Preparation method of controllable nanowire composite micro-channel etched with assistance of microsphere template

The preparation of nanowire composite microflowers through downic liquid method and plasma etching technology solved the problem of low heat transfer performance of microflower radiator, achieved the stability and simplicity of template preparation, and expanded the application range of materials.

CN119079929AActive Publication Date: 2024-12-06DALIAN UNIV OF TECH
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202411192763.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing microflower radiators have low heat transfer performance due to high pressure drop and flow boiling instability, and the stability and uniformity of single-layer microsphere templates are difficult to control, which affects the nanowire composite microflower preparation.

Method used

The monolayer polystyrene microsphere template was prepared by the downliquid method, and the template size was adjusted by plasma etching. Combined with magnetron sputtering and water bath etching technology, controllable nanowire composite microflower was prepared instead of lifting method. Improve the stability and simplicity of template preparation.

Benefits of technology

It effectively solves the stability and uniformity of the template preparation of lifting method, reduces the cost and experimental cycle, realizes controllable preparation of nanowire structure, and expands to the surface applications of other new materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079929A_ABST
    Figure CN119079929A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a controllable nanowire composite micro-channel through microsphere template auxiliary etching, and belongs to the field of micro-nano structure surface preparation and reinforced heat dissipation structure.The method comprises the steps that a single-layer polystyrene microsphere template is prepared through a down-flow method, and the size of the single-layer polystyrene microsphere template is regulated through plasma etching; the preparation method disclosed by the invention effectively makes up for the defects of an existing Czochralski method for preparing a single-layer template, and proposes that a plasma etching method is adopted to replace a common reactive ion etching method to adjust the size of the template at the same time; and the nanowire structure is prepared under the assistance of the microsphere template.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of micro-nano structure surface preparation and enhanced heat dissipation structure, and in particular relates to a method for preparing a controllable nanowire composite microchannel assisted by microsphere template etching. Background Art

[0002] Microfluidic heat dissipation technology has received extensive attention and research due to its ultra-high heat transfer efficiency and compact design. Microfluidic heat sinks use the advantages of microscale effects and phase change latent heat to achieve high heat flux density heat dissipation. Due to the extremely small size of the microchannel structure, the heat exchange area between the working fluid and the flow channel is increased, which makes the working fluid temperature rise very quickly, greatly improving the heat dissipation efficiency. Due to the advantages of good temperature uniformity, simple equipment system structure, small mass, and stable operation, the microfluidic heat dissipation system is expected to become one of the solutions for heat dissipation of high-density heat-generating electronic equipment in the future, and has broad application prospects in computer chip cooling, aerospace, phased array radar antenna heat dissipation and other fields.

[0003] At present, the widespread application of microchannel heat sinks faces some challenges: high pressure drop and flow boiling instability lead to low heat transfer coefficient and critical heat flux (CHF). Flow boiling instability can seriously affect the heat transfer performance of the working fluid in the microchannel. The pressure drop, wall temperature and mass flux in the microchannel oscillate during flow boiling. Transient flow pattern alternation may lead to counterflow, rapid growth and expansion of bubbles and even reflux. The existence of system pressure leads to instability of flow boiling in the microchannel, resulting in temperature oscillation, which in turn affects the stability of system pressure and creates a vicious cycle. In addition, the size of the microchannel, volume compressibility and unstable flow of the heat dissipating medium will also affect the pressure. With the increase of heat dissipation flux, the steam gradually increases, and then the vapor phase will occupy the entire flow channel, and even reverse flow will occur.

[0004] Based on the current research status, the micro-nanostructure modification of the microfluidic channel wall to enhance the heat transfer performance has certain research prospects. The modification of super-wetting micro-nanostructures in the microfluidic channel can significantly increase the heat transfer area of ​​the microfluidic channel, while interrupting and redeveloping the flow and thermal boundary layer, achieving the effect of improving the two-phase convection heat transfer. On the other hand, the enhanced structure can also increase the effective nucleation sites of bubbles, promote bubble nucleation, thereby promoting two-phase flow behavior and reducing serious two-phase flow instability. At present, the material of the chip is mainly silicon. The use of nanostructures to modify the microfluidic channel wall is superior to other structures in terms of manufacturing difficulty. It can also change the properties of the wall from a microscopic perspective and has excellent stability.

[0005] At present, the preparation process of silicon nanowires is very mature, including: chemical vapor deposition, molecular beam epitaxy (MEB), laser ablation (LA), oxide-assisted, solution method and etching method. According to the growth mode, it is mainly divided into bottom-up increment and top-down reduction. The bottom-up growth mode uses silicon or silicon compounds as the source, and forms nanoclusters and molecular / atomic crystals through high-temperature decomposition, and combines phase change to realize the transformation of gas phase / liquid phase silicon source to solid silicon nanowires. The preparation processes of this mode mainly include: metal catalyzed gas-liquid-solid (VLS) method, supercritical solution-liquid-solid (SFLS) synthesis method, solid-liquid-solid (SLS) growth method, oxide-assisted growth method, etc. The top-down growth mode is based on silicon bulk material, and uses chemical reaction or physical process to reduce silicon material from macroscopic scale to nanoscale to realize the preparation of nanowire array. The preparation processes of this mode mainly include plasma etching, reactive ion etching (RIE), metal-assisted chemical etching (MACE), etc. The bottom-up preparation method can selectively prepare nanowires of corresponding sizes, and the parameters such as diameter and length are more controllable, but this method has extremely high requirements for equipment and is very costly, and is only applicable to the preparation of single nanowires. The top-down preparation method is not completely controllable.

[0006] The controllable preparation of micro-nano structures is closely related to the distribution of metal catalysts in the metal-assisted method. The microsphere template-assisted method can effectively solve the problem of uniform and controllable distribution of templates, thereby realizing the controllable preparation of micro-nano structures such as nanowires. The most critical part of the template-assisted preparation process is the preparation of a single-layer microsphere template. Currently, the common methods for preparing a single-layer template are spin coating and Czochralski method.

