Mine truck tire body fractional vulcanization forming retreading method and device

Through the refurbishment method of carcass of mine-card tires, the problem of steel wire and inner tube breaking of belt layers after large-scale truck tires is renovated is solved, the service life and quality of the refurbished tires are improved, and more efficient resource circulation is achieved use.

CN119078259APending Publication Date: 2024-12-06GAOAN HENGXIN TIRE RETREADING FACTORY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411437185.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing tire renovation technology is difficult to effectively solve the problems of steel wires, inner tube breakage and tread delamination of the belt tires after renovation, resulting in a short service life of refurbished tires and unable to meet production needs.

Method used

The carcass carcass of mineral trucks is renovated by the secondary vulcanization molding and renovation method, including the primary vulcanization mold device, the press device and the secondary vulcanization tank device. Through the secondary vulcanization treatment and the press processing, the belt layer and the tread layer are enhanced. Adhesion force forms a more stable carcass structure.

Benefits of technology

It significantly improves the service life and quality of refurbished tires, extends the service time of refurbished tires, enhances tear resistance and wear resistance, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119078259A_ABST
    Figure CN119078259A_ABST
Patent Text Reader

Abstract

The invention discloses a mine truck tire body fractional vulcanization molding retreading method and device, which is a process for performing secondary vulcanization molding retreading treatment on a retreaded tire body, and comprises a primary vulcanization mold device, a pressing machine device and a secondary vulcanization tank device, according to the renovated mine truck tire, the renovated mine truck tire can be prepared by controlling technological parameters of secondary vulcanization treatment on the renovated tire body and pressing the secondary vulcanization tire body by adopting a pressing machine device, so that the phenomenon that the inner tire is punctured due to the fact that a belt steel wire moves into the tire body can be effectively prevented; the service life of the retreaded mine truck tire is greatly prolonged, the preparation process and the pressing device are simple, and the comprehensive preparation and use cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the field of tire retreading technology and devices, mainly to a process method and device for retreading heavy-duty truck tires, and in particular to a method and device for retreading mining truck tires by step vulcanization molding. Background technology:

[0002] Heavy-duty trucks used in mines, such as mining trucks, are also called mining trucks or mining trucks for transportation. Their working environment is usually relatively harsh. There are many gravels on the working site road surface, and various sharp objects such as nails and iron sheets will cause great damage to the tires. Therefore, the tires used for mining trucks and engineering machinery are generally easy to damage. Therefore, the easily damaged tires used for mining trucks are relatively large in size and use a lot of materials, so their cost is also high. According to the current price, each tire used for mining trucks costs more than 10,000 yuan or even more than 20,000 yuan. Directly discarding the damaged tires used for old mining tires and engineering machinery will not only waste raw materials, but also easily cause pollution to the environment. Therefore, in order to control the use cost of mining truck tires, refurbishing and reusing the old mining truck tires is the best way to reduce the use cost of heavy-duty trucks, and it can also be recycled, environmentally friendly and economical.

[0003] As disclosed in the Chinese patent application publication number CN 110014681 A, the invention titled "A Method for Renovating Engineering Machinery Tires" discloses a method for retreading engineering machinery tires, which comprises sleeve-joining and gluing two old tires of suitable sizes, one large and one small, together. After adopting the above scheme, the two old tires are retreaded into a new tire with both the tread and the sidewalls nearly doubled in thickness. The integrated sidewall not only doubles the load-bearing capacity, but also greatly increases the impact resistance. Even if the original outer tire is damaged, it will not affect the use because it is the same body as the inner tire.

[0004] Chinese patent CN 112606454, the disclosed invention name is "A method for tire retreading", the present invention discloses a method for tire retreading, comprising the following steps: (1) fixing the tire by means of a detection device, and detecting the through holes on the tire and the nails stuck on the tire surface; (2) after removing the nails on the tire surface, grinding the tire surface to remove the stains on the tire surface; (3) applying glue on the tire surface, wrapping the cord fabric on the tire crown, and pasting the middle cushion glue; the steps of pasting the middle cushion glue are as follows: pasting 2-3 layers of middle cushion glue on the position where the cord fabric is not wrapped, and then pasting 1 layer of middle cushion glue on the tire crown; (4) sending the processed tire into a vulcanizer for vulcanization. In the present invention, by pasting a thicker middle cushion glue on the position where the cord fabric is not wrapped, it is possible to effectively avoid the position where the cord fabric is not wrapped to be easily damaged during the later use process, thereby extending the service life of the tire body and improving the overall quality of the retreaded tire.

[0005] Another example is the "A Tire Retreading Process" disclosed in the application publication number CN 113085239 A. The present invention provides a tire retreading process, which includes the following steps: Step 1: Determine whether the tire meets the retreading standard and clean the qualified tires; Step 2: Grind the tire surface by a grinder, and the surface roughness of the tire after grinding reaches a predetermined range value; Step 3: Inflate the tire body; Step 4: Place the tire in an extruder, and the extruder drives the tread rubber to adhere to the tread at high pressure; Step 5: Roll the tire tread by a rolling device; Step 6: After molding, the tire is transported to a drying room for drying; Step 8: Check and trim the treated tire. By newly judging whether the tire meets the standard for secondary use, the service life of the tire is increased, and the later molding of the tire is further strengthened by drying and vulcanization treatment, and the phenomenon of later cracking is reduced. Finally, the safety of the tire is further improved by checking and trimming.

[0006] The Chinese patent application publication number is CN 104441722 A, and the disclosed invention name is "Method for manufacturing a whole-round pre-cured tread of a giant mining tire by a spiral push method". The present invention relates to a method for manufacturing a whole-round pre-cured tread of a giant mining tire by a spiral push method. The purpose of the present invention is to solve the technical difficulties in the current retreading and remanufacturing of giant mining tires. The technical solution of the present invention is to use a cold feed screw extruder to push the rubber into the mold through the rubber inlet of the mold, and fill the mold with the rubber through continuous spiral thrust, and apply a higher pressure to the rubber through pulses to make the rubber more dense, and the physical and mechanical properties and wear resistance of the tread after vulcanization are improved.

[0007] There is also a Chinese patent announcement CN 107405850 A, the name of the invention disclosed is "Expandable rim for tire tread polishing device and method", the invention discloses a machine for retreading tires, the machine includes: a rotatable hub, the rotatable hub includes a movable conical element; and an expandable rim arranged around the rotatable hub. The expandable rim includes a plurality of shoe plates. Each of the plurality of shoe plates may have a base portion and an edge portion. The base portion may have a two-piece structure, and the two-piece structure allows replacement of worn interfaces that may include channels and ramps. The present invention also discloses a method for assembling an expandable rim for a tire retreading machine, and a method for maintaining a machine with an expandable rim.

[0008] Another example is the invention titled "A Method for Renovating Waste Solid Tires" disclosed in the Chinese patent application publication number CN 116638805 A. The present invention provides a method for renovating waste solid tires, which relates to the technical field of waste solid tire renovation. The method for renovating waste solid tires comprises the following steps: S1. First, the waste solid tires are efficiently cleaned, S2. The cleaned waste tires are then inspected by staff, S5. The waste solid tires that have been cut are bonded to the core, S6. The waste solid tires that have been bonded are glued, S7. The waste solid tires that have been glued are implanted with rubber pattern films, and then air-dried, and S8. The waste solid tires that have been glued are implanted with rubber pattern films. The present invention classifies the waste solid tires, thereby shortening the time for refurbishing waste tires, improving the efficiency of refurbishing waste tires, and at the same time, maximizing the utilization rate of waste tires, reducing the waste of resources and environmental pollution. etc,

[0009] Another example is Chinese patent application No. 202410105992.8, the name of the invention applied for is "Pre-cured composite tread tire retreading method, composite tread and retreaded tire". The present invention belongs to the technical field of pre-cured tread retreading tires, and specifically relates to a pre-cured composite tread tire retreading method, composite tread and retreaded tire. A pre-cured composite tread tire retreading method includes the following steps: S1, washing and inspecting the tire body, S2, grinding the surface of the tire body, S3, repairing the tire body, S4, manufacturing a pre-cured composite tread, S5, bonding the pre-cured composite tread to the tire body to obtain a pre-cured composite tread tire, and S6, testing the pre-cured composite tread tire. Therefore, there is no need for secondary and multiple vulcanization of the retreaded tire, which reduces the investment in personnel and equipment, saves energy, is more green and environmentally friendly, simplifies the tire retreading process, reduces the investment in tire retreading equipment, and realizes tire retreading in a more efficient and energy-saving manner, thereby reducing the retreading cost.

[0010] For example, the Chinese patent announcement number CN 116766655 A discloses the invention title "A novel method for refurbishing giant tires". The present invention provides a novel method for refurbishing giant tires, which relates to the field of tire refurbishment technology. The novel method for refurbishing giant tires comprises the following steps: S1. Preliminary inspection, S2. Milling: exposing the tire body, S3. Tire repair, S4. Tire construction, S5. Tire vulcanization, S6. Final inspection. The tire refurbishment method of the present invention consists of several major steps, including milling, tire repair, construction, and vulcanization. The refurbishment method is simple and fast, which can extend the service life of the tire, reduce the cost during the refurbishment process, and avoid secondary damage to the tire during the tire vulcanization process. At the same time, a preliminary inspection is performed before refurbishing the tire, and it is determined whether the tire can be subsequently refurbished, reducing the risk of the tire body being rejected when entering the refurbishment workshop for preliminary inspection. Etc.

[0011] From the technical solutions disclosed in the above patent applications, it can be seen that there are a large number of methods and devices for refurbishing various old tires, and the main method is to use a one-time vulcanization molding refurbishment process, that is, the old tire embryo to be refurbished is subjected to processes such as gluing and cord fabric, molding, vulcanization, etc., and then a one-time vulcanization and molding process is used to prepare a refurbished tire. After refurbishing with this tire refurbishment process, the tire is very likely to break the belt layer and the steel wire will flow into the tire body, thereby crushing the tire inner tube and making the refurbished tire unusable. Especially for large trucks, mining trucks, and loaders, because their tire diameters are relatively large and they carry heavy loads, they are more likely to have the above-mentioned quality problems when they are refurbished using a one-time vulcanization molding process. At the same time, due to the use of a one-time vulcanization molding refurbishment process, the outer layer of the tire and the bottom embryo layer of the tire are not specially pressed, or only a simple pressing process is performed, and the vulcanization process is directly performed. Or there is no special pressing device for pressing. The adhesion between the tread layer of the old tire and the underlying embryo layer or the pre-cured tread layer and the underlying embryo layer is not very strong. Therefore, for large-diameter retread tires used in large mines and retread tires used in construction machinery, the retreaded surface layer and the underlying embryo layer of the retread tire are easily delaminated during actual use due to insufficient adhesion, causing damage to the retreaded tire and making it unusable.

[0012] From the current status of tire retreading, there is no successful retreading process and product for the retreading of large truck tires, that is, the retreading products of mining trucks with tire diameters above 1400. Generally, large retreaded tires used in mines will have problems such as steel wire breaking the inner tube, tread layer separation from the carcass, retread tread delamination, and tread wear resistance after about 3 months of use, and even tire explosion. Therefore, it is difficult for such retreaded tires to meet the quality standard requirements and cannot meet the actual production needs.

