material mold as described above to clean the hot pressing mold, and the step of spraying the release agent is omitted during the product processing and molding process.
[0094] Specifically, the processing and forming method of the thermosetting composite material provided by the present invention adopts the mold cleaning method of the thermosetting composite material mold as described above to clean the hot pressing mold, and the subsequent product processing and forming process can adopt the existing processing and forming steps except for omitting the step of spraying the release agent.
[0095] For example, lay up fiber-reinforced materials → place in a pressurized mold → inject resin or prepreg → vacuum seal → heat and pressurize to solidify the resin → cool and demould → post-processing.
[0096] In order to better explain the mold cleaning method and processing method of the thermosetting composite material mold provided by the present invention in detail, the following examples are given:
[0097] Example 1
[0098] The residues in the hot pressing mold are epoxy resin, residual fibers, release agents and other foreign matter. When the hot pressing mold is used to process the product, the molding temperature of the product is 160°C.
[0099] Step S1, adding primer to the hot pressing mold to be cleaned, placing the hot pressing mold with the primer in an environment of 160° C., hot pressing and vulcanizing the primer in the hot pressing mold for 7 minutes, taking out the vulcanized primer, and taking out part of the softened resin in the hot pressing mold, thereby completing the primary mold cleaning of the hot pressing mold;
[0100] Step S2, adding mold clearing glue into the hot pressing mold after primary mold clearing, placing the hot pressing mold with the mold clearing glue in an environment of 160° C., hot pressing and vulcanizing the mold clearing glue in the hot pressing mold for 7 minutes, tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold, and the surface of the hot pressing mold is smooth, clean and free of residue, and the intermediate mold clearing of the hot pressing mold is completed at this time;
[0101] Step S3, adding silicone rubber mold lubricating glue containing a release agent component into the hot pressing mold that has completed the intermediate mold cleaning, placing the hot pressing mold with the silicone rubber mold lubricating glue in a vacuum environment at a temperature of 160°C, and hot-pressing and vulcanizing the silicone rubber mold lubricating glue containing a release agent component in the hot pressing mold for 5 minutes, repeating this operation twice, and completing the mold cleaning process of the hot pressing mold.
[0102] After the above-mentioned mold cleaning step, the surface of the hot pressing mold is free of foreign matter, smooth and clean, and in the subsequent use process, when the mold release agent is not sprayed, a good demoulding effect can be achieved.
[0103] Example 2
[0104] The residues in the hot press mold are epoxy resin, residual fibers, release agents and other foreign matter. When the hot press mold is used to process the product, the molding temperature of the product is 140°C.
[0105] Step S1, adding primer to the hot pressing mold to be cleaned, placing the hot pressing mold with the primer in an environment of 140° C., hot pressing and vulcanizing the primer in the hot pressing mold for 10 minutes, taking out the vulcanized primer, and taking out part of the softened resin in the hot pressing mold, thereby completing the primary mold cleaning of the hot pressing mold;
[0106] Step S2, adding mold clearing glue to the hot pressing mold that has completed the primary mold clearing, placing the hot pressing mold with the mold clearing glue in an environment of 140° C., hot pressing and vulcanizing the mold clearing glue in the hot pressing mold for 10 minutes, tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold, repeating this operation three times, the surface of the hot pressing mold is smooth, clean and free of residue, and the intermediate mold clearing of the hot pressing mold is completed at this time;
[0107] Step S3, adding silicone rubber mold lubricating glue containing a release agent component into the hot pressing mold that has completed the intermediate mold cleaning, placing the hot pressing mold with the silicone rubber mold lubricating glue in a vacuum environment at a temperature of 140°C, and hot-pressing and vulcanizing the silicone rubber mold lubricating glue containing a release agent component in the hot pressing mold for 10 minutes, repeating this operation three times to complete the mold cleaning process of the hot pressing mold.
[0108] After the above-mentioned mold cleaning step, the surface of the hot pressing mold is free of foreign matter, smooth and clean, and in the subsequent use process, when the mold release agent is not sprayed, a good demoulding effect can be achieved.
[0109] Example 3
[0110] The residues in the hot pressing mold are epoxy resin, residual fibers, release agents and other foreign matter. When the hot pressing mold is used to process the product, the molding temperature of the product is 180℃.