[0007] Spin coating is a common surface preparation method in experiments. It is widely used because of its controllable and efficient characteristics. The operation of spin coating is also very simple. You only need to control the corresponding parameters. This method requires attention to the amount of dripping, rotation speed and rotation time. If too much dripping is added, multiple layers will be formed. If too little dripping is added, the surface microspheres will be too dispersed. If the rotation is too fast, the microspheres will gather to the edge or even be thrown out of the surface due to the centrifugal force. If it is too slow, the microspheres cannot reach the edge of the surface and only spread in the center. The same is true for the rotation time and speed. If it is too long, there will be too much at the edge, and if it is too short, it will only spread in the center.

[0008] The pulling method is very common in template self-assembly. The operation steps are very simple, but it is difficult to achieve successfully. The most important thing to pay attention to in the pulling method is the speed of adding the microsphere solution and the pulling speed. The needle of the syringe should not be too thick, and the solution must be added slowly along the wall. Too fast will cause the microspheres to rush into the solution and fail to fully spread on the surface to form a continuous microsphere film. Secondly, the pulling speed and stability are also the key to the experiment. The pulling should not be too fast, resulting in the surface not being able to fully contact the microsphere film and being pulled out of the liquid. Secondly, the pulling process must maintain a uniform speed so that the template on the surface is uniform. Stability is also a very important but difficult to control point. Slight shaking during the pulling process will cause the microsphere film on the surface to be shaken and destroyed, and the resulting template will be uneven.

[0009] The preparation of templates in microfluidic channels has more limitations than that on a plane, and the simple and fast spin coating method cannot be applied in microfluidic channels. Summary of the invention

[0010] In order to solve the above technical problems, the present invention proposes a method for preparing a controllable nanowire composite microfluidic channel assisted by microsphere template etching. The present invention adopts a liquid drop method to prepare a single-layer polystyrene microsphere template, adopts plasma etching to adjust the size of the single-layer polystyrene microsphere template, and obtains the controllable nanowire composite microfluidic channel after magnetron sputtering and water bath etching. This preparation method effectively makes up for the shortcomings of the existing pulling method for preparing a single-layer template, and at the same time proposes to use plasma etching instead of the commonly used reactive ion etching method to adjust the template size, so as to realize the microsphere template-assisted preparation of nanowire structures.

[0011] To achieve the above object, the present invention provides the following technical solutions:

[0012] A method for preparing a controllable nanowire composite microchannel assisted by microsphere template etching, comprising: preparing a single-layer polystyrene (PS) microsphere template by a liquid drop method, regulating the size of the single-layer polystyrene microsphere template by plasma etching, and obtaining the controllable nanowire composite microchannel by magnetron sputtering and water bath etching.

[0013] Preferably, the method for preparing the controllable nanowire composite microfluidic channel assisted by microsphere template etching comprises the following steps:

[0014] Pre-treating the substrate material;

[0015] The PS microsphere solution was diluted, the supernatant was mixed with anhydrous ethanol after centrifugation, and the mixture was obtained after ultrasonication in ice water;

[0016] The liquid-dropping funnel is fixed vertically on an iron frame, the mixed liquid is sucked into a syringe, and the syringe containing the mixed liquid is fixed vertically on the iron frame, the syringe is located above the liquid-dropping funnel, the needle tip of the syringe is close to the inner wall of the liquid-dropping funnel, and a container is provided below the liquid-dropping funnel, the container is used to hold the solution dripping from the liquid-dropping funnel;

[0017] The piston of the liquid-dropping funnel is closed, a silicon wafer is placed in the liquid-dropping funnel, and water is poured in until the silicon wafer is submerged; the piston of the syringe is pulled out to allow the PS microsphere solution to move downward under the action of gravity, so that the mixed solution can slide toward the water surface along a fixed path, and the dripping speed of the mixed solution at the needle tip of the syringe is controlled so that continuous ripples can be formed on the water surface. After the mixed solution is dripped, it is allowed to stand to allow the PS microspheres to spread completely on the liquid surface (the liquid surface here refers to the interface formed by the mixed solution sliding from the syringe and the water in the liquid-dropping funnel). After the liquid surface is stable, the piston of the liquid-dropping funnel is opened to allow water to drip into the container, and the liquid surface is kept to drop without fluctuation until the liquid surface is lower than the silicon wafer, and the PS microspheres remain on the silicon wafer. After standing, it is dried to obtain a single-layer PS microsphere template;

[0018] The single-layer PS microsphere template is etched by plasma etching, and then a layer of noble metal catalyst is sputtered at the gaps of the PS microsphere template by magnetron sputtering, and etching is performed under water bath conditions to obtain the controllable nanowire composite microchannel.

[0019] Considering that the speed and stability issues during the pulling process are difficult to solve, the present invention uses reverse thinking to allow the liquid level to decrease at a uniform rate, and finally attach the PS microspheres to the surface, i.e., the liquid drop method. The present invention uses the liquid drop method to prepare a controllable nanowire composite microfluidic channel. The present invention uses the liquid drop method instead of the pulling method to prepare the template, which effectively solves the problem of uneven template preparation due to operational stability caused by the pulling method, and the present invention uses a plasma etching method to control the template size, which has a low cost and a short experimental cycle, and the preparation process is more concise.

[0020] Preferably, the method for pretreating the substrate material comprises the following steps: cleaning the substrate material, drying it with nitrogen, and then performing surface hydrophilic treatment.