[0013] Therefore, how to provide a method and device for refurbishing the carcass of mining truck tires by vulcanization molding in batches; especially for mining truck tires with larger diameters used for mining trucks, how to refurbish them? The existing one-time vulcanization molding process method is adopted. Although this saves the one-time vulcanization process, it is easy for the belt layer of the refurbished tire to run into the carcass with steel wire, puncturing the inner carcass, causing the refurbished tire to be unusable or the service life not meeting the requirements; at the same time, during the refurbishing process, when the surface pattern layer and the inner carcass, i.e., the base carcass, are bonded, the bonding strength of the glue is not enough, and there is no special pressing device, or the structure of the pressing device is not reasonable, so that the refurbished tire after pressing enters the next process due to the pressing force or without pressing, so that the quality of the refurbished tire is unqualified, etc., so that the service life requirements cannot be met. In order to improve the utilization rate of mining truck tire refurbishment, save production costs, and meet the requirements of environmental protection and circular economy. Summary of the invention:

[0014] The present invention provides a method and device for refurbishing a mining truck tire carcass by stepwise vulcanization molding, which is a process for refurbishing a refurbishable carcass by secondary vulcanization molding, comprising a primary vulcanization mold device, a pressing machine device, and a secondary vulcanizing tank device. By controlling the process technical parameters of the secondary vulcanization treatment of the refurbishable carcass and pressing the secondary vulcanized carcass by a pressing machine device, the refurbished mining truck tire prepared can effectively prevent the occurrence of belt steel wires running into the carcass to cause the inner tube to be punctured, etc., which makes the refurbished mining truck tire unusable in a short period of time, thereby greatly improving the service life of the refurbished mining truck tire. The preparation process and pressing device are simple, and the comprehensive preparation and use cost is low.

[0015] One of the purposes of the present invention is to provide a method for refurbishing a mining truck tire carcass by vulcanization molding in stages, which is a process for refurbishing a mining truck tire carcass by secondary vulcanization molding, and includes the following steps:

[0016] 1) Select the tire bodies that can be used for retreading from the used tires of mining trucks, which are the retread tire bodies.

[0017] 2) The refurbishable carcass in step 1) is cleaned and cooled and dried, and the drying temperature is controlled at 40-50° C. and the drying time is controlled at 40-65 minutes to obtain a clean refurbishable carcass.

[0018] 3) The original belt layer on the clean retreadable carcass in step 2) is completely peeled off to the tire body steel wire layer, which is to peel off the retreadable carcass. 4) The outer wall surface of the peeled retreadable carcass in step 3) is polished, and the outer wall surface of the tire is cleaned until it is free of dust and impurities, and it is checked that there is no broken steel wire on the outer wall surface of the peeled retreadable carcass, which is to polish the retreadable carcass.

[0019] 5) Apply glue. After the surface of the carcass that can be refurbished is cleaned by grinding in step 4, apply a layer of glue and dry it for 30-50 minutes. The drying temperature is controlled to be 65-80°C. This is to apply glue to the carcass that can be refurbished.

[0020] 6) Pasting the middle cushion rubber layer, pasting the middle cushion rubber layer on the outer wall surface of the surface layer of the side of the tire body that contacts the ground by brushing the glue in step 5), so that the tire body can be refurbished by pasting the middle cushion rubber layer,

[0021] 7) Attaching a belt layer: attaching a new belt layer on the wall surface of the middle cushion layer of the refurbished carcass in step 6), controlling the width of the belt layer to correspond to the width of the refurbished carcass with the middle cushion layer, and attaching a new belt layer on the wall surface of the middle cushion layer of the refurbished carcass.

[0022] 8) applying buffer glue, applying buffer glue on the outer wall of the tire body that can be refurbished by applying the belt layer in step 7), wherein the tire body can be refurbished by applying buffer glue, and the buffer glue is an uncured raw rubber sheet;

[0023] 9) First molding, inflation and vulcanization: the cushioning rubber refurbishable carcass prepared in step 8) is placed in the inner cavity of the first lower vulcanization cavity 201 of the first vulcanization mold device, and the corresponding inner tube is placed in the inner cavity of the cushioning rubber refurbishable carcass, and the inner tube is inflated. After the inflation is completed, the first molding, inflation and vulcanization treatment is performed to obtain a first vulcanized carcass.

[0024] 10) preparing a polished primary vulcanized smooth tire body, removing the primary vulcanized tire body from the primary vulcanization mold device in step 9), checking whether the primary vulcanized tire body is qualified, performing secondary polishing and secondary cushion rubber layer treatment on the wall surface of the qualified primary vulcanized tire body, and drying to obtain a primary polished vulcanized smooth tire body,

[0025] 11), a retreadable tire body is made by laminating a pre-cured tread layer or an old tire tread on the outer surface of the polished and vulcanized tire body 101, and then the pre-cured tread layer is affixed to the outer surface of the tire body 101, and then the tire body 101 is sent to a laminating machine for laminating.

[0026] 12) performing a second vulcanization treatment in a vulcanization tank device, packaging and packaging the retreaded tire pressed in step 11) and placing it in the inner cavity of a secondary vulcanization tank device, closing the cover of the secondary vulcanization tank device, performing a second vulcanization treatment, and manufacturing a secondary vulcanized retreaded tire product;

[0027] 13) Testing and trial use: testing the secondary vulcanized retreaded tire product prepared in step 12) to see if the vulcanization is in place and whether the retreaded tire body is bulging. If the trial is qualified, the retreaded tire product is obtained.

[0028] Furthermore, the retreadable tire body in step 1) refers to a tire body for retreading whose tire body, sidewalls and tire wire layer are not disconnected and is a used tire that has been used recently.

[0029] Furthermore, in step 7), a belt layer is applied, and a new belt layer containing steel wire material is applied on the surface of the refurbishable carcass with the middle rubber layer, and the number of belt layers applied on the outer surface of the refurbishable carcass with the middle rubber layer is controlled to be 4-5 layers.

[0030] Preferably, in step 9), the first molding and inflation vulcanization are performed under the following conditions: the first vulcanization time is controlled to be 210-300 minutes, and the first vulcanization temperature is controlled to be 142-155°C.

[0031] The method for refurbishing a mining truck tire carcass by multiple vulcanization molding comprises the following steps: step 12) performing a second vulcanization treatment in a vulcanizing tank device, controlling the second vulcanization treatment time to be 400-600 minutes, and the second vulcanization treatment temperature to be 110-125°C.

[0032] The method for refurbishing a mining truck tire carcass by partial vulcanization molding is as follows: the shape of the belt layer attached to the surface of the refurbishable carcass with the middle cushion rubber layer is controlled to be an oblique quadrilateral structure, the length of the belt layer is controlled to be equal to the circumference length of the outer wall surface of the refurbishable carcass with the middle cushion rubber layer, and each layer of the belt layer is controlled to be sequentially and correspondingly coated on the outer wall surface of the circumference of the refurbishable carcass with the middle cushion rubber layer.

[0033] The method for refurbishing a mining truck tire carcass by multiple vulcanization molding is preferably such that the belt layer directly coated on the outer surface of the refurbishable carcass attached to the center cushion rubber layer is controlled to be the first belt layer, and the corresponding belt layer attached to the surface of the first belt layer is the second belt layer, and the others are similarly controlled to control the included angle B1 of the two sides of the oblique quadrilateral of the first belt layer to be 24.5-25.5 degrees, and the included angles of the two sides of the second belt layer and the remaining belt layers are all B2=13.5-14.5 degrees; and the width of the second belt layer coated on the surface of the refurbishable carcass attached to the center cushion rubber layer is controlled to be larger than the width of other belt layers coated on the surface of the refurbishable carcass attached to the center cushion rubber layer.

[0034] Preferably, purified carbon nanomaterials can be added to the adhesive during the application of the adhesive in the present invention to improve the performance of the adhesive layer, mainly to improve its adhesion.

[0035] Another object of the present invention is to provide a device for realizing the above-mentioned method for refurbishing the tire carcass of a mining truck by step-by-step vulcanization molding, comprising a primary vulcanization mold device, a pressing machine device, and a secondary vulcanization tank device. The primary vulcanization mold device comprises a primary lower vulcanization cavity, a positioning boss arranged at the center of the inner cavity of the primary lower vulcanization cavity, a guide rail bracket, a fixed cross bar, a primary upper vulcanization cavity, an upper positioning platen, a first hydraulic cylinder, an air extraction hose, a primary vulcanization electric control box, and a lower positioning base plate seat. The primary lower vulcanization cavity is arranged on the lower positioning base plate seat, and one end of the guide rail bracket is fixedly connected to the lower positioning base plate seat. The other end of the bottom plate seat is fixedly connected to the upper positioning platen, the primary upper vulcanization chamber is correspondingly arranged above the primary lower vulcanization chamber and is connected to the guide rail bracket through a fixed cross bar, the first hydraulic cylinder is arranged above the upper positioning platen, and is correspondingly connected to the primary upper vulcanization chamber and the primary lower vulcanization chamber through corresponding pipelines; the secondary vulcanization tank device includes a vulcanization tank body, an inner cavity of a vulcanization tank, a tank cover, a vulcanization tank bracket, a vulcanization control instrument, a vulcanization tank control box and an exhaust pipe arranged on the vulcanization tank body, and the pressed refurbishable tire body can be placed in the hollow inner cavity of the inner cavity of the vulcanization tank for secondary vulcanization treatment;

[0036] Specifically, the laminating machine device comprises a laminating and clamping mechanism and a tire laminating and stabilizing mechanism;

[0037] The pressing and clamping mechanism comprises a pressing base, a pressing column, an upper rolling part, a movable rolling part and a carcass positioning part; one end of the pressing column is fixedly connected to the corresponding position of the pressing base, and the upper rolling part is arranged on the top of the other end;

[0038] The upper rolling part includes a rolling motor and an upper rolling wheel, and the upper rolling wheel is movably connected to the output rotating shaft of the rolling motor through a rotating shaft;

[0039] The movable rolling part includes a vertical groove, a swing clamping rod, a lower rolling wheel, a vertical hydraulic oil cylinder, and a hinged ear plate, which are arranged at a corresponding position in the middle of the pressing column. The corresponding position in the middle of the swing clamping rod is movably arranged in the vertical groove through a hinged component, and a lower rolling wheel is arranged at one end thereof, and the lower rolling wheel corresponds to the upper rolling wheel. The other end of the swing clamping rod is movably connected to one end of the hinged ear plate, and the other end of the hinged ear plate is movably connected to one end of the vertical hydraulic oil cylinder, and the other end of the vertical hydraulic oil cylinder is connected to the corresponding position of the pressing base.

[0040] The carcass positioning part is arranged below the movable rolling part, located at the corresponding position between the vertical groove on the pressing column and the pressing base, and includes a lifting positioning motor and a positioning supporting wheel. The positioning supporting wheel is connected to the output shaft of the lifting positioning motor and corresponds to the lower rolling wheel and the upper rolling wheel vertically up and down along the longitudinal direction.