[0111] Step S1, adding primer to the hot pressing mold to be cleaned, placing the hot pressing mold with the primer in an environment of 180° C., hot pressing and vulcanizing the primer in the hot pressing mold for 3 minutes, taking out the vulcanized primer, and taking out part of the softened resin in the hot pressing mold, thereby completing the primary mold cleaning of the hot pressing mold;
[0112] Step S2, adding mold clearing glue to the hot pressing mold that has completed the primary mold clearing, placing the hot pressing mold with the mold clearing glue in an environment of 180° C., hot pressing and vulcanizing the mold clearing glue in the hot pressing mold for 3 minutes, tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold, repeating this operation twice, the surface of the hot pressing mold is smooth, clean and free of residue, and the intermediate mold clearing of the hot pressing mold is completed at this time;
[0113] Step S3, add silicone rubber mold lubricating glue containing a release agent component into the hot pressing mold that has completed the intermediate mold cleaning, place the hot pressing mold with the silicone rubber mold lubricating glue in a vacuum environment at a temperature of 180°C, and hot-press vulcanize the silicone rubber mold lubricating glue containing a release agent component in the hot pressing mold for 1 minute. Repeat this operation three times to complete the mold cleaning process of the hot pressing mold.
[0114] After the above-mentioned mold cleaning step, the surface of the hot pressing mold is free of foreign matter, smooth and clean, and in the subsequent use process, when the mold release agent is not sprayed, a good demoulding effect can be achieved.
[0115] Example 4
[0116] The residues in the hot pressing mold are epoxy resin, residual fibers, release agents and other foreign matter. When the hot pressing mold is used to process the product, the molding temperature of the product is 120℃.
[0117] Step S1, adding primer to the hot pressing mold to be cleaned, placing the hot pressing mold with the primer in an environment of 120° C., hot pressing and vulcanizing the primer in the hot pressing mold for 15 minutes, taking out the vulcanized primer, and taking out a small amount of softened resin in the hot pressing mold, thereby completing the primary mold cleaning of the hot pressing mold;
[0118] Step S2, adding mold clearing glue to the hot pressing mold that has completed the primary mold clearing, placing the hot pressing mold with the mold clearing glue in an environment of 120° C., hot pressing and vulcanizing the mold clearing glue in the hot pressing mold for 15 minutes, tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold, repeating this operation three times, there is still some residue on the surface of the hot pressing mold, continue to repeat the above steps S1 and S2 for fifteen and twelve times respectively, the surface of the hot pressing mold is smooth, clean and free of residue, and the intermediate mold clearing of the hot pressing mold is completed at this time;
[0119] Step S3, adding silicone rubber mold lubricating glue containing a release agent component into the hot pressing mold that has completed the intermediate mold cleaning, placing the hot pressing mold with the silicone rubber mold lubricating glue in a vacuum environment at a temperature of 120°C, and hot-pressing and vulcanizing the silicone rubber mold lubricating glue containing a release agent component in the hot pressing mold for 12 minutes, repeating this operation three times to complete the mold cleaning process of the hot pressing mold.
[0120] Although the hot pressing mold after the above-mentioned mold cleaning step can achieve the effect of no foreign matter remaining on the surface and being smooth and clean, it is necessary to repeat steps S1 and S2 multiple times to achieve the effect of no foreign matter remaining on the surface. In the subsequent use process, when the release agent is not sprayed, a better demolding effect can also be achieved.
[0121] Example 5
[0122] The residues in the hot pressing mold are epoxy resin, residual fibers, release agents and other foreign matter. When the hot pressing mold is used to process the product, the molding temperature of the product is 200℃.
[0123] Step S1, adding primer to the hot pressing mold to be cleaned, placing the hot pressing mold with the primer in an environment of 200° C., hot pressing and vulcanizing the primer in the hot pressing mold for 2 minutes, and when taking out the vulcanized primer, it is found that the tear strength of the vulcanized primer on the surface of the mold cavity decreases, and there are debris in the tearing process, and the operation of cleaning the debris needs to be added, and the primary mold cleaning of the hot pressing mold is completed;
[0124] Step S2, adding mold clearing glue to the hot pressing mold that has completed the primary mold clearing, placing the hot pressing mold with the mold clearing glue in an environment of 200° C., hot pressing and vulcanizing the mold clearing glue in the hot pressing mold for 2 minutes, and tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold. It is found that the vulcanized mold clearing glue has a decreased tear strength, and there are debris in the tearing process, and an operation of cleaning the debris needs to be increased. After repeating this step ten times, the surface of the hot pressing mold can be smooth, clean and free of residue, and the intermediate mold clearing of the hot pressing mold is completed at this time;
[0125] Step S3, adding silicone rubber mold lubricating glue containing a release agent component into the hot pressing mold that has completed the intermediate mold cleaning, placing the hot pressing mold with the silicone rubber mold lubricating glue in a vacuum environment at a temperature of 200°C, and hot-pressing and vulcanizing the silicone rubber mold lubricating glue containing a release agent component in the hot pressing mold for 1 minute, repeating this operation twice, and completing the mold cleaning process of the hot pressing mold.