[0021] More preferably, the method for pretreating the substrate material is:

[0022] (1) Ultrasonic treatment with acetone for 10 min to remove organic impurities on the surface;

[0023] (2) Cleaning the silicon wafer with dilute hydrofluoric acid (HF with a mass concentration of 40% and H2O mixed in a volume ratio of 1:2) for 15 minutes to remove the native oxide layer on the surface of the silicon wafer;

[0024] (3) Ultrasonic cleaning with deionized water for 10 min to remove residual solution;

[0025] (4) heating a mixture of hydrochloric acid and hydrogen peroxide (HCl with a mass concentration of 36-38%, H2O2 with a mass concentration of 30% and H2O in a volume ratio of 1:1:5) in a 70° C. water bath for 25 min;

[0026] (5) ultrasonic cleaning with deionized water to remove residual solution;

[0027] (6) Soak in anhydrous ethanol for later use to prevent oxidation.

[0028] Preferably, the substrate material is a material having semiconductor properties, high thermal conductivity, good chemical stability, high mechanical strength and hardness, such as silicon wafer, silicon nitride or gallium nitride.

[0029] Preferably, the concentration of the PS microsphere solution is 25 mg / mL, and the diameter of the PS microspheres is 400 nm.

[0030] Preferably, the PS microsphere solution is diluted with anhydrous ethanol. When the PS microsphere solution is diluted with anhydrous ethanol, it is ensured that the supernatant after centrifugation is mixed with anhydrous ethanol to allow a single layer of PS microspheres to spread on the liquid surface of the downcomer.

[0031] Preferably, the centrifugal speed is 3000-7000rpm. In order to solve the problem of impurities and PS microsphere aggregation in the solution, the present invention adds a centrifugal step after obtaining the PS microsphere ethanol solution, and finds that the centrifugal speed has a great influence on the microsphere content in the supernatant. At a speed of 3000-12000rpm, centrifuge for 10 minutes, take the supernatant, and analyze the surface electron microscopy image obtained by the liquid drop. It can be seen that the centrifugal speed should not be too high. At 11000rpm, the PS microsphere content in the supernatant is too small. At 3000-7000rpm, the number of PS microspheres retained in the supernatant is large, which can meet the requirements of removing impurities and agglomeration and retaining independent PS microspheres.

[0032] Preferably, in the step of obtaining the mixed solution after ultrasonication in ice water, the frequency of the ultrasonication is 40 kHz and the time of the ultrasonication is 5-10 min.

[0033] Preferably, pouring water until the silicon wafer is submerged comprises: pouring deionized water until the water level is 5 mm higher than the silicon wafer.

[0034] More preferably, the liquid-dropping funnel used in the present invention is made of glass as a whole, the funnel part is a column plus cone structure, the lower part of the cone is connected to a sharp-nosed conduit, and the connection between the column and the cone is fixedly connected with a honeycomb leak plate, which can realize the stable placement of the substrate material and the uniform drop of the liquid level, and the sharp-nosed conduit is provided with a piston. First, the PS microsphere solution is diluted 2 times with anhydrous ethanol, and then centrifuged at a speed of 3000-7000rpm, and the supernatant is mixed with anhydrous ethanol in a volume ratio of 1:1, and a mixed solution is obtained after ultrasonication in ice water. Anhydrous ethanol can be used as a spreading agent to spread the PS microspheres fully on the surface, effectively reducing the probability of overlap, and the high volatility of anhydrous ethanol is conducive to surface drying. The prepared solution is placed in ice water for ultrasonication to prevent the deposition and aggregation of the PS microspheres, and the ice water can prevent the temperature rise of the solution during the ultrasonication from causing the microsphere morphology to be destroyed. The ultrasonic frequency should not be too high to prevent the microspheres from being shattered.

[0035] Preferably, the liquid-dropping funnel of the present invention is provided with a piston and a flat-bottomed sieve hole. The flat-bottomed sieve hole can realize the stable placement of the silicon wafer sample and can also ensure that the liquid flow rate near the silicon wafer is consistent and stable; the piston can realize the control of the liquid drop speed to ensure that the liquid surface falls steadily at a uniform speed, so that the surface PS microsphere film (referring to the film formed by the PS microspheres being tightly and evenly arranged on the liquid surface) is not disturbed.

[0036] PS microspheres are insoluble in water. When the ethanol solution of PS microspheres is injected into deionized water, ethanol and water are miscible, and PS microspheres will float on the water surface. In this way, PS microspheres will form a thin film on the liquid surface, and cover the surface of the silicon wafer as the liquid surface falls. However, when placing the silicon wafer, it should be noted that the silicon wafer should be tilted at a certain angle. It should not be placed directly on the surface of the flat-bottomed sieve. Placing the silicon wafer directly parallel will block some holes, so that the liquid can only flow out from the unblocked holes near the silicon wafer during the liquid drop process, causing disturbances in the liquid flow direction near the silicon wafer, and ripples will appear in the liquid drop result. It is preferred that the tilt angle of the silicon wafer be 10-15° when placing it.

[0037] Preferably, during plasma etching, the oxygen flow rate is 0.2-0.6mL / s, and the etching time is 8-12min. The present invention uses plasma etching to regulate the size of PS microspheres. Plasma etching is a technology commonly used in micro-nano processing, which uses ion beams to induce chemical reactions and physical erosion on the surface of materials, thereby achieving precise etching of materials. In general, plasma etching is a complex process involving plasma physics and chemical reaction kinetics. By controlling the energy, flow rate and composition of the ion beam, high-precision etching of the surface of the material can be achieved, which has a wide range of applications in the field of micro-nano processing. The present invention uses plasma etching to etch PS microspheres, so that the diameter of the PS microspheres is reduced, and gaps appear between the microspheres. This step is a key step in template preparation and is the key to controllable nanowires. This process can achieve regulation of the size of the PS template, thereby affecting the distribution of nanowires. The present invention etches the surface of a silicon wafer with a single-layer PS microsphere template through a plasma cleaning machine at a certain oxygen flow rate (oxygen flow rate is 0.2-0.6 mL / s) for a period of time (etching time is 8-12 min) to obtain a single-layer PS microsphere template of different sizes. The longer the processing time, the greater the oxygen flow rate, the greater the change in the diameter of the PS microsphere, and the oxygen flow rate should not be too high. If the diameter of the single-layer PS microsphere is reduced too much, the PS microsphere will be deformed, affecting the micro-nano structure morphology. The single-layer PS microsphere template after plasma treatment realizes the control of the microsphere diameter, and then controls the spacing and diameter of the nanowires formed by subsequent etching. Secondly, theoretically, by changing the initial PS microsphere diameter, the center distance of the nanowires can be regulated after plasma etching, thereby expanding the nanowire size controllable range (the diameter of the PS microsphere affects the diameter of the nanowire. The surface nanowires prepared by PS microspheres with a diameter of 400nm must be less than 400nm, and the theoretical center distance between nanowires is also 400nm. Replacing with PS microspheres of other sizes can theoretically adjust the diameter range of the nanowires and also realize the regulation of the center distance).