[0041] The device described in the present invention, wherein the tire pressing stabilization mechanism includes a tire pressing movable frame, a longitudinal adjustment module, a transverse adjustment module, a mounting frame column and a tire pressing installation assembly, wherein the longitudinal adjustment module and the transverse adjustment module are arranged at corresponding positions on the tire pressing movable frame, one end of the mounting frame column is fixedly connected to the tire pressing movable frame, and the other end is provided with a tire pressing installation assembly; the tire pressing installation assembly is used to adjust the corresponding position of the once-polished and vulcanized smooth tire body on the pressing machine device, so that the upper rolling wheel and the lower rolling wheel on the pressing machine device perform pressing and compacting processing on the once-polished and vulcanized smooth tire body and the pre-vulcanized tread layer attached to the outer surface wall surface of the circumference thereof along the circumference direction of the once-polished and vulcanized smooth tire body.

[0042] The device described in the present invention, wherein the tire pressing installation assembly is provided with a clamping tire body unit, and the clamping tire body unit includes a clamping slide rail, two clamping sliders, two clamping roller rods, two clamping rollers, and a bidirectional cylinder. The two clamping sliders are respectively arranged at corresponding positions on the clamping slide rail, one end of the two clamping roller rods is respectively connected to corresponding positions of the two clamping sliders, and the other end is respectively provided with a clamping roller, and the two ends of the bidirectional cylinder are respectively connected to corresponding positions in the middle of the two clamping roller rods, and the two clamping rollers can clamp the once-polished and vulcanized smooth tire body that undergoes pressing and tightening treatment.

[0043] The present invention discloses a method and device for refurbishing mining truck tires by vulcanization molding in batches. The above-mentioned process method and device have the following beneficial effects: First, the present invention is aimed at the tires for mining trucks, that is, refurbished tires for trucks, which have the characteristics of large diameter and volume. Generally, the tires for single large trucks are expensive, and usually when refurbishing old tires. The carcass is generally subjected to a one-time vulcanization molding process. Although this can reduce its production cost, the service life of the refurbished tire prepared therefrom is short, mainly because the belt layer steel wire runs into the carcass. This causes the refurbished mining truck tire to be unusable in a short period of time. The present invention adopts a process method for secondary vulcanization of the refurbished carcass, and the first vulcanization method is to vulcanize the belt layer or protective layer of the carcass onto the stripped refurbishable carcass, and the second vulcanization can vulcanize the pre-vulcanized tread layer or the old tread of the tire onto the once polished and vulcanized smooth carcass 101, that is, the entire pressed refurbishable tire 102 is subjected to a second vulcanization treatment. In this way, the belt layer, the middle cushion rubber layer and the pre-cured tread layer or the old tread of the tire are integrated with the retreaded tire body, thereby greatly improving the strength, tear resistance and other properties of the retreaded tire products and improving the product quality of the retreaded tires.

[0044] Second, the present invention greatly enhances the durability and strength of the retreaded tire of a heavy truck by attaching multiple layers of belt steel wires or belt layers of steel wire material structure on the surface of the retreaded tire body with the middle cushion layer, and controls the belt angle and belt width of each layer, thereby enhancing the stability and wear resistance of the retreaded tire, that is, the tear strength reaches more than 89 (kN·m-1), and the hardness reaches more than 70 Shore A hardness / degree, while the prior art is only about 70 and 55, and the specific data are shown in the following Table 1. Etc.

[0045] On the other hand, the purified carbon nanotube raw material can be added to the rubber slurry of the present invention, which can enhance the bonding strength between the tire body and the middle cushion rubber layer, and between the crown layer, the shoulder layer and the belt layer, thereby improving the connection performance of the joint of the retreaded tire, thus greatly extending the service life of the retreaded tire.

[0046] Third, the present invention adopts the above-mentioned process method for secondary vulcanization molding of the retread tire carcass. When the pressing device of the present invention is used to attach the pre-vulcanized tread layer to the secondary cushion rubber layer on the surface of the retreaded carcass, the pressing machine device performs a pressing treatment and then performs a secondary vulcanization treatment, thereby greatly preventing the steel cord fabric, that is, the steel wire in the belt layer steel wire, from running into the carcass, thereby puncturing the inner tube in the inner cavity of the retreaded carcass, causing the retreaded tire to be unusable. This is mainly because when the carcass is vulcanized in a mold with a hinge, the belt layer steel wire in the original carcass becomes loose due to the extrusion of the mold, and the molding is irregular, which causes the belt layer steel wire to puncture the inner tube during actual use, causing the retreaded tire to be unusable. The retreaded tire prepared using the process method and device of the present invention greatly increases the service life of the retreaded tire.

[0047] The determination methods of the performance parameters of the present invention may refer to the methods commonly used in the art, such as GB / T 7037-207, GB / T 528-2008, GB / T 3512-2014, truck GB / T 5327, and the like. Description of the drawings:

[0048] Figure 1 , is a schematic structural diagram of a primary vulcanization mold device according to an embodiment of the present invention;

[0049] Figure 2 , which is a schematic diagram of placing a primary vulcanization tire body 1 into a primary vulcanization mold device according to an embodiment of the present invention;

[0050] Figure 3 , is a structural schematic diagram of the pressing and clamping mechanism of the pressing machine device 3 of the present invention;

[0051] Figure 4 ,for Figure 3 Right view,

[0052] Figure 5 , for the present invention Figure 3 Schematic diagram of the upper rolling wheel 307 and the lower rolling wheel 305 being pressed together to grind and vulcanize the smooth tire body 101;

[0053] Figure 6 ,for Figure 5 Right view;

[0054] Figure 7 ,for Figure 3 Including a structural schematic diagram of a tire pressing stabilization mechanism;

[0055] Figure 8 ,for Figure 7 A schematic diagram of pressing a polished and vulcanized smooth tire body 101;

[0056] Fig. 9 2 is a schematic diagram of the structure of the tire pressing and mounting assembly of the device of the present invention for clamping a polished and vulcanized smooth tire body 101. The tire pressing and stabilizing mechanism transports the polished and vulcanized smooth tire body 101 to the upper rolling wheel 307 and the lower rolling wheel 305 on the pressing and clamping mechanism. During the pressing and clamping work, the two clamping rollers 508 help the polished and vulcanized smooth tire body 101 to keep stable rotation during rolling and pressing.

[0057] Fig.10 , is a schematic structural diagram of the secondary vulcanization tank device 4 of the present invention.

[0058] Fig.11 , is a partial cross-sectional schematic diagram of a belt-covered retreaded carcass 7 formed by attaching 4-5 layers of new belt layers to the surface of a cushion rubber-covered retreaded carcass 6 according to an embodiment of the present invention;

[0059] Fig.12 ,for Fig.11 A magnified schematic diagram of the middle A part; a cross-sectional schematic diagram showing the 5-layer belt layer;

[0060] Fig.13 , a schematic structural diagram of the first belt layer 801 having an oblique quadrilateral structure, wherein the angle between the two oblique sides is B1; that is, the angle B1 between any long side and any short side;

[0061] Fig.14 , is a schematic diagram of the structure of the angle B2 between the two oblique sides of the second belt layer 802 of the oblique quadrilateral structure; the angles between the two oblique sides of the third belt layer 803, the fourth belt layer 804 to the fifth belt layer 805 are all the same as the angle B2 of the second belt layer 802. The angle between the two oblique sides refers to the minimum angle B2 between a long side and a short side of the oblique quadrilateral.

[0062] In the figure, 1, a primary vulcanized tire body, 101, a primary polished and vulcanized smooth tire body, 102, a pressed retreaded tire, 2, a primary vulcanized mold device, 201, a primary lower vulcanization cavity, 202, a positioning boss, 203, a guide rail bracket, 204, a fixed cross bar, 205, a primary upper vulcanization cavity, 206, an upper positioning platen, 207, a first hydraulic cylinder, 208, an exhaust hose, 209, a primary vulcanized electric control box, 2010, a lower positioning base plate seat, 3, a pressing machine device, 301, a pressing base, 302, a pressing column, 303, a vertical groove, 304, a swing clamp rod, 305, a lower rolling wheel, 306, a pressing motor, 307, an upper rolling wheel, 308, a lifting and positioning motor, 309, a positioning support wheel, 3010, a vertical hydraulic cylinder, 3011, a hinged ear plate, 3012, pressing electric control box, 4, secondary vulcanizing tank device, 401, vulcanizing tank body, 402, vulcanizing tank inner cavity, 403, tank cover, 404, vulcanizing tank bracket, 4045 vulcanization control instrument, 406, vulcanizing tank control box, 407, exhaust pipe, 5, tire pressing mobile frame, 501, longitudinal adjustment module, 502, lateral adjustment module, 503, installation frame column, 504, tire pressing installation assembly, 505, clamping slide rail, 506, clamping slider, 507, clamping roller rod, 508, clamping roller, 509, two-way cylinder, 6, the tire body can be refurbished by sticking the middle cushion rubber layer, 7, the tire body can be refurbished by sticking the belt layer, 801, the first belt layer, 802, the second belt layer, 803, the third belt layer, 804, the fourth belt layer, 805, the fifth belt layer. Specific implementation method:

[0063] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. The present invention is not limited to the embodiments.

[0064] The present invention discloses a method for refurbishing a mining truck tire carcass by multiple vulcanization molding, which is a process method for refurbishing a mining truck tire carcass by secondary vulcanization molding, and includes the following steps:

[0065] 1) Selecting tire bodies that can be used for retreading from used tires of mining trucks, which are retreadable tire bodies. The retreadable tire bodies refer to tire bodies whose tire bodies, sidewalls and tire wire layers are not disconnected and are used tires that have been used recently;

[0066] 2) The refurbishable carcass in step 1) is cleaned and cooled and dried, and the drying temperature is controlled at 40-50° C. and the drying time is controlled at 40-65 minutes to obtain a clean refurbishable carcass.

[0067] 3) The original belt layer on the clean retreadable carcass in step 2) is completely peeled off to the tire body steel wire layer, which is to peel off the retreadable carcass. 4) The outer wall surface of the peeled retreadable carcass in step 3) is polished, and the outer wall surface of the tire is cleaned until it is free of dust and impurities, and it is checked that there is no broken steel wire on the outer wall surface of the peeled retreadable carcass, which is to polish the retreadable carcass.

[0068] 5) Apply glue. After the surface of the carcass that can be refurbished is cleaned by grinding in step 4, apply a layer of glue and dry it for 30-50 minutes. The drying temperature is controlled to be 65-80°C. This is to apply glue to the carcass that can be refurbished.

[0069] 6) Pasting the middle cushion rubber layer, pasting the middle cushion rubber layer on the outer wall surface of the surface layer of the side of the tire body that contacts the ground by brushing the glue slurry in step 5,

[0070] 7) Attaching a belt layer: attaching a new belt layer on the wall surface of the middle cushion layer of the refurbishable carcass 6 of step 6), controlling the width of the belt layer to correspond to the width of the refurbishable carcass 6 of the middle cushion layer, and attaching a new belt layer on the wall surface of the middle cushion layer of the refurbishable carcass 6 of step 6,

[0071] 8) Pasting buffer glue, pasting buffer glue on the outer wall surface of the belt layer refurbishable carcass 7 in step 7), wherein the buffer glue is an unvulcanized raw rubber sheet;

[0072] 9) First molding, inflation and vulcanization: the cushioning rubber refurbishable tire body prepared in step 8) is placed in the first lower vulcanization cavity 201 of the first vulcanization mold device 2, and the corresponding inner tube is placed in the inner cavity of the cushioning rubber refurbishable tire body, and the inner tube is inflated. After the inflation is completed, the first molding, inflation and vulcanization treatment is performed to obtain a first vulcanized tire body 1.