[0126] Although the hot pressing mold after the above-mentioned mold cleaning step can achieve a surface free of foreign matter and smooth and clean, a debris cleaning step needs to be added during step S1 and step S2, and the operation of step S2 needs to be repeated multiple times; in the subsequent use process, when the release agent is not sprayed, a better demolding effect can also be achieved.
[0127] It should be noted that this embodiment is only for the purpose of describing in detail the mold cleaning method and processing method of the thermosetting composite material mold provided by the present invention in practical application, and does not limit the technical solution provided by the present invention.
[0128] It can be seen from the above specific implementation methods that the mold cleaning method and processing method of the thermosetting composite material mold provided by the present invention, from the above technical scheme, it can be seen that the mold cleaning method and processing method of the thermosetting composite material mold provided by the present invention, by sequentially adding primer hot pressing vulcanization, mold cleaning glue hot pressing vulcanization and silicone rubber mold lubrication glue hot pressing vulcanization into the hot pressing mold to clean the mold cavity surface of the hot pressing mold, will not affect the mold cavity surface of the hot pressing mold; first, the hot pressing vulcanized primer is used to soften the residual resin in the hot pressing mold, so that the adhesion of the softened resin to the metal surface of the mold cavity is reduced, and when the vulcanized primer is torn off from the mold cavity surface, part of the resin is taken out The mold cleaning glue is used to soften the resin; it is then adhered to the surface of the mold cavity by hot-pressing vulcanized mold cleaning glue. When the hot-pressing vulcanized mold cleaning glue is torn off, the foreign matter precipitated from the surface of the mold cavity and the remaining softened resin are separated and removed together. There is no need to unload the mold, and the complex mold cavity surface of the thermosetting composite material mold used in the production of electronic products can be thoroughly cleaned in all directions without dead ends; finally, the mold release agent component precipitated from the hot-pressing vulcanized silicone rubber mold lubricating glue is dispersed to the surface of the mold cavity, so that the hot-pressing mold after mold cleaning does not need to be sprayed with a mold release agent when producing thermosetting composite material products, which effectively solves the problems of environmental pollution and inability to accurately control film thickness in the prior art when demolding by spraying a mold release agent.
[0129] As described above with reference to the accompanying drawings, the mold clearing method and processing method of the thermosetting composite material mold proposed in the present invention are described by way of example. However, those skilled in the art should understand that various improvements can be made to the mold clearing method and processing method of the thermosetting composite material mold proposed in the present invention without departing from the content of the present invention. Therefore, the protection scope of the present invention should be determined by the content of the attached claims.
Claims
1. A mold cleaning method, characterized in that: The steps include: Adding primer into the hot pressing mold to be cleaned, softening the resin remaining on the inner wall of the hot pressing mold by hot pressing and vulcanizing the primer in the hot pressing mold, tearing off the hot pressing and vulcanized primer from the cavity surface of the hot pressing mold to take out part of the softened resin in the hot pressing mold, and completing the primary mold cleaning of the hot pressing mold; Adding mold clearing glue into the hot pressing mold that has completed the primary mold clearing, allowing the mold clearing glue to be hot-pressed and vulcanized in the hot pressing mold, tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold to remove the remaining softened resin and other residual foreign matter in the hot pressing mold, and completing the intermediate mold clearing of the hot pressing mold; Add silicone rubber mold lubricating glue containing a release agent component into the hot pressing mold that has completed the intermediate mold cleaning, and vulcanize the silicone rubber mold lubricating glue in the hot pressing mold under vacuum conditions, so that the release agent component precipitated by the vulcanization of the silicone rubber mold lubricating glue is dispersed on the surface of the mold cavity, and the vulcanized silicone rubber mold lubricating glue is taken out from the hot pressing mold to complete the mold cleaning of the hot pressing mold.
2. The mold cleaning method according to claim 1, characterized in that: The step of adding a primer into the hot pressing mold to be cleaned and allowing the primer to be hot-pressed and vulcanized in the hot pressing mold to soften the resin remaining on the inner wall of the hot pressing mold comprises: The hot pressing mold for taking out the hot pressing molded product is used as the hot pressing mold to be cleaned; Adding a primer into the hot pressing mold to be cleaned, placing the hot pressing mold with the primer added at a first vulcanization temperature, and hot pressing and vulcanizing the primer in the pressing mold for a first vulcanization time to soften the resin remaining on the inner wall of the pressing mold; Wherein, the first vulcanization temperature is the same as the product molding temperature when the hot pressing mold is used to process the product; the first vulcanization temperature ranges from 140°C to 180°C; The first vulcanization time ranges from 3 min to 10 min.