[0038] Preferably, when etching is performed under water bath conditions, it is performed in an etching solution, which is a mixed solution of HF (hydrofluoric acid), H2O2 (hydrogen peroxide) and water, wherein the mass concentration of HF is 40%, the mass concentration of H2O2 is 30%, and the volume ratio of HF, H2O2 and deionized water is 5:1:15.

[0039] Preferably, the etching time in a water bath is 10-30 min, and the etching temperature in a water bath is 30-70° C.

[0040] Preferably, the etching time in a water bath is 20 min, and the etching temperature in a water bath is 70° C.

[0041] Preferably, the noble metal catalyst is silver, platinum or gold.

[0042] Compared with the prior art, the present invention has the following advantages and technical effects:

[0043] In order to solve the problem of stability of the pulling method in template preparation, the present invention designs a liquid drop method to replace the common pulling method to prepare a PS microsphere monolayer template, and designs a corresponding liquid drop funnel. At the same time, in terms of template regulation, a plasma etching method is used instead of a common reactive ion etching method. The plasma etching method is simple to operate, has low cost and a shorter cycle. The method of the present invention uses a liquid drop method to assist a plasma etching method to prepare a monolayer microsphere template and then control the distribution of a metal catalyst, thereby realizing the preparation of a nanowire structure on a silicon-based surface. In addition, it can also be extended to other new material surfaces such as silicon nitride, gallium nitride, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0045] Figure 1 It is a schematic structural diagram of the downcomer funnel used in the downcomer method of the present invention.

[0046] Figure 2 Schematic diagram of the experimental device of the liquid reduction method in the method of the present invention.

[0047] Figure 3 This is a SEM image of the surface obtained after precipitation of a solution prepared by centrifuging the supernatant and anhydrous ethanol in a volume ratio of 1:1 in Example 1.

[0048] Figure 4 These are SEM images of the silicon wafer surface after plasma etching of the single-layer PS microsphere template in Example 1 at different magnifications, where a is 2000 times, b is 5000 times, and c is 20000 times.

[0049] Figure 5 These are SEM images of the surface of the template with a single layer of PS microspheres after magnetron sputtering and water bath etching in Example 1 at different magnifications, a is 1000 times, b is 3000 times, and c is 4000 times.

[0050] Figure 6 These are SEM images of the spreading results of PS microspheres in the flow channel in Example 6 at different magnifications, where a and b are the liquid drop conditions in the flow channel, and c and d are partial enlarged images of a and b, respectively.

[0051] Figure 7 These are SEM images at different magnifications of the flow channel surface after plasma etching in Example 6.

[0052] Figure 8These are SEM images of the channel surface at different magnifications after magnetron sputtering and water bath etching in Example 6, where a is 1500 times and b is 6500 times. DETAILED DESCRIPTION

[0053] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0054] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0055] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0056] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0057] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0058] All raw materials used in the examples of the present invention are commercially available.

[0059] In the present invention, the base material is a material having semiconductor properties, high thermal conductivity, good chemical stability, high mechanical strength and hardness, such as a silicon wafer, silicon nitride or gallium nitride. The embodiments of the present invention are described with the base material being a silicon wafer and a microchannel heat sink (which is also a silicon material).

[0060] In the present invention, the noble metal catalyst is silver, platinum or gold. Plasma etching can be performed using the above noble metal catalysts. Taking all factors into consideration, silver is used as the noble metal catalyst in the embodiments of the present invention.

[0061] In the present invention, it should be noted that the diameter of the nanowire is not equal to the diameter of the PS microsphere after plasma treatment. This is because the magnetron sputtering process is not vertical sputtering, and the noble metal catalyst (such as Ag) is not directly deposited during the etching process. + ) will diffuse freely, and some areas that are not sputtered to Ag and not covered by PS microspheres will also be etched, so the diameter of the nanowires formed by etching is smaller than the diameter of the treated PS microspheres.

[0062] In the embodiment of the present invention, the microchannel heat sink is independently designed and outsourced, and is a silicon wafer of 18.14*16.14 mm in size, with a set of channels etched internally with a width of 300 μm, a length of 11.14 mm, and a depth of 300 μm.

[0063] The structural schematic diagram of the downcomer used in the method of the present invention is shown in Figure 1 The liquid-dropping funnel is made of glass as a whole. The funnel part is a column plus cone structure. The inner diameter of the column is 5 cm. A pointed tube is connected to the lower part of the cone. A honeycomb leak plate is fixedly connected to the connection between the column and the cone. The honeycomb leak plate can realize the stable placement of the base material and can realize the uniform drop of the liquid level. The pointed tube is equipped with a piston to adjust the liquid drop rate.

[0064] The schematic diagram of the experimental device of the liquid reduction method of the present invention is shown in Figure 2 .

[0065] The materials required in the examples and comparative examples of the present invention are shown in Table 1.

[0066] Table 1 Materials required for the preparation of micro-nanostructures by microsphere-assisted method

[0067]

[0068]

[0069] Note: In Table 1, “%” refers to mass percentage.

[0070] The technical solution of the present invention is further illustrated by the following embodiments.