[0073] 10) preparing a polished primary vulcanized smooth tire body, moving the primary vulcanized tire body 1 of step 9) out of the corresponding primary lower vulcanization cavity 201 of the primary vulcanization mold device 2, checking whether the primary vulcanized tire body 1 is qualified, performing secondary polishing and secondary cushioning rubber layer treatment on the wall surface of the qualified primary vulcanized tire body 1, and drying to obtain a primary polished vulcanized smooth tire body 101,

[0074] 11), a retreadable tire body is made by laminating and bonding a pre-cured tread layer on the outer surface of the polished and vulcanized smooth tire body 101, and then the pre-cured tread layer is sent to the laminating machine device 3 for laminating treatment, so as to laminarly bond a retreadable tire 102.

[0075] 12) performing a second vulcanization treatment in a vulcanization tank device, packaging and packaging the retreaded tire 102 pressed in step 11) and placing it in the inner cavity of a secondary vulcanization tank device 4, closing the tank cover 402 of the secondary vulcanization tank device, performing a second vulcanization treatment, and manufacturing a secondary vulcanized retreaded tire product;

[0076] 13) Testing and trial use: testing the secondary vulcanized retreaded tire product prepared in step 12) to see if the vulcanization is in place and whether the retreaded tire body is bulging. If the trial is qualified, the retreaded tire product is obtained.

[0077] Preferably, in the method for refurbishing a mining truck tire carcass by multiple vulcanization molding, step 7) affixing a belt layer, affixing a brand new belt layer containing steel wire material on the surface of the refurbishable carcass 6 with the middle cushion rubber layer, and controlling the number of belt layers affixed on the outer surface of the refurbishable carcass 6 with the middle cushion rubber layer to be 4-5 layers.

[0078] Furthermore, in step 9), the first molding and inflation vulcanization are performed, and the first molding and inflation vulcanization conditions are controlled to control the first vulcanization time to be 210-300 minutes and the first vulcanization temperature to be 142-155°C.

[0079] Step 12) performing a second vulcanization treatment in a vulcanization tank, wherein the second vulcanization treatment time is controlled to be 400-600 minutes, and the second vulcanization treatment temperature is controlled to be 110-125°C.

[0080] Furthermore, the method for refurbishing a mining truck tire carcass by multiple vulcanization molding is to control the shape of the belt layer attached to the surface of the refurbishable carcass 6 with the middle cushion rubber layer to be an oblique quadrilateral structure, or a diamond structure, to control the length of the belt layer to be equivalent to the circumference length of the outer wall surface of the refurbishable carcass 6 with the middle cushion rubber layer, and to control each layer of the belt layer to be able to be sequentially and correspondingly coated on the outer surface wall surface of the circumference of the refurbishable carcass 6 with the middle cushion rubber layer.

[0081] Preferably, the belt layer directly coated on the outer surface wall of the refurbishable carcass 6 with the center cushion rubber layer is controlled to be the first belt layer 801, and the corresponding belt layer attached to the surface wall of the first belt layer 801 is the second belt layer 802, and the others are similarly controlled, and the angle B1 between the two sides of the oblique quadrilateral of the first belt layer 801 is controlled to be 24.5-25.5 degrees, and the angles between the two sides of the second belt layer 802 and the remaining belt layers are all B2=13.5-14.5 degrees; and the width of the second belt layer 802 coated on the surface of the refurbishable carcass 6 with the center cushion rubber layer is controlled to be larger than the width of other belt layers coated on the surface of the refurbishable carcass 6 with the center cushion rubber layer.

[0082] In order to increase the roughness of the tire grinding surface to enhance its bonding force, the present invention preferably controls the roughness of the tire tread after grinding to about RA 6.4-6.7.

[0083] like Figure 1-10As shown, another object of the present invention is to provide a device for realizing the above-mentioned method for refurbishing a mining truck tire by step vulcanization molding, comprising a primary vulcanization mold device 2, a pressing machine device 3, and a secondary vulcanization tank device 4. The primary vulcanization mold device 2 comprises a primary lower vulcanization cavity 201, a positioning boss 202 arranged at the center of the inner cavity of the primary lower vulcanization cavity 201, a guide rail bracket 203, a fixed cross bar 204, a primary upper vulcanization cavity 205, an upper positioning plate 206, a first hydraulic cylinder 207, an exhaust hose 208, a primary vulcanization electric control box 209 and a lower positioning base plate seat 210. The primary lower vulcanization cavity 201 is arranged on the lower positioning base plate seat 210, and one end of the guide rail bracket 203 is fixedly connected to the lower positioning base plate seat 210. The other end is fixedly connected to the upper positioning platen 206, the primary upper vulcanization chamber 205 is correspondingly arranged above the primary lower vulcanization chamber 201 and is connected to the guide rail bracket 203 through the fixed cross bar 204, the first hydraulic cylinder 207 is arranged above the upper positioning platen 206, and is correspondingly connected to the primary upper vulcanization chamber 205 and the primary lower vulcanization chamber 201 through corresponding pipelines; the secondary vulcanization tank device 4 includes a vulcanization tank body 401, a vulcanization tank inner cavity 402, a tank cover 403, a vulcanization tank bracket 404, a vulcanization control instrument 405, a vulcanization tank control box 406 and an exhaust pipe 407 arranged on the vulcanization tank body 401, and the pressed retread tire 102 can be placed in the hollow inner cavity of the vulcanization tank inner cavity 402 for secondary vulcanization treatment;

[0084] The laminating machine device 3 includes a laminating and clamping mechanism and a tire laminating and stabilizing mechanism;

[0085] The pressing and clamping mechanism includes a pressing base 301, a pressing column 302, an upper rolling part, a movable rolling part and a carcass positioning part; one end of the pressing column 302 is fixedly connected to the corresponding position of the pressing base 301, and the upper rolling part is arranged on the top of the other end;

[0086] The upper rolling part includes a rolling motor 306 and an upper rolling wheel 307. The upper rolling wheel 307 is movably connected to the output rotating shaft of the rolling motor 306 through a rotating shaft.

[0087] The movable rolling part includes a vertical slot 303, a swing clamping rod 304, a lower rolling wheel 305, a vertical hydraulic cylinder 3010, and a hinged ear plate 3011, which are arranged at a corresponding position in the middle of the pressing column 302. The corresponding position in the middle of the swing clamping rod 304 is movably arranged in the vertical slot 303 through a hinged component, and a lower rolling wheel 305 is arranged at one end of the swing clamping rod, and the lower rolling wheel 305 corresponds to the upper rolling wheel 307. The other end of the swing clamping rod 304 is movably connected to one end of the hinged ear plate 3011, and the other end of the hinged ear plate 3011 is movably connected to one end of the vertical hydraulic cylinder 3010, and the other end of the vertical hydraulic cylinder 3010 is connected to the corresponding position of the pressing base 301.

[0088] The carcass positioning portion is arranged below the movable rolling portion, located above the pressing base 301 and at a corresponding position between the vertical groove 303 on the pressing column 302, and includes a lifting and positioning motor 308 and a positioning support wheel 309. The positioning support wheel 309 is connected to the output shaft of the lifting and positioning motor 308 and corresponds to the lower rolling wheel 305 and the upper rolling wheel 307 vertically in the longitudinal direction up and down.

[0089] The device, wherein the tire pressing stabilization mechanism includes a tire pressing movable frame 5, a longitudinal adjustment module 501, a transverse adjustment module 502, a mounting column 503 and a tire pressing installation assembly 504, wherein the longitudinal adjustment module 501 and the transverse adjustment module 502 are arranged at corresponding positions on the tire pressing movable frame 5, one end of the mounting column 503 is fixedly connected to the tire pressing movable frame 5, and the other end is provided with a tire pressing installation assembly 504; the tire pressing installation assembly 504 is used to adjust the corresponding position of the once-polished and vulcanized smooth tire body 101 on the pressing machine device 3, so that the upper rolling wheel 307 and the lower rolling wheel 305 on the pressing machine device 3 perform pressing and compacting processing on the once-polished and vulcanized smooth tire body 101 and the pre-vulcanized tread layer attached to the outer peripheral wall surface thereof along the circumferential direction of the once-polished and vulcanized smooth tire body 101.

[0090] The device, wherein the tire pressing installation assembly 504 is provided with a clamping tire body unit, and the clamping tire body unit includes a clamping slide rail 505, two clamping sliders 506, two clamping roller rods 507, two clamping rollers 508, and a bidirectional cylinder 509. The two clamping sliders 506 are respectively arranged at corresponding positions on the clamping slide rail 505, one end of the two clamping roller rods 507 is respectively connected to the corresponding positions of the two clamping sliders 506, and the other end is respectively provided with a clamping roller 508, and the two ends of the bidirectional cylinder 509 are respectively connected to the corresponding positions in the middle of the two clamping roller rods 507, and the two clamping rollers 508 can clamp the once-polished and vulcanized smooth tire body 101 that undergoes pressing and compacting treatment.

[0091] All matters not described in the following embodiments are implemented according to the above specific implementation methods.

[0092] Embodiment 1,

[0093] The retreaded mining truck tires prepared in this embodiment are described by taking mining truck tires with product specifications of 14.00R25 or 14.00R24 as an example.

[0094] The present invention discloses a method for refurbishing a mining truck tire carcass by multiple vulcanization molding, which is a process method for refurbishing a mining truck tire carcass by secondary vulcanization molding, and includes the following method steps:

[0095] 1) Selecting tire bodies that can be used for retreading from used tires of mining trucks, which are retreadable tire bodies. The retreadable tire bodies refer to tire bodies whose tire bodies, sidewalls and tire wire layers are not disconnected and are used tires that have been used recently;

[0096] 2) The refurbishable carcass in step 1) is cleaned and cooled and dried, and the drying temperature is controlled at 40-50° C. and the drying time is controlled at 40-65 minutes to obtain a clean refurbishable carcass.

[0097] 3) The original belt layer on the clean retreadable carcass in step 2) is completely peeled off to the tire body steel wire layer, in order to peel off the retreadable carcass,

[0098] 4) Grinding the outer wall of the tire body stripped for retreading in step 3), cleaning the outer wall of the tire until it is clean and free of dust and impurities, and checking that there is no broken steel wire on the outer wall of the tire body stripped for retreading, in order to grind the tire body for retreading,

[0099] 5) Apply glue. After the surface of the carcass that can be refurbished is cleaned by grinding in step 4, apply a layer of glue and dry it for 30-50 minutes. The drying temperature is controlled to be 65-80°C. This is to apply glue to the carcass that can be refurbished.

[0100] 6) Pasting the middle cushion rubber layer, in step 5), the middle cushion rubber layer is pasted on the outer wall surface of the circumference of the surface layer of the side of the tire body that contacts the ground by brushing the glue mortar, and the tire body 6 is pasted with the middle cushion rubber layer, FIG. Fig.11 As shown;

[0101] 7) Attaching a belt layer, attaching a brand new belt layer on the wall surface of the middle cushion layer of the refurbishable carcass 6 of the step 6), wherein the brand new belt layer is made of steel wire material, and the width of the belt layer is controlled to correspond to the width of the middle cushion layer refurbishable carcass 6, and the belt layer refurbishable carcass 7 is attached, preferably, a brand new belt layer containing steel wire material is attached on the surface of the middle cushion layer refurbishable carcass 6, and the number of belt layers attached on the outer surface of the middle cushion layer refurbishable carcass 6 is controlled to be 5; Fig.12 As shown;

[0102] Preferably, the shape of the belt layer attached to the surface of the refurbishable carcass 6 with the middle cushion rubber layer is controlled to be an oblique quadrilateral structure, the length of the belt layer is controlled to be equivalent to the circumference length of the outer wall surface of the refurbishable carcass 6 with the middle cushion rubber layer, and each layer of the belt layer is controlled to be able to be coated on the outer wall surface of the circumference of the refurbishable carcass 6 with the middle cushion rubber layer in sequence.