3. The mold cleaning method according to claim 1, characterized in that: The ingredients of the primer include unvulcanized rubber, detergent, filler, vulcanizer, and softener; wherein, The unvulcanized rubber is a base rubber compounded with natural rubber and butadiene rubber in any proportion; The cleaning agent is a high boiling point compound containing an amino group and / or a high boiling point compound containing an amine group; The filler is any one of white carbon black, titanium dioxide, calcium carbonate, clay, talcum powder, or a mixture of several of them in any proportion; The vulcanizing agent is one of sulfur, sulfur donor, peroxide, amine or a mixture of several of them in any proportion; The softener is any one of aromatic oils, naphthenic oils and vaseline.
4. The mold cleaning method according to claim 1, characterized in that: The method includes adding mold clearing glue into the hot pressing mold that has completed the primary mold clearing, vulcanizing the mold clearing glue in the hot pressing mold, tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold to remove the remaining softened resin and other residual foreign matter in the hot pressing mold, and completing the intermediate mold clearing of the hot pressing mold, including: Adding mold clearing glue into the hot pressing mold after the primary mold clearing, placing the hot pressing mold with the mold clearing glue at a second vulcanization temperature, allowing the mold clearing glue to be hot-pressed and vulcanized in the hot pressing mold for a second vulcanization time, and then tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold; If after tearing off the vulcanized mold clearing glue from the mold cavity surface of the hot pressing mold, the mold cavity surface of the hot pressing mold is smooth and free of residual foreign matter, the intermediate mold clearing of the hot pressing mold is completed; otherwise, repeat the step of adding mold clearing glue into the hot pressing mold for hot pressing vulcanization until the mold cavity surface of the hot pressing mold is smooth and free of residual foreign matter, and the intermediate mold clearing of the hot pressing mold is completed; wherein, The second vulcanization temperature is the same as the product molding temperature when the hot pressing mold is used to process the product; the second vulcanization temperature ranges from 140°C to 180°C; The second vulcanization time ranges from 3 min to 10 min.
5. The mold cleaning method according to claim 1, characterized in that: The components of the mold cleaning glue include unvulcanized rubber, cleaning agent, main filler, auxiliary filler and vulcanizing agent; wherein, The unvulcanized rubber is a base rubber compounded with natural rubber and butadiene rubber in any proportion; The cleaning agent is a high boiling point compound containing an amino group and / or a high boiling point compound containing an amine group; The main filler is any one of white carbon black, titanium dioxide, calcium carbonate, clay, talcum powder, or a mixture of several of them in any proportion; The auxiliary filler is zeolite powder with a porous structure The vulcanizing agent is any one of sulfur, sulfur donor, peroxide and amine.
6. The mold cleaning method according to claim 1, characterized in that: The hot pressing vulcanization temperature of the silicone rubber mold lubricant is the same as the product molding temperature when the hot pressing mold is used to process the product, and the hot pressing vulcanization temperature of the silicone rubber mold lubricant is in the range of 100° C.-200° C.; The hot pressing vulcanization time of the silicone rubber mold lubricant is 1 min-10 min.
7. The mold cleaning method according to claim 1, characterized in that: The silicone rubber mold lubricant comprises silicone rubber raw rubber, pre-treated filler, internal demoulding aid, self-lubricating aid, cross-linking agent and catalyst.
8. The mold cleaning method according to claim 7, characterized in that: The silicone rubber is solid silicone rubber or liquid silicone rubber.
9. The mold cleaning method according to claim 1, characterized in that: During the hot pressing and vulcanization of the primer in the hot pressing mold, the hot pressing and vulcanization of the mold clearing glue in the hot pressing mold, and the hot pressing and vulcanization of the silicone rubber mold lubricating glue in the hot pressing mold, the pressure in the hot pressing mold is the same.
10. A method for processing and molding a thermosetting composite material, characterized in that: The hot pressing mold is cleaned by using the mold cleaning method as described in any one of claims 1 to 9, and the step of spraying a mold release agent is omitted during the product processing and molding process.
Citation Information
Cited By
Mold moistening method for exhaust port of IC plastic package mold
CN122378988A