[0071] Example 1

[0072] (1) Pretreatment of silicon wafers: Clean the silicon wafers as follows: (1) Ultrasonic treatment with acetone for 10 minutes to remove organic impurities on the surface; (2) Ultrasonic treatment with dilute hydrofluoric acid (HF with a mass concentration of 40% and H2O mixed in a volume ratio of 1:2) for 15 minutes to remove the native oxide layer on the surface of the silicon wafer; (3) Ultrasonic treatment with deionized water for 10 minutes to remove the residual solution; (4) Heating a mixed solution of hydrochloric acid and hydrogen peroxide (HCl with a mass concentration of 36%, H2O2 with a mass concentration of 30% and H2O mixed in a volume ratio of 1:1:5) in a 70°C water bath for 25 minutes; (5) Ultrasonic treatment with deionized water to remove the residual solution; (6) Soak in anhydrous ethanol for later use to prevent oxidation. After drying with nitrogen, the surface is treated with hydrophilicity, that is, plasma treatment is used for 1 minute to make the surface of the silicon wafer temporarily hydrophilic;

[0073] (2) A 25 mg / mL PS microsphere solution was diluted 2 times with anhydrous ethanol, centrifuged at 5000 rpm for 10 min, and then the supernatant was mixed with anhydrous ethanol at a volume ratio of 1:1 (which helps the PS microspheres spread). The mixture was sonicated at a low frequency (specifically 40 kHz) in ice water for 8 min to obtain a mixed solution for subsequent liquid drop experiments;

[0074] (3) A liquid-reducing funnel with a piston and a flat-bottomed sieve hole is fixed vertically on an iron frame, and the mixed liquid is sucked into a syringe. The syringe containing the mixed liquid is fixed vertically on the iron frame. The syringe is located above the liquid-reducing funnel, and the needle tip of the syringe is close to the inner wall of the liquid-reducing funnel. A beaker is provided below the liquid-reducing funnel for holding the solution dripping from the liquid-reducing funnel. The piston of the liquid-dropping funnel was closed, and the pretreated silicon wafer was placed in the liquid-dropping funnel with an inclination angle of 10°. Deionized water was poured in until the silicon wafer was submerged (the water surface was 5 mm higher than the surface of the silicon wafer); the piston of the syringe was pulled out to allow the PS microsphere solution to move downward under the action of gravity, so that the mixed solution could slide to the water surface along a fixed path, and the dripping speed of the mixed solution at the needle tip of the syringe was controlled so that continuous ripples could be formed on the water surface. After the mixed solution was dripped, it was allowed to stand to allow the PS microspheres to spread completely on the liquid surface. After the liquid surface was stable, the piston of the liquid-dropping funnel was opened to allow the solution to drip into the beaker, and the liquid surface was kept to drop without fluctuation until it was lower than the silicon wafer. The PS microspheres remained on the silicon wafer, and after standing for 3 minutes, they were dried in an oven to obtain a single-layer PS microsphere template. The SEM image of the surface of the solution prepared by centrifuging the supernatant and anhydrous ethanol in a volume ratio of 1:1 after liquid drop was shown in FIG. Figure 3 , it can be seen that the surface of PS microspheres is evenly spread, achieving a single layer of dense arrangement in a large area;

[0075] (4) Plasma etching was used to regulate the single-layer PS microsphere template: a silicon wafer with a single-layer PS microsphere template was placed in a plasma cleaning chamber and bombarded with pure oxygen in a vacuum environment for 10 min (i.e., the etching time was 10 min). The oxygen flow rate was 0.2 mL / s to achieve the etching effect. After etching, the diameter of the PS microspheres in the single-layer PS microsphere template was 270 nm. The SEM images of the silicon wafer surface at different magnifications after plasma etching of the single-layer PS microsphere template are shown in FIG. Figure 4 It can be seen that the PS microspheres are evenly distributed on the surface of the silicon wafer after plasma treatment. After magnification, it can be observed that the etched PS microspheres are proportionally reduced, maintaining the original spherical shape and with neat specifications.

[0076] (5) Then, a layer of silver (Ag) catalyst is sputtered in the gap of the single-layer PS microsphere template by magnetron sputtering (ensuring that the upper limit of the thickness of the catalyst does not exceed the radius of the PS microsphere after plasma treatment, and the thickness of the catalyst layer in this embodiment is 30 nm). Although the surface of the PS microsphere is covered with a silver layer after magnetron sputtering, its distribution is not affected. The sample after magnetron sputtering is placed in an etching solution (a mixed solution obtained by mixing HF, H2O2 and deionized water in a volume ratio of 5:1:15) and etched in a 70°C water bath for 20 minutes. After etching, it is soaked in dilute nitric acid (mass concentration of 65%) for 3 hours, then rinsed with deionized water, and dried with nitrogen to obtain a controllable nanowire composite microchannel. In this embodiment, the SEM images of the surface of the single-layer PS microsphere template after magnetron sputtering and water bath etching at different magnifications are shown as follows Figure 5 As shown, it can be seen that the nanowire structure is more obvious, there is less silver catalyst residue at the tip, and the nanowire structure can be clearly observed.

[0077] Example 2

[0078] The same as Example 1, except that the flow rate of oxygen in step (4) is 0.6 mL / s and the etching time is 8 min.

[0079] In this embodiment, the diameter of the PS microspheres in the single-layer PS microsphere template after etching is 140 nm.

[0080] Example 3

[0081] The same as Example 1, except that the flow rate of oxygen in step (4) is 0.6 mL / s and the etching time is 12 min.

[0082] In this embodiment, the diameter of the PS microspheres in the single-layer PS microsphere template after etching is 90 nm.

[0083] It can be seen from Examples 1 to 3 that after 8 minutes of plasma treatment with an oxygen flow of 0.6 mL / s, the diameter of the PS microspheres decreased from 400 nm to 140 nm, and after 12 minutes of treatment, it decreased from 400 nm to 90 nm. After 10 minutes of treatment at an oxygen flow rate of 0.2 mL / s, the diameter of the PS microspheres decreased from 400 nm to 270 nm. If the etching time continues to increase for more than 15 minutes, the PS microspheres will be deformed or even washed away.