[0103] like Figure 12-14As shown, the belt layer directly coated on the outer surface wall of the tire body 6 that can be retreaded with the middle cushion rubber layer is the first belt layer 801, and the corresponding belt layer 802 is attached to the surface wall of the first belt layer 801, and the others are similar, that is, the third belt layer 803 is attached to the outer surface of the second belt layer 802, and the fourth belt layer 804 is attached to the outer surface of the third belt layer 803, and the fifth belt layer 805 is attached to the outer surface of the second belt layer 804; Fig.12 As shown, the angle B1 between the two sides of the oblique quadrilateral of the first belt layer 801 is controlled to be 25.0 degrees. Fig.13 As shown, the angles on both sides of the second belt layer 802 and the remaining belt layers, namely the third belt layer 803, the fourth belt layer 804, and the fifth belt layer 805 are all B2 = 14 degrees; and the width of the second belt layer 802 wrapped on the surface of the tire body 6 that can be retreaded with the middle cushion rubber layer is controlled to be greater than the width of the other belt layers wrapped on the surface of the tire body 6 that can be retreaded with the middle cushion rubber layer. That is, the width of the second belt layer 802 is greater than the width of the first belt layer 801, the third belt layer 803, the fourth belt layer 804, and the fifth belt layer 805; the width referred to here refers to the width of the belt layer wrapped on the tire body of the retreaded tire. Fig.11 Width dimensions shown, i.e. Fig.13 , 14 The perpendicular distance between the short sides of the two oblique quadrilaterals;

[0104] 8) applying buffer glue, in step 7), applying buffer glue on the outer wall of the tire body 7 that can be refurbished with the belt layer, and applying buffer glue can refurbish the tire body, wherein the buffer glue is an unvulcanized raw rubber sheet;

[0105] 9) First molding, inflation and vulcanization, the cushioning rubber refurbishable tire body prepared in step 8) is placed in the first lower vulcanization cavity 201 of the first vulcanization mold device 2, and the corresponding inner tube is placed in the inner cavity of the cushioning rubber refurbishable tire body, and the inner tube is inflated. After the inflation is completed, the first molding, inflation and vulcanization treatment is performed to obtain a first vulcanized tire body 1. The first molding, inflation and vulcanization conditions are controlled to control the first vulcanization time to 210-300 minutes and the first vulcanization temperature to 145° C.;

[0106] 10) preparing a polished primary vulcanized smooth tire body, moving the primary vulcanized tire body 1 of step 9) out of the corresponding primary lower vulcanization cavity 201 of the primary vulcanization mold device 2, checking whether the primary vulcanized tire body 1 is qualified, performing secondary polishing and secondary cushioning rubber layer treatment on the wall surface of the qualified primary vulcanized tire body 1, and drying to obtain a primary polished vulcanized smooth tire body 101,

[0107] 11), a retread tire body is made by laminating and bonding a pre-cured tread layer on the outer surface of the polished and vulcanized smooth tire body 101, and then a patterned rubber layer, i.e., a ground contact layer of the retreaded tire, is formed and sent to a laminating machine device 3 for laminating treatment, so as to laminarly bond a retreaded tire 102.

[0108] 12) Second vulcanization treatment in a vulcanization tank device, the retreaded tire 102 pressed in step 11) is packaged and placed in the inner cavity of the secondary vulcanization tank device 4, the tank cover 402 of the secondary vulcanization tank device is closed, and the second vulcanization treatment is performed, the second vulcanization treatment time is controlled to be 500 minutes, and the second vulcanization treatment temperature is controlled to be 110-125° C. to prepare a secondary vulcanized retreaded tire product;

[0109] 13) Testing and trial use: testing the secondary vulcanized retreaded tire product prepared in step 12) to see if the vulcanization is in place and whether the retreaded tire body is bulging. If the trial is qualified, the retreaded tire product is obtained.

[0110] In order to increase the roughness of the tire grinding surface to enhance its bonding force, in Example 1 of the present invention, the roughness of the tire tread after grinding is controlled to be about RA 6.7.

[0111] Another object of the present invention is to implement the above-mentioned method for refurbishing the tire carcass of a mining truck by vulcanization molding in stages. Figure 1-3 , including a primary vulcanization mold device 2, a pressing machine device 3, and a secondary vulcanization tank device 4. The primary vulcanization mold device 2 includes a primary lower vulcanization chamber 201, a positioning boss 202 arranged at the center of the inner cavity of the primary lower vulcanization chamber 201, a guide rail bracket 203, a fixed cross bar 204, a primary upper vulcanization chamber 205, an upper positioning platen 206, a first hydraulic cylinder 207, an exhaust hose 208, a primary vulcanization electric control box 209 and a lower positioning base plate seat 210. The primary lower vulcanization chamber 201 is arranged on the lower positioning base plate seat 210, one end of the guide rail bracket 203 is fixedly connected to the lower positioning base plate seat 210, and the other end is fixedly connected to the upper positioning platen 206. The secondary upper vulcanization chamber 205 is correspondingly arranged above the primary lower vulcanization chamber 201 and connected to the guide rail bracket 203 through the fixed cross bar 204. The first hydraulic cylinder 207 is arranged above the upper positioning platen 206 and is correspondingly connected to the primary upper vulcanization chamber 205 and the primary lower vulcanization chamber 201 through corresponding pipelines; the secondary vulcanization tank device 4 includes a vulcanization tank body 401, a vulcanization tank inner cavity 402, a tank cover 403, a vulcanization tank bracket 404, a vulcanization control instrument 405, a vulcanization tank control box 406 and an exhaust pipe 407 arranged on the vulcanization tank body 401, and the pressed retread tire 102 can be placed in the hollow inner cavity of the vulcanization tank inner cavity 402 for secondary vulcanization treatment;

[0112] Specifically, the laminating machine device 3 includes a laminating and clamping mechanism and a tire laminating and stabilizing mechanism;

[0113] like Figure 3 , 4As shown, the pressing and clamping mechanism includes a pressing base 301, a pressing column 302, an upper rolling part, a movable rolling part and a carcass positioning part; one end of the pressing column 302 is fixedly connected to the corresponding position of the pressing base 301, and the upper rolling part is arranged on the top of the other end;

[0114] The upper rolling part includes a rolling motor 306 and an upper rolling wheel 307. The upper rolling wheel 307 is movably connected to the output rotating shaft of the rolling motor 306 through a rotating shaft.

[0115] like Figure 3-5 As shown, the movable rolling part includes a vertical slot 303, a swing clamping rod 304, a lower rolling wheel 305, a vertical hydraulic cylinder 3010, and a hinged ear plate 3011, which are arranged at a corresponding position in the middle of the pressing column 302. The corresponding position in the middle of the swing clamping rod 304 is movably arranged in the vertical slot 303 through a hinged component, and a lower rolling wheel 305 is arranged at one end thereof, and the lower rolling wheel 305 corresponds to the upper rolling wheel 307. The other end of the swing clamping rod 304 is movably connected to one end of the hinged ear plate 3011, and the other end of the hinged ear plate 3011 is movably connected to one end of the vertical hydraulic cylinder 3010, and the other end of the vertical hydraulic cylinder 3010 is connected to the corresponding position of the pressing base 301.

[0116] like Figure 3 , 4 As shown, the carcass positioning portion is arranged below the movable rolling portion, located above the pressing base 301 and at a corresponding position between the vertical groove 303 on the pressing column 302, and includes a lifting and positioning motor 308 and a positioning support wheel 309. The positioning support wheel 309 is connected to the output shaft of the lifting and positioning motor 308 and corresponds to the lower rolling wheel 305 and the upper rolling wheel 307 vertically in the longitudinal direction up and down.

[0117] like Figure 7 , 8 As shown, further, the device, wherein the tire pressing stabilization mechanism includes a tire pressing movable frame 5, a longitudinal adjustment module 501, a transverse adjustment module 502, a mounting column 503 and a tire pressing installation assembly 504, wherein the longitudinal adjustment module 501 and the transverse adjustment module 502 are arranged at corresponding positions on the tire pressing movable frame 5, one end of the mounting column 503 is fixedly connected to the tire pressing movable frame 5, and the other end is provided with a tire pressing installation assembly 504; the tire pressing installation assembly 504 is used to adjust the corresponding position of the once-polished and vulcanized smooth tire body 101 on the pressing machine device 3, so that the upper rolling wheel 307 and the lower rolling wheel 305 on the pressing machine device 3 perform pressing and compacting processing on the once-polished and vulcanized smooth tire body 101 and the pre-vulcanized tread layer attached to the outer peripheral wall surface thereof along the circumferential direction of the once-polished and vulcanized smooth tire body 101.

[0118] like Fig. 9As shown, the tire pressing and installation assembly 504 is provided with a clamping tire body unit, and the clamping tire body unit includes a clamping slide rail 505, two clamping sliders 506, two clamping roller rods 507, two clamping rollers 508, and a two-way cylinder 509. The two clamping sliders 506 are respectively arranged at corresponding positions on the clamping slide rail 505, one end of the two clamping roller rods 507 is respectively connected to the corresponding positions of the two clamping sliders 506, and the other end is respectively provided with a clamping roller 508, and the two ends of the two-way cylinder 509 are respectively connected to the corresponding positions in the middle of the two clamping roller rods 507. The two clamping rollers 508 can clamp the once-polished and vulcanized smooth tire body 101 that is subjected to pressing and compacting treatment.

[0119] The tire pressing and stabilizing mechanism device disclosed in the present invention is mainly aimed at the fact that the mining truck tire of the truck is large in size and needs to be placed on the corresponding lower rolling wheel 305 and upper rolling wheel 307 on the pressing machine device 3 for pressing and pressing. The longitudinal adjustment module 501 and the lateral adjustment module 502 on the tire pressing and stabilizing mechanism device can adjust and place the secondary vulcanized tire body 101 vertically and horizontally, such as Figure 8 The schematic diagram of the structure of placing the secondary vulcanized tire body 101 on the pressing machine device 3 is shown. Fig. 9 What is shown is a schematic diagram of the mounting frame assembly 504 with two clamping rollers 508 clamping the secondary vulcanized tire body 101. The tightness of the clamping of the two clamping rollers 508 is controlled by a bidirectional cylinder 509, which greatly saves the labor intensity of the workers and also greatly improves the production efficiency.

[0120] Specific working process: after the screened retreadable tire body is processed into a buffer tread rubber retreadable tire body through the above process, it enters the cavity of the primary lower vulcanization cavity 201 of the primary vulcanization mold device 2 for primary vulcanization and corresponding treatment as a primary polished and vulcanized smooth tire body 101, the primary polished and vulcanized smooth tire body 101 is attached to the pre-vulcanized tread layer, and then pressed by the pressing machine device 3 to be a pressed retreadable tire 102, and the pressed flap-type tire 102 is sent into the vulcanization tank inner cavity 402 of the secondary vulcanization tank device 4 for secondary vulcanization treatment in the vulcanization tank device, and is tested and tried as a retreaded tire product.

[0121] The trial situation shows that the retreaded tire product prepared in Example 1 was installed on a mining truck and applied to a large fleet in Qingyuan, Guangdong. The number of retreaded tires used was about 100. After 5-6 months of use, a lot of belt layer steel wires ran into the carcass and punctured the inner tube, making it unusable. Under the same use conditions, the retreaded tires of the prior art generally had the situation of the retreaded tires in this example, with the inner tube punctured and unusable, in 2-3 months. The usage data is shown in Table 1 below.

[0122] Example 2

[0123] This embodiment 2 is also for preparing retreaded tires with product specifications of 14.00R25 or 14.00R24 for mining trucks.

[0124] The present invention discloses a method for refurbishing a mining truck tire carcass by multiple vulcanization molding, which is a process method for refurbishing a mining truck tire carcass by secondary vulcanization molding, and includes the following method steps:

[0125] 1) Selecting tire bodies that can be used for retreading from used tires of mining trucks, which are retreadable tire bodies. The retreadable tire bodies refer to tire bodies whose tire bodies, sidewalls and tire wire layers are not disconnected and are used tires that have been used recently;

[0126] 2) The refurbishable carcass in step 1) is cleaned and cooled and dried, and the drying temperature is controlled at 40-50° C. and the drying time is controlled at 40-65 minutes to obtain a clean refurbishable carcass.

[0127] 3) The original belt layer on the clean retreadable carcass in step 2) is completely peeled off to the tire body steel wire layer, in order to peel off the retreadable carcass,

[0128] 4) Grinding the outer wall of the tire body stripped for retreading in step 3), cleaning the outer wall of the tire until it is clean and free of dust and impurities, and checking that there is no broken steel wire on the outer wall of the tire body stripped for retreading, in order to grind the tire body for retreading,

[0129] 5) Apply glue. After the surface of the carcass that can be refurbished is cleaned by grinding in step 4, apply a layer of glue and dry it for 30-50 minutes. The drying temperature is controlled to be 65-80°C. This is to apply glue to the carcass that can be refurbished.

[0130] 6) Pasting the middle cushion rubber layer, in step 5), the middle cushion rubber layer is pasted on the outer wall surface of the circumference of the surface layer of the side of the tire body that contacts the ground by brushing the glue mortar, and the tire body 6 is pasted with the middle cushion rubber layer, FIG. Fig.11 As shown;

[0131] 7) Attaching a belt layer, attaching a brand new belt layer on the wall surface of the middle cushion layer of the refurbishable carcass 6 of the step 6), wherein the brand new belt layer is made of steel wire material, and the width of the belt layer is controlled to correspond to the width of the middle cushion layer refurbishable carcass 6, and the belt layer refurbishable carcass 7 is attached, preferably, a brand new belt layer containing steel wire material is attached on the surface of the middle cushion layer refurbishable carcass 6, and the number of belt layers attached on the outer surface of the middle cushion layer refurbishable carcass 6 is controlled to be 4; Fig.12 As shown;

[0132] Preferably, the shape of the belt layer attached to the surface of the refurbishable carcass 6 with the middle cushion rubber layer is controlled to be an oblique quadrilateral structure, the length of the belt layer is controlled to be equivalent to the circumference length of the outer wall surface of the refurbishable carcass 6 with the middle cushion rubber layer, and each layer of the belt layer is controlled to be able to be coated on the outer wall surface of the circumference of the refurbishable carcass 6 with the middle cushion rubber layer in sequence.

[0133] like Figure 12-14 As shown, the belt layer directly coated on the outer surface wall of the tire body 6 that can be retreaded with the middle cushion rubber layer is the first belt layer 801, and the corresponding belt layer 802 is attached to the surface wall of the first belt layer 801, and the others are similar, that is, the third belt layer 803 is attached to the outer surface of the second belt layer 802, and the fourth belt layer 804 is attached to the outer surface of the third belt layer 803, and the fifth belt layer 805 is attached to the outer surface of the second belt layer 804; Fig.12 As shown, the angle B1 between the two sides of the oblique quadrilateral of the first belt layer 801 is controlled to be 25.5 degrees. Fig.13 As shown, the angles on both sides of the second belt layer 802 and the remaining belt layers, namely the third belt layer 803 and the fourth belt layer 804, are all B2 = 14.5 degrees; and the width of the second belt layer 802 wrapped on the surface of the tire body 6 that can be retreaded with the middle cushion rubber layer is controlled to be greater than the width of the other belt layers wrapped on the surface of the tire body 6 that can be retreaded with the middle cushion rubber layer. That is, the width of the second belt layer 802 is greater than the width of the first belt layer 801, the third belt layer 803, and the fourth belt layer 804; the width referred to here refers to the width of the belt layer wrapped on the tire body of the retreaded tire. Fig.11 Width dimensions shown, i.e. Fig.13 , 14 The perpendicular distance between the short sides of the two oblique quadrilaterals;

[0134] 8) Pasting buffer glue, pasting buffer glue on the outer wall surface of the belt layer refurbishable carcass 7 in step 7), wherein the buffer glue is an unvulcanized raw rubber sheet;

[0135] 9) First molding, inflation and vulcanization, the cushioning rubber refurbishable tire body prepared in step 8) is placed in the first lower vulcanization cavity 201 of the first vulcanization mold device 2, and the corresponding inner tube is placed in the inner cavity of the cushioning rubber refurbishable tire body, and the inner tube is inflated. After the inflation is completed, the first molding, inflation and vulcanization treatment is performed to obtain a first vulcanized tire body 1. The first molding, inflation and vulcanization conditions are controlled to control the first vulcanization time to 210-300 minutes and the first vulcanization temperature to 150° C.;

[0136] 10) preparing a polished primary vulcanized smooth tire body, moving the primary vulcanized tire body 1 of step 9) out of the corresponding primary lower vulcanization cavity 201 of the primary vulcanization mold device 2, checking whether the primary vulcanized tire body 1 is qualified, performing secondary polishing and secondary cushioning rubber layer treatment on the wall surface of the qualified primary vulcanized tire body 1, and drying to obtain a primary polished vulcanized smooth tire body 101,

[0137] 11), a retreadable tire body is prepared by laminating a pre-cured tread layer on the outer surface of the circumference of the polished and vulcanized tire body 101, or laminating an old tire tread layer, and then sending it to a laminating machine device 3 for laminating treatment, so as to laminar a retreadable tire 102.

[0138] 12) Second vulcanization treatment in a vulcanization tank device, the retreaded tire 102 pressed in step 11) is packaged and placed in the inner cavity of the secondary vulcanization tank device 4, the tank cover 402 of the secondary vulcanization tank device is closed, and the second vulcanization treatment is performed, the second vulcanization treatment time is controlled to be 550 minutes, and the second vulcanization treatment temperature is controlled to be 110-125° C. to prepare a secondary vulcanized retreaded tire product;

[0139] 13) Testing and trial use: testing the secondary vulcanized retreaded tire product prepared in step 12) to see if the vulcanization is in place and whether the retreaded tire body is bulging. If the trial is qualified, the retreaded tire product is obtained.

[0140] In order to increase the roughness of the polished surface of the tire to enhance its bonding force, in Example 1 of the present invention, the roughness of the tread after polishing is controlled to be about RA 6.5.

[0141] Another object of the present invention is to implement the above-mentioned method for refurbishing the tire carcass of a mining truck by vulcanization molding in stages. Figure 1-3 , including a primary vulcanization mold device 2, a pressing machine device 3, and a secondary vulcanization tank device 4. The primary vulcanization mold device 2 includes a primary lower vulcanization chamber 201, a positioning boss 202 arranged at the center of the inner cavity of the primary lower vulcanization chamber 201, a guide rail bracket 203, a fixed cross bar 204, a primary upper vulcanization chamber 205, an upper positioning platen 206, a first hydraulic cylinder 207, an exhaust hose 208, a primary vulcanization electric control box 209 and a lower positioning base plate seat 210. The primary lower vulcanization chamber 201 is arranged on the lower positioning base plate seat 210, one end of the guide rail bracket 203 is fixedly connected to the lower positioning base plate seat 210, and the other end is fixedly connected to the upper positioning platen 206. The secondary upper vulcanization chamber 205 is correspondingly arranged above the primary lower vulcanization chamber 201 and connected to the guide rail bracket 203 through the fixed cross bar 204. The first hydraulic cylinder 207 is arranged above the upper positioning platen 206 and is correspondingly connected to the primary upper vulcanization chamber 205 and the primary lower vulcanization chamber 201 through corresponding pipelines; the secondary vulcanization tank device 4 includes a vulcanization tank body 401, a vulcanization tank inner cavity 402, a tank cover 403, a vulcanization tank bracket 404, a vulcanization control instrument 405, a vulcanization tank control box 406 and an exhaust pipe 407 arranged on the vulcanization tank body 401, and the pressed retread tire 102 can be placed in the hollow inner cavity of the vulcanization tank inner cavity 402 for secondary vulcanization treatment;

[0142] Specifically, the laminating machine device 3 includes a laminating and clamping mechanism and a tire laminating and stabilizing mechanism;

[0143] like Figure 3 , 4 As shown, the pressing and clamping mechanism includes a pressing base 301, a pressing column 302, an upper rolling part, a movable rolling part and a carcass positioning part; one end of the pressing column 302 is fixedly connected to the corresponding position of the pressing base 301, and the upper rolling part is arranged on the top of the other end;

[0144] The upper rolling part includes a rolling motor 306 and an upper rolling wheel 307. The upper rolling wheel 307 is movably connected to the output rotating shaft of the rolling motor 306 through a rotating shaft.

[0145] like Figure 3-5 As shown, the movable rolling part includes a vertical slot 303, a swing clamping rod 304, a lower rolling wheel 305, a vertical hydraulic cylinder 3010, and a hinged ear plate 3011, which are arranged at a corresponding position in the middle of the pressing column 302. The corresponding position in the middle of the swing clamping rod 304 is movably arranged in the vertical slot 303 through a hinged component, and a lower rolling wheel 305 is arranged at one end thereof, and the lower rolling wheel 305 corresponds to the upper rolling wheel 307. The other end of the swing clamping rod 304 is movably connected to one end of the hinged ear plate 3011, and the other end of the hinged ear plate 3011 is movably connected to one end of the vertical hydraulic cylinder 3010, and the other end of the vertical hydraulic cylinder 3010 is connected to the corresponding position of the pressing base 301.

[0146] like Figure 3 , 4 As shown, the carcass positioning portion is arranged below the movable rolling portion, located above the pressing base 301 and at a corresponding position between the vertical groove 303 on the pressing column 302, and includes a lifting and positioning motor 308 and a positioning support wheel 309. The positioning support wheel 309 is connected to the output shaft of the lifting and positioning motor 308 and corresponds to the lower rolling wheel 305 and the upper rolling wheel 307 vertically in the longitudinal direction up and down.