[0084] From the above experimental results, it can be seen that plasma treatment should control two conditions: treatment time and oxygen flow rate. The longer the treatment time and the greater the oxygen flow rate, the greater the change in the diameter of the PS microspheres. The oxygen flow rate should not be too high. Excessive reduction in the diameter of the PS microspheres will cause the PS microspheres to deform and affect the micro-nanostructure morphology.

[0085] The PS microsphere template after plasma treatment realizes the control of the microsphere diameter, thereby controlling the spacing and diameter of the nanowires formed after subsequent etching. Secondly, theoretically, by changing the initial PS microsphere diameter, the center distance of the nanowires can be regulated after plasma etching treatment, thereby expanding the controllable range of nanowire size.

[0086] Example 4

[0087] (1) Pre-treating the silicon wafer: the same as in Example 1;

[0088] (2) A 25 mg / mL PS microsphere solution was diluted 2 times with anhydrous ethanol, centrifuged at 3000 rpm for 10 min, and then the supernatant was mixed with anhydrous ethanol at a volume ratio of 1:1. The mixture was ultrasonicated at a low frequency (40 kHz) in ice water for 5 min to obtain a mixed solution;

[0089] (3) A liquid-reducing funnel with a piston and a flat-bottomed sieve hole is fixed vertically on an iron frame, and the mixed liquid is sucked into a syringe. The syringe containing the mixed liquid is fixed vertically on the iron frame. The syringe is located above the liquid-reducing funnel, and the needle tip of the syringe is close to the inner wall of the liquid-reducing funnel. A beaker is provided below the liquid-reducing funnel for holding the solution dripping from the liquid-reducing funnel. Close the piston of the liquid-dropping funnel, put the pretreated silicon wafer into the liquid-dropping funnel, tilt the silicon wafer at an angle of 15°, pour in deionized water until the silicon wafer is submerged (the water surface is 5 mm higher than the silicon wafer surface); pull out the piston of the syringe to allow the PS microsphere solution to move downward under the action of gravity, so that the mixed solution can slide to the water surface along a fixed path, control the dripping speed of the mixed solution at the needle tip of the syringe, so that it can form continuous ripples on the water surface, and after the mixed solution is dripped, let it stand to allow the PS microspheres to spread completely on the liquid surface. After the liquid surface stabilizes, open the piston of the liquid-dropping funnel, let the solution drip into the beaker, and keep the liquid surface from fluctuating and falling until the liquid surface is lower than the silicon wafer. The PS microspheres remain on the silicon wafer, and after standing for 3 minutes, use an oven to dry to obtain a single-layer PS microsphere template. The surface of the PS microspheres is evenly spread, and a single-layer dense arrangement is achieved over a large area;

[0090] (4) Plasma etching was used to regulate the single-layer PS microsphere template: a silicon wafer with a single-layer PS microsphere template was placed in a plasma cleaning chamber and bombarded with pure oxygen in a vacuum environment for 10 min at a flow rate of 0.2 mL / s to achieve an etching effect;

[0091] (5) Then, a layer of Ag catalyst was sputtered in the gap of the single-layer PS microsphere template by magnetron sputtering. Although the surface of the PS microsphere was covered with the Ag layer after magnetron sputtering, its distribution was not affected. The sample after magnetron sputtering was placed in an etching solution (a mixed solution of HF, H2O2 and deionized water in a volume ratio of 5:1:15) and etched for 30 minutes in a 30°C water bath. After etching, it was soaked in dilute nitric acid (mass concentration of 65%) for 3 hours and then rinsed with deionized water and dried with nitrogen to obtain a controllable nanowire composite microfluidic channel. The nanowire structure can be clearly observed from the SEM image, and there is less residual silver catalyst at the tip.

[0092] Example 5

[0093] (1) Pre-treating the silicon wafer: the same as in Example 1;

[0094] (2) A 25 mg / mL PS microsphere solution was diluted 2 times with anhydrous ethanol, centrifuged at 7000 rpm for 10 min, and then the supernatant was mixed with anhydrous ethanol at a volume ratio of 1:1. The mixture was ultrasonicated at a low frequency (40 kHz) in ice water for 10 min to obtain a mixed solution;

[0095] (3) A liquid-reducing funnel with a piston and a flat-bottomed sieve hole is fixed vertically on an iron frame, and the mixed liquid is sucked into a syringe. The syringe containing the mixed liquid is fixed vertically on the iron frame. The syringe is located above the liquid-reducing funnel, and the needle tip of the syringe is close to the inner wall of the liquid-reducing funnel. A beaker is provided below the liquid-reducing funnel for holding the solution dripping from the liquid-reducing funnel. Close the piston of the liquid-dropping funnel, put the pretreated silicon wafer into the liquid-dropping funnel, tilt the silicon wafer at an angle of 12°, pour in deionized water until the silicon wafer is submerged (the water surface is 5 mm higher than the silicon wafer surface); pull out the piston of the syringe to allow the PS microsphere solution to move downward under the action of gravity, so that the mixed solution can slide to the water surface along a fixed path, and control the dripping speed of the mixed solution at the needle tip of the syringe so that it can form continuous ripples on the water surface. After the mixed solution is dripped, let it stand to allow the PS microspheres to spread completely on the liquid surface. After the liquid surface stabilizes, open the piston of the liquid-dropping funnel to allow the solution to drip into the beaker, and keep the liquid surface from fluctuating and falling until the liquid surface is lower than the silicon wafer. The PS microspheres remain on the silicon wafer, and after standing for 3 minutes, use an oven to dry to obtain a single-layer PS microsphere template. The surface of the PS microspheres is evenly spread, and a single-layer dense arrangement is achieved over a large area.