[0147] like Figure 7 , 8 As shown, further, the device, wherein the tire pressing stabilization mechanism includes a tire pressing movable frame 5, a longitudinal adjustment module 501, a transverse adjustment module 502, a mounting column 503 and a tire pressing installation assembly 504, wherein the longitudinal adjustment module 501 and the transverse adjustment module 502 are arranged at corresponding positions on the tire pressing movable frame 5, one end of the mounting column 503 is fixedly connected to the tire pressing movable frame 5, and the other end is provided with a tire pressing installation assembly 504; the tire pressing installation assembly 504 is used to adjust the corresponding position of the once-polished and vulcanized smooth tire body 101 on the pressing machine device 3, so that the upper rolling wheel 307 and the lower rolling wheel 305 on the pressing machine device 3 perform pressing and compacting processing on the once-polished and vulcanized smooth tire body 101 and the pre-vulcanized tread layer attached to the outer peripheral wall surface thereof along the circumferential direction of the once-polished and vulcanized smooth tire body 101.

[0148] like Fig. 9 As shown, the tire pressing and installation assembly 504 is provided with a clamping tire body unit, and the clamping tire body unit includes a clamping slide rail 505, two clamping sliders 506, two clamping roller rods 507, two clamping rollers 508, and a two-way cylinder 509. The two clamping sliders 506 are respectively arranged at corresponding positions on the clamping slide rail 505, one end of the two clamping roller rods 507 is respectively connected to the corresponding positions of the two clamping sliders 506, and the other end is respectively provided with a clamping roller 508, and the two ends of the two-way cylinder 509 are respectively connected to the corresponding positions in the middle of the two clamping roller rods 507. The two clamping rollers 508 can clamp the once-polished and vulcanized smooth tire body 101 that is subjected to pressing and compacting treatment.

[0149] The tire pressing and stabilizing mechanism device disclosed in the present invention is mainly aimed at the fact that the mining truck tire of the truck is large in size and needs to be placed on the corresponding lower rolling wheel 305 and upper rolling wheel 307 on the pressing machine device 3 for pressing and pressing. The longitudinal adjustment module 501 and the lateral adjustment module 502 on the tire pressing and stabilizing mechanism device can adjust and place the secondary vulcanized tire body 101 vertically and horizontally, such as Figure 8 The schematic diagram of the structure of placing the secondary vulcanized tire body 101 on the pressing machine device 3 is shown. Fig. 9 What is shown is a schematic diagram of the mounting frame assembly 504 with two clamping rollers 508 clamping the secondary vulcanized tire body 101. The tightness of the clamping of the two clamping rollers 508 is controlled by a bidirectional cylinder 509, which greatly saves the labor intensity of the workers and also greatly improves the production efficiency.

[0150] Specific working process: after the screened retreadable tire body is processed into a buffer tread rubber retreadable tire body through the above process, it enters the cavity of the primary lower vulcanization cavity 201 of the primary vulcanization mold device 2 for primary vulcanization and corresponding treatment as a primary polished and vulcanized smooth tire body 101, the primary polished and vulcanized smooth tire body 101 is attached to the pre-vulcanized tread layer, and then pressed by the pressing machine device 3 to be a pressed retreadable tire 102, and the pressed flap-type tire 102 is sent into the vulcanization tank inner cavity 402 of the secondary vulcanization tank device 4 for secondary vulcanization treatment in the vulcanization tank device, and is tested and tried as a retreaded tire product.

[0151] The trial results show that the retreaded mining truck tires prepared in Example 1 were used in a large fleet in Qingyuan, Guangdong. The number of retreaded tires used was about 100. After 5-6 months of use, many belt layer steel wires were found to run into the carcass and punctured the inner tube, making it unusable. Under the same use conditions, the retreaded tires of the prior art generally had the situation of the retreaded tires of this embodiment punctured and unusable after 2-3 months.

[0152] Embodiment 3,

[0153] In order to improve the roughness of the tire grinding surface to enhance its adhesion, the roughness of the tire tread after grinding is controlled to be around RA 6.4.

[0154] The tire pressing and stabilizing mechanism device disclosed in the present invention is mainly aimed at the fact that the mining truck tires of the truck are large in size and need to be placed on the corresponding lower rolling wheel 305 and upper rolling wheel 307 on the pressing machine device 3 for pressing and pressing. The longitudinal adjustment module 501 and the lateral adjustment module 502 on the tire pressing and stabilizing mechanism device can adjust and place the polished and vulcanized tire body 101 in the vertical and lateral directions, such as Figure 8 The schematic diagram of the structure of placing the once-polished and vulcanized smooth tire body 101 on the laminating machine device 3 is shown. Fig. 9 What is shown is a schematic diagram of the polished and vulcanized smooth tire body 1011 being clamped once by two clamping rollers 508 of the mounting frame assembly 504. The tightness of the clamping of the two clamping rollers 508 is controlled by a two-way cylinder 509, which greatly saves the labor intensity of the workers and also greatly improves their production efficiency.

[0155] Specific working process: after the screened retreadable tire body is processed into a buffer tread rubber retreadable tire body through the above process, it enters the cavity of the primary lower vulcanization cavity 201 of the primary vulcanization mold device 2 for primary vulcanization and corresponding treatment as a primary polished and vulcanized smooth tire body 101, the primary polished and vulcanized smooth tire body 101 is attached to the pre-vulcanized tread layer, and then pressed by the pressing machine device 3 to be a pressed retreadable tire 102, and the pressed flap-type tire 102 is sent into the vulcanization tank inner cavity 402 of the secondary vulcanization tank device 4 for secondary vulcanization treatment in the vulcanization tank device, and is tested and tried as a retreaded tire product.

[0156] The trial situation shows that the retreaded mining truck tires prepared in Example 3 were applied to a large fleet in Qingyuan, Guangdong, with about 100 retreaded tires and a mining site in Panzhihua Iron and Steel Group, Sichuan. After 5-6 months of use, a lot of belt layer steel wires ran into the tire body and punctured the inner tube, making it unusable. Other test data are slightly higher than those in Examples 1 and 2. Similarly, the retreaded tires prepared by the prior art had inner tube punctures after about 3 months of use and could not be used. The retreaded tires prepared in the following comparative examples are the same as those in the above examples. This is the inventor's description of the experimental process.

[0157] Comparative Example 1

[0158] The retreadable tire body and preparation method steps used in Comparative Example 1 of the present invention are the same as those of the present invention and Example 1, and other technical parameter controls are also carried out according to the existing technical scheme. Moreover, Comparative Example 1 adopts a one-time vulcanization process technology method, and at the same time, the existing device is used for compaction and pressing during pressing to prepare a retreaded tire product.

[0159] The trial situation shows that the retreaded mining truck tire prepared in comparative example 1 was applied to a large fleet in Qingyuan, Guangdong. The number of retreaded tires used was about 100. After 2-3 months of use, a large number of belt layer steel wires were found to run into the carcass and puncture the inner tube, making it unusable. At the same time, since the tire surface and the carcass layer could not be effectively combined during the vulcanization of the tire without the use of reinforced slurry, the prepared tread layer was not wear-resistant, and the risk factor of tire explosion increased until the carcass and tread delamination occurred, resulting in degumming and easy tire explosion.

[0160] Comparative Example 2

[0161] The retreadable tire body and other technical parameters of the preparation method used in Comparative Example 2 of the present invention are the same as those of Example 2, but the difference is that Comparative Example 1 adopts a one-time vulcanization process and a conventional slurry glue is used in the slurry material for applying the slurry layer, and the pressing machine device 3 used in Examples 1 and 2 of the present invention is not used for pressing and pressing to prepare the retreaded tire product. By comparison, the preparation efficiency is more than 20% lower than that of Examples 1 and 2, and the labor intensity of the workers is also greater.

[0162] The trial situation shows that the retreaded mining truck tires prepared in comparative example 2 were applied to a large fleet in Qingyuan, Guangdong, and a construction site of Panzhihua Iron and Steel Group. The number of retreaded tires used was about 100. After 2-3 months of use, a large number of belt layer steel wires were found to penetrate into the carcass and puncture the inner tube, making it unusable. At the same time, since the tire surface and the carcass layer cannot be effectively combined during the vulcanization of the tire without the use of reinforced slurry, the prepared tread layer is not wear-resistant, and the risk factor of tire explosion increases until the carcass and tread delamination occurs, degumming occurs, and the tire is easy to explode. Other test data are shown in Tables 1 and 2.

[0163] The retreaded tire for mining trucks, i.e., the retreaded tire for trucks, prepared by the above method of the present invention has been tested by relevant departments, and the main technical parameters are as follows:

[0164] Testing basis: The strength test of this retreaded tire is carried out according to the method specified in GB / T 5327, and the testing site is the industrial and mining sites in Sichuan and Guangdong Province. No defects in appearance.

[0165] Table 1, test data:

[0166] Shore A hardness / degree Tear strength / (kN·m-1) Example 1 71 89.68 Example 2 68 89.14 Comparative Example 1 55 70.42 Comparative Example 2 54 66.86

[0167] Description: From the test data in Table 1 above, it can be seen that the retreaded tire prepared by the method and device of the present invention has excellent hardness, tear strength and cutting resistance. The retreaded tire of the present invention has a large adhesion between each layer and high strength. At the same time, it adopts 4-5 layers of belt layers containing steel wires, and controls the angle of the first belt layer to be about 25 degrees, which is larger than the angle of about 13 degrees of the other belt layers of the second to fifth layers, and at the same time controls the width of the second belt layer 802 to be larger than the width of the first, third to fifth belt layers, so that the tear strength of the tire is significantly improved. This is because the present invention adopts the above-mentioned belt layer structure. With the reduction of the belt layer angle and the narrowing of the width, the rigidity of the retreaded tire increases, the sinking amount is reduced, the contact area is correspondingly reduced, the shear stress of the tire is also reduced, etc., and the performance of the retreaded tire is improved. At the same time, the present invention adopts the above-mentioned press device structure, which also greatly improves the work efficiency when retreading tires and reduces the labor intensity of workers. The data of Example 3 is slightly higher than that of Examples 1 and 2, and the description is omitted here.

[0168] In the tear strength test, according to the relevant national testing standards, the retreaded tires prepared in the embodiments of the present invention are described by the number of wounds longer than 30 mm as tested in Table 2 below. Table 2 below is a tear wound test report, which is described by the data of 200 hours of operation. It mainly shows the number of wounds longer than 30 mm and the average number of wounds under trial conditions.

[0169] Table 2

[0170]

[0171] It is noted that the test methods of the performance parameters of the above test reports can be carried out in accordance with relevant national standards or industry standards. It can be seen from the above test data that the retreaded tire prepared by the method and device disclosed in the present invention has enhanced tear strength and significantly improved cut resistance due to the use of the above belt layer structure and the secondary vulcanization treatment of the tire body. The number of wounds of 30 mm in length is significantly less than that of the retreaded tires in the prior art. Effectively save resources. Realize the effective recycling of waste resources.