[0096] (4) Plasma etching was used to regulate the single-layer PS microsphere template: a silicon wafer with a single-layer PS microsphere template was placed in a plasma cleaning chamber and bombarded with pure oxygen in a vacuum environment for 10 min at a flow rate of 0.2 mL / s to achieve an etching effect;

[0097] (5) Then, a layer of Ag catalyst was sputtered in the gap of the single-layer PS microsphere template by magnetron sputtering. Although the surface of the PS microsphere was covered with the Ag layer after magnetron sputtering, its distribution was not affected. The sample after magnetron sputtering was placed in an etching solution (a mixed solution of HF, H2O2 and deionized water in a volume ratio of 5:1:15) and etched for 10 minutes in a 60°C water bath. After etching, it was soaked in dilute nitric acid (mass concentration of 65%) for 3 hours and then rinsed with deionized water and dried with nitrogen to obtain a controllable nanowire composite microfluidic channel. The nanowire structure can be clearly observed from the SEM image, and there is less residual silver catalyst at the tip.

[0098] Example 6

[0099] The same as Example 1, except that the silicon wafer is replaced with a microchannel heat sink. When the microchannel heat sink is placed in step (3), the flow channel therein is ensured to be an up-and-down structure. During the liquid drop method, the liquid level is allowed to drop along the flow channel to ensure that the bottom of the flow channel can contact the microsphere film formed on the liquid surface. The spreading results of the PS microspheres in the flow channel after step (3) at different magnifications are shown in FIG. Figure 6, it can be seen that the PS microspheres are indeed distributed inside the flow channel obtained in step (3), and some areas are spread over a large area, and a local monolayer is observed to be tightly arranged; after 10 minutes of plasma treatment in step (4), the diameter of the PS microspheres in the flow channel is reduced to 270nm, and the PS microsphere monolayer spacing is locally regulated inside the flow channel ( Figure 7 ); The surface structure of the flow channel at different magnifications after step (5) is shown Figure 8 , the existence of nanowire structure can be observed from inside the flow channel.

[0100] Comparative Example 1

[0101] The same as Example 1, except that in step (2), the 25 mg / mL PS microsphere solution was directly diluted 2 times with anhydrous ethanol, centrifuged at 5000 rpm for 10 min in a centrifuge, and the supernatant was sonicated at a low frequency (40 kHz) in ice water for 8 min before performing a liquid drop experiment.

[0102] Since anhydrous ethanol was not added to the supernatant in this comparative example, the PS microspheres were not fully spread, and there were cases of no spreading and multi-layer spreading, and the subsequent steps could not be carried out.

[0103] Comparative Example 2

[0104] The same as Example 1, except that step (2) is as follows: 25 mg / mL PS microsphere solution is diluted 3 times with anhydrous ethanol, centrifuged at 5000 rpm for 10 min in a centrifuge, the supernatant is mixed with anhydrous ethanol at a volume ratio of 1:1, and the mixed solution is obtained after low-frequency (40 kHz) ultrasonication in ice water for 8 min, and the subsequent liquid reduction experiment is carried out.

[0105] Since the concentration of PS microspheres in the supernatant obtained by centrifugation was low after dilution 3 times in this comparative example, the PS microspheres were spread more evenly after liquid precipitation and were distributed in a single layer, but there were many local blanks and the subsequent steps could not be carried out.

[0106] Comparative Example 3

[0107] The same as Example 1, except that step (2) is as follows: 25 mg / mL PS microsphere solution is diluted 5 times with anhydrous ethanol, centrifuged at 5000 rpm for 10 min in a centrifuge, the supernatant is mixed with anhydrous ethanol at a volume ratio of 1:1, and the mixed solution is obtained after low-frequency (40 kHz) ultrasonication in ice water for 8 min, and the subsequent liquid reduction experiment is carried out.

[0108] Since the concentration of PS microspheres in the supernatant obtained by centrifugation was too low after dilution by 5 times in this comparative example, the PS microspheres on the surface were loosely and disorderly distributed after liquid precipitation, and the subsequent steps could not be performed.

[0109] Comparative Example 4

[0110] Same as Example 1, except that the rotation speed during centrifugation in step (2) is 11000 rpm.

[0111] In this comparative example, the centrifugal speed was high, and the content of PS microspheres in the supernatant was too small to proceed to the subsequent steps.

[0112] Comparative Example 5

[0113] The same as Example 1, except that after centrifugation in step (2), the supernatant is mixed with anhydrous ethanol in a volume ratio of 1:2.

[0114] In this comparative example, a large amount of anhydrous ethanol was added after centrifugation, and the content of PS microspheres in the mixed solution was too small. The PS microspheres could not be fully spread on the liquid surface, and the subsequent steps could not be performed.

[0115] In summary, in the preparation method of the controllable nanowire composite microfluidic channel assisted by microsphere template etching of the present invention, in order to solve the problems of impurities and PS microsphere aggregation in the solution, a centrifugation step is added, and the centrifugation is carried out at a speed of 3000-12000 rpm for 10 minutes, and the supernatant is taken. From the surface electron microscope analysis obtained by the falling liquid, it can be seen that the centrifugal speed should not be too high. At 11000 rpm, the content of PS microspheres in the supernatant is too small. At 3000-7000 rpm, the number of PS microspheres retained in the supernatant is relatively large, which can meet the requirements of removing impurities and agglomerations and retaining independent PS microspheres. Therefore, the present invention preferably centrifuges at a speed of 3000-7000 rpm.

[0116] Comparison of the liquid reduction and spin coating of PS microsphere solutions under different dilution multiples (Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3), respectively diluted 5 times, 3 times, 2 times and centrifuged, after taking out the supernatant, anhydrous ethanol was added at a volume ratio of 1:1 to reduce the liquid. After 5 times dilution and centrifugation, the concentration of PS microsphere solution was too low, and after reducing the liquid, the surface PS microspheres were loosely and disorderly distributed; the PS microsphere concentration of the PS microsphere solution after 3 times dilution was high, but the spreading was uneven; the concentration of PS microspheres diluted 2 times was appropriate, and the surface spreading was relatively uniform, but there were still local non-spreading and multi-layer situations; in order to improve the local non-spreading and multi-layer situation after 2 times dilution, anhydrous ethanol was added again, and the PS microsphere solution was diluted 2 times, and after centrifugation, the supernatant was taken and mixed with anhydrous ethanol at a volume ratio of 1:1. From the SEM image, it can be seen that the surface of PS microspheres is evenly spread, and a single layer is tightly arranged in a large area.

[0117] In the preparation method of the controllable nanowire composite microchannel assisted by microsphere template etching of the present invention, two conditions, the treatment time and the oxygen flow rate, should be controlled during plasma etching. The longer the treatment time, the greater the oxygen flow rate, and the greater the change in the diameter of the PS microspheres. The oxygen flow rate should not be too high. Excessive reduction in the diameter of the PS microspheres will cause the PS microspheres to deform, affecting the morphology of the micro-nano structure.

[0118] The PS microsphere template after plasma treatment can control the diameter of the microspheres, and then control the spacing and diameter of the nanowires formed after subsequent etching. Secondly, by changing the initial PS microsphere diameter, the center distance of the nanowires can be regulated after plasma etching. At the same time, the oxygen flow rate and time of plasma treatment can control the diameter of the nanowires, thereby achieving controllable preparation.

[0119] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a controllable nanowire composite microfluidic channel by microsphere template-assisted etching, characterized in that: A single-layer polystyrene microsphere template is prepared by a liquid drop method, and the size of the single-layer polystyrene microsphere template is regulated by plasma etching. The controllable nanowire composite microchannel is obtained by magnetron sputtering and water bath etching.

2. The method for preparing a controllable nanowire composite microfluidic channel by microsphere template-assisted etching according to claim 1, characterized in that: The following steps are involved: Pre-treating the substrate material; The polystyrene microsphere solution was diluted, the supernatant was mixed with anhydrous ethanol after centrifugation, and the mixture was obtained after ultrasonication in ice water; The liquid-dropping funnel is fixed vertically on an iron frame, the mixed liquid is sucked into a syringe, and the syringe containing the mixed liquid is fixed vertically on the iron frame, the syringe is located above the liquid-dropping funnel, the needle tip of the syringe is close to the inner wall of the liquid-dropping funnel, and a container is provided below the liquid-dropping funnel, the container is used to hold the solution dripping from the liquid-dropping funnel; The piston of the liquid-dropping funnel is closed, a silicon wafer is placed in the liquid-dropping funnel, and water is poured in until the silicon wafer is submerged; the piston of the syringe is pulled out to allow the polystyrene microsphere solution to move downward under the action of gravity, so that the mixed liquid can slide toward the water surface along a fixed path, and the dripping speed of the mixed liquid at the needle tip of the syringe is controlled so that continuous ripples can be formed on the water surface; after the mixed liquid is dripped, the liquid is allowed to stand to allow the polystyrene microspheres to spread completely on the liquid surface; after the liquid surface is stable, the piston of the liquid-dropping funnel is opened to allow the solution in the liquid-dropping funnel to drip into the container, and the liquid surface is kept to drop without fluctuation until the liquid surface is lower than the silicon wafer, and the polystyrene microspheres remain on the silicon wafer; after the liquid is allowed to stand, the mixture is dried to obtain a single-layer polystyrene microsphere template; The single-layer polystyrene microsphere template is etched by plasma etching, and then a layer of noble metal catalyst is sputtered at the gaps of the polystyrene microsphere template by magnetron sputtering, and etching is performed under water bath conditions to obtain the controllable nanowire composite microchannel.

3. The method for preparing a controllable nanowire composite microfluidic channel by microsphere template-assisted etching according to claim 2, characterized in that: The method for pre-treating the base material comprises the following steps: cleaning the base material, drying it with nitrogen and then performing surface hydrophilic treatment.

4. The method for preparing a controllable nanowire composite microchannel by microsphere template-assisted etching according to claim 2, characterized in that: The polystyrene microsphere solution is diluted with anhydrous ethanol.

5. The method for preparing a controllable nanowire composite microchannel by microsphere template-assisted etching according to claim 2, characterized in that: The centrifugal speed is 3000-7000 rpm.

6. The method for preparing a controllable nanowire composite microfluidic channel by microsphere template-assisted etching according to claim 2, characterized in that: The frequency of the ultrasound is 20-40 kHz.

7. The method for preparing a controllable nanowire composite microfluidic channel by microsphere template-assisted etching according to claim 2, characterized in that: During plasma etching, the oxygen flow rate is 0.2-0.6 mL / s, and the etching time is 8-12 min.

8. The method for preparing a controllable nanowire composite microfluidic channel by microsphere template-assisted etching according to claim 2, characterized in that: When etching is performed under water bath conditions, it is performed in an etching solution, and the etching solution is a mixed solution of HF, H2O2 and water.

9. The method for preparing a controllable nanowire composite microfluidic channel by microsphere template-assisted etching according to claim 2, characterized in that: The etching time under water bath conditions is 10-30 minutes, and the etching temperature under water bath conditions is 30-70°C.

10. The method for preparing a controllable nanowire composite microfluidic channel by microsphere template-assisted etching according to claim 9, characterized in that: The etching time under water bath conditions is 20 min, and the etching temperature under water bath conditions is 70°C.

Citation Information

Patent Citations

  • Large-area single-layer compact nano-microsphere film assembly method and device, and use method of device

    CN106115613A

  • Micro-nano fluidic chip based on nanometer gap between nanometer structures and preparation method thereof

    CN108097338A

  • SERS substrate with microscopic ordered nanostructures and preparation method

    CN113125406A

  • Gallium nitride nanowire array and processing method thereof

    CN115692189A

  • Manufacturing method of micro-fluidic chip combined with SERS (Surface Enhanced Raman Scattering) substrate and used for capturing and analyzing CTCs (CCTCs)

    CN116902906A