Claims

1. A method for refurbishing a mining truck tire carcass by secondary vulcanization molding, which is a process method for refurbishing a mining truck tire carcass by secondary vulcanization molding, and is characterized by: The method comprises the following steps: 1) Select the tire bodies that can be used for retreading from the used tires of mining trucks, which are the retread tire bodies. 2) Clean the refurbishable carcass in step 1, cool and dry it, and control the drying temperature to 40-50℃ and the drying time to 40-65 minutes to make a clean refurbishable carcass. 3) For step 2), the original belt layer on the clean retreadable carcass is completely peeled off to the tire body steel wire layer. To peel off the retreadable carcass, 4) Grind the outer wall of the tire body that can be retreaded in step 3), clean the outer wall of the tire until it is clean and free of dust and impurities, and check that there are no broken wires on the outer wall of the tire body that can be retreaded. 5) Apply glue. After the surface of the carcass that can be refurbished is cleaned by grinding in step 4, apply a layer of glue and dry it for a total of 30-50 minutes. The drying temperature is controlled at 65-80℃. This is to apply glue to the carcass that can be refurbished. 6) Pasting the middle cushion rubber layer, pasting the middle cushion rubber layer on the outer wall surface of the surface layer of the tire body in contact with the ground in step 5), which is pasting the middle cushion rubber layer on the tire body (6). 7) Attaching a belt layer: attaching a new belt layer on the wall surface of the middle cushion layer of the refurbishable carcass (6) in step 6), controlling the width of the belt layer to correspond to the width of the middle cushion layer refurbishable carcass (6), to form a belt layer refurbishable carcass (7). 8) applying buffer glue, applying buffer glue on the outer wall surface of the belt layer retreadable carcass (7) in step 7), wherein the buffer glue is an uncured raw rubber sheet; 9) First molding, inflation and vulcanization, the cushioning rubber refurbishable tire body prepared in step 8) is placed in the inner cavity of the primary lower vulcanization cavity (201) of the primary vulcanization mold device (2), and a corresponding inner tube is placed in the inner cavity of the cushioning rubber refurbishable tire body, and the inner tube is inflated. After the inflation is completed, the first molding, inflation and vulcanization treatment is performed to obtain a primary vulcanized tire body (1). 10) preparing a polished primary vulcanized smooth tire body, moving the primary vulcanized tire body (1) of step 9) out of the primary vulcanization mold device (2), checking whether the primary vulcanized tire body (1) is qualified, performing secondary polishing and secondary cushioning rubber layer treatment on the wall surface of the qualified primary vulcanized tire body (1), and drying to obtain a primary polished vulcanized smooth tire body (101). 11), a retreadable tire body is prepared by laminating a pre-cured tread layer or an old tire tread on the outer wall of the circumference of the polished and vulcanized tire body (101), and then the pre-cured tread layer is attached to the outer wall of the circumference of the tire body (101), and the tire body (101) is sent to a laminating machine (3) for laminating to form a retreadable tire (102). 12) performing a second vulcanization treatment in a vulcanization tank device, packaging and packaging the retreaded tire (102) pressed in step 11) and placing it in the inner cavity of a secondary vulcanization tank device (4), closing the lid (402) of the secondary vulcanization tank device, performing a second vulcanization treatment, and manufacturing a secondary vulcanized retreaded tire product; 13) Testing and trial use: The secondary vulcanized retreaded tire product prepared in step 12) is tested to see whether the vulcanization is in place and whether the retreaded tire body is bulging. If the trial is qualified, it is a retreaded tire product.

2. The method for refurbishing a mining truck tire carcass by vulcanization molding in batches according to claim 1, characterized in that: The retreadable tire body in step 1) refers to a tire body for retreading whose tire body, sidewalls and tire wire layer are not disconnected and is a used tire that has been used recently.

3. The method for refurbishing a mining truck tire carcass by vulcanization molding in batches according to claim 1, characterized in that: Step 7) pasting the belt layer, pasting a new belt layer containing steel wire material on the surface of the tire body (6) that can be refurbished by pasting the middle cushion rubber layer, and controlling the number of belt layers pasted on the outer surface of the tire body (6) that can be refurbished by pasting the middle cushion rubber layer to be 4-5 layers.

4. The method for refurbishing a mining truck tire carcass by vulcanization molding in batches according to claim 1, characterized in that: Step 9) First molding, inflation and vulcanization. The conditions for the first molding, inflation and vulcanization are as follows: the first vulcanization time is controlled to be 210-300 minutes, and the first vulcanization temperature is controlled to be 142-155°C.

5. The method for refurbishing a mining truck tire carcass by vulcanization molding in batches according to claim 1, characterized in that: Step 12) Perform the second vulcanization treatment in a vulcanization tank, control the second vulcanization treatment time to be 400-600 minutes, and the second vulcanization treatment temperature to be 110-125°C.

6. The method for refurbishing a mining truck tire carcass by vulcanization molding in batches according to claim 3, characterized in that: The shape of the belt layer attached to the surface of the refurbishable carcass (6) with the middle cushion rubber layer is controlled to be an oblique quadrilateral structure, the length of the belt layer is controlled to be equal to the circumference length of the outer wall surface of the refurbishable carcass (6) with the middle cushion rubber layer, and each layer of the belt layer is controlled to be able to be coated on the outer wall surface of the circumference of the refurbishable carcass (6) with the middle cushion rubber layer in sequence.

7. A method for refurbishing a mining truck tire carcass by vulcanization molding in batches according to claim 3 or 6, characterized in that: The belt layer directly coated on the outer surface of the tire body 6 that can be refurbished with the middle cushion rubber layer is controlled to be the first belt layer (801), and the corresponding belt layer attached to the surface of the first belt layer (801) is the second belt layer (802), and the others are similar. The angle B1 between the two sides of the oblique quadrilateral of the first belt layer (801) is controlled to be 24.5-25.5 degrees, and the angles between the two sides of the second belt layer (802) and the remaining belt layers are all controlled to be B2=13.5-14.5 degrees; and the width of the second belt layer (802) coated on the surface of the tire body (6) that can be refurbished with the middle cushion rubber layer is controlled to be larger than the width of other belt layers coated on the surface of the tire body (6) that can be refurbished with the middle cushion rubber layer.

8. A device for realizing the method for refurbishing a mining truck tire carcass by stepwise vulcanization molding as claimed in claim 1, comprising a primary vulcanization mold device (2), a pressing machine device (3), and a secondary vulcanization tank device (4), wherein the primary vulcanization mold device (2) comprises a primary lower vulcanization chamber (201), a positioning boss (202) arranged at the center of the inner cavity of the primary lower vulcanization chamber (201), a guide rail bracket (203), a fixed cross bar (204), a primary upper vulcanization chamber (205), an upper positioning platen (206), a first hydraulic cylinder (207), an exhaust hose (208), a primary vulcanization electric control box (209), and a lower positioning base plate seat (210), wherein the primary lower vulcanization chamber (201) is arranged on the lower positioning base plate seat (210), and one end of the guide rail bracket (203) is fixed to the lower positioning base plate seat (210). The first upper vulcanizing chamber (205) is fixedly connected to the lower positioning base plate (210) and the other end is fixedly connected to the upper positioning plate (206). The first upper vulcanizing chamber (205) is correspondingly arranged above the first lower vulcanizing chamber (201) and connected to the guide rail bracket (203) through a fixed cross bar (204). The first hydraulic cylinder (207) is arranged above the upper positioning plate (206) and is correspondingly connected to the first upper vulcanizing chamber (205) and the first lower vulcanizing chamber (201) through corresponding pipelines. The secondary vulcanizing tank device (4) includes a vulcanizing tank body (401), a vulcanizing tank inner cavity (402), a tank cover (403), a vulcanizing tank bracket (404), a vulcanizing control instrument (405), a vulcanizing tank control box (406) and an exhaust pipe (407) arranged on the vulcanizing tank body (401). The pressed retreaded tire (102) can be placed in the hollow inner cavity of the vulcanizing tank inner cavity 402 for secondary vulcanization treatment; Its characteristics are: The laminating machine device (3) comprises a laminating and clamping mechanism and a tire laminating and stabilizing mechanism; The pressing and clamping mechanism comprises a pressing base (301), a pressing column (302), an upper rolling portion, a movable rolling portion and a carcass positioning portion; one end of the pressing column (302) is fixedly connected to a corresponding position of the pressing base (301), and the top of the other end is provided with an upper rolling portion; The upper rolling part comprises a rolling motor (306) and an upper rolling wheel (307), and the upper rolling wheel (307) is movably connected to the output rotating shaft of the rolling motor (306) via a rotating shaft; The movable rolling part comprises a vertical groove (303) arranged at a corresponding position in the middle of the pressing column (302), a swing clamping rod (304), a lower rolling wheel (305), a vertical hydraulic cylinder (3010), and a hinged ear plate (3011); the corresponding position in the middle of the swing clamping rod (304) is movably arranged in the vertical groove (303) through a hinged component, one end of the swing clamping rod is provided with a lower rolling wheel (305), the lower rolling wheel (305) corresponds to the upper rolling wheel (307), the other end of the swing clamping rod (304) is movably connected to one end of the hinged ear plate (3011), the other end of the hinged ear plate (3011) is movably connected to one end of the vertical hydraulic cylinder (3010), and the other end of the vertical hydraulic cylinder (3010) is connected to a corresponding position of the pressing base (301); The carcass positioning portion is arranged below the movable rolling portion, located above the pressing base (301) and at a corresponding position between the vertical groove (303) on the pressing column (302), and comprises a lifting and positioning motor (308) and a positioning support wheel (309). The positioning support wheel (309) is connected to the output shaft of the lifting and positioning motor (308) and corresponds to the lower rolling wheel (305) and the upper rolling wheel (307) vertically in the longitudinal direction.

9. The device according to claim 8, characterized in that: The tire pressing stabilizing mechanism comprises a tire pressing movable frame (5), a longitudinal adjustment module (501), a transverse adjustment module (502), a mounting frame column (503) and a tire pressing mounting assembly (504); the longitudinal adjustment module (501) and the transverse adjustment module (502) are arranged at corresponding positions on the tire pressing movable frame (5); one end of the mounting frame column (503) is fixedly connected to the tire pressing movable frame (5), and the other end is provided with a tire pressing mounting assembly (504); the corresponding position of the once-polished and vulcanized smooth tire body (101) on the pressing machine device (3) is adjusted by the tire pressing mounting assembly (504), so that the upper rolling wheel (307) and the lower rolling wheel (305) on the pressing machine device (3) perform pressing and compacting processing on the once-polished and vulcanized smooth tire body (101) and the molded pattern rubber layer attached to the outer surface wall of the circumference thereof along the circumference direction of the once-polished and vulcanized smooth tire body (101).

10. The device according to claim 8, characterized in that: The tire pressing and installation assembly (504) is provided with a clamping tire body unit, which comprises a clamping slide rail (505), two clamping sliders (506), two clamping roller rods (507), two clamping rollers (508), and a bidirectional cylinder (509). The two clamping sliders (506) are respectively arranged at corresponding positions on the clamping slide rail (505). One end of the two clamping roller rods (507) is respectively connected to corresponding positions of the two clamping sliders (506), and the other end is respectively provided with a clamping roller (508). The two ends of the bidirectional cylinder (509) are respectively connected to corresponding positions in the middle of the two clamping roller rods (507). The two clamping rollers (508) can clamp the polished and vulcanized smooth tire body (101) that is subjected to a pressing and compacting process.

Citation Information

Patent Citations

  • Method for preparing rounded pre-vulcanized tyre surface of giant-scale tyre for mining by screw-type pushing-in process

    CN104441722A

  • Expandable rim for tire tread buffing apparatus and method

    CN107405850A

  • Construction machine tire retreading method

    CN110014681A

  • Method for retreading tire

    CN112606454A

  • Tire retreading process

    CN113085239A