Porous carbon nitride, preparation method and application thereof, self-energized photoelectrochemical sensor and application of self-energized photoelectrochemical sensor

Porous carbon nitride rich in pore structures was prepared by gradient calcining method and used for self-energized photoelectrochemical sensors. The problems of detection height limit and poor photocatalytic performance in the prior art are solved, and the ability to efficiently detect Pb2+ in water is achieved.

CN119079941APending Publication Date: 2024-12-06NORTHEAST GASOLINEEUM UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411187556.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When detecting heavy metal ion Pb2+ in water, existing electrochemical sensors have problems such as detecting height limit, requiring a three-electrode system and relying on external power supply, and the photocatalytic performance of the original bulk carbon nitride is poor.

Method used

Porous carbon nitride is prepared by gradient roasting method, and porous carbon nitride is formed by mixing and reaction of melamine, acidic reagents and ethylene glycol as the electrode material for self-energized photoelectrochemical sensors to improve photocatalytic performance.

Benefits of technology

A self-energy photoelectrochemical sensor with low detection limit and high electrochemical performance response is realized, which can efficiently detect Pb2+ in water, and improve the absorption range and electron hole separation rate through the porous structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079941A_ABST
    Figure CN119079941A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of heavy metal ion detection, and particularly relates to porous carbon nitride, a preparation method and application thereof, a self-energized photoelectrochemical sensor and application thereof. The invention provides a preparation method of porous carbon nitride, which comprises the following steps: mixing melamine, an acidic reagent, ethylene glycol and water to obtain a pretreated precursor; and carrying out gradient roasting on the pretreated precursor to obtain the porous carbon nitride. The porous carbon nitride prepared by the method disclosed by the invention has a relatively large specific surface area and a relatively large light absorption range, a smaller band gap and a higher photo-induced electron and hole separation rate, is applied to self-energized electrochemical sensing detection of Pb < 2 + > in water, and has the characteristics of relatively low detection limit and relatively high electrochemical performance response.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of heavy metal ion detection, and specifically relates to a porous carbon nitride and a preparation method and application thereof, a self-powered photoelectrochemical sensor and application thereof. Background Art

[0002] Heavy metal ions Pb in water 2+ Due to its toxicity, electrochemical sensing has been widely used in recent years to detect heavy metal ions in water. However, it has the disadvantages of requiring a power supply, high detection limit, and the need to involve three electrodes (working electrode, auxiliary electrode, and reference electrode). Compared with traditional electrochemical sensors, self-powered electrochemical sensors have many potential advantages, such as low detection limit, two-electrode system, and energy supply. The traditional catalytic material used in self-powered electrochemical sensors is mainly semiconductor carbon nitride, but the original bulk carbon nitride still has poor photocatalytic performance due to the high recombination rate of charge carriers and weak visible light absorption. Summary of the invention

[0003] The purpose of the present invention is to provide a porous carbon nitride and a preparation method and application thereof, a self-powered photoelectrochemical sensor and application thereof. The porous carbon nitride obtained by the method provided by the present invention is applied to a self-powered electrochemical sensor and has excellent photocatalytic performance.

[0004] In order to achieve the above object, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing porous carbon nitride, comprising the following steps:

[0006] Mixing melamine, an acidic reagent, ethylene glycol and water to obtain a pretreatment precursor;

[0007] The pretreated precursor is subjected to gradient calcination to obtain the porous carbon nitride.

[0008] Preferably, the mass ratio of melamine to water is 3:10-15;

[0009] The acidic reagent includes hydrochloric acid or acetic acid, and the concentration of the acidic reagent is 8 to 12 mol·L -1 , the volume ratio of the acidic reagent to ethylene glycol is 0.5-1:1-1.5;

[0010] The volume ratio of the acidic reagent to water is 1:2-5.

[0011] Preferably, the mixing comprises:

[0012] Ultrasonic dispersion of melamine in water to obtain a mixed solution, and then adding an acidic reagent and ethylene glycol to the mixed solution for stirring;

[0013] The ultrasonic dispersion time is 0.5 to 1 hour, and the temperature is room temperature; the stirring time is 1 to 3 hours.

[0014] Preferably, the procedure of the gradient calcination is:

[0015] Performing a first heating from room temperature to a first temperature at a first heating rate;

[0016] The second temperature is raised from the first temperature to the second temperature at a second temperature rising rate, and the temperature is kept constant.

[0017] Preferably, the first heating rate is 5°C / min, the first temperature is 250-300°C, and the first heating time is 45-55min;

[0018] The second heating rate is 10° C. / min, the second temperature is 550-600° C., the second heating time is 30-35 min, and the insulation time is 2-4 h.

[0019] The present invention also provides porous carbon nitride prepared by the preparation method described in the above technical solution, wherein the specific surface area of ​​the porous carbon nitride is 10 to 46 m 2 / g.

[0020] The present invention also provides the use of the porous carbon nitride described in the above technical solution as an electrode material in self-powered photoelectrochemical sensing.

[0021] The present invention also provides a self-powered photoelectrochemical sensor, comprising a photoanode, a cathode and an electrolyte, wherein the electrode material on the photoanode is the porous carbon nitride described in the above technical solution.

[0022] Preferably, the cathode comprises carbon paper and a cathode material loaded on the carbon paper; the cathode material comprises iron phthalocyanine;

[0023] The electrolyte is a nitric acid solution.

[0024] The present invention also provides the self-powered photoelectrochemical sensor described in the above technical solution for detecting Pb 2+ Application in.

[0025] The present invention provides a method for preparing porous carbon nitride, comprising the following steps: mixing melamine, an acidic reagent, ethylene glycol and water to obtain a pretreated precursor; gradient calcining the pretreated precursor to obtain the porous carbon nitride. In the present invention, hydrogen bonds are formed between ethylene glycol and melamine molecules, which hinder the thermal polymerization of some amino groups with other amino groups, thereby facilitating the formation of a pore structure. At the same time, by reacting the acidic reagent with melamine, part of the melamine is converted into cyanuric acid. During calcination, cyanuric acid cannot polymerize with melamine, further promoting the formation of a pore structure. The present invention adopts the above-mentioned dual pore-making mechanism to make the obtained carbon nitride more porous. The porous carbon nitride prepared by the present invention has a large specific surface area and light absorption range, a smaller band gap, and a faster separation rate of photogenerated electrons and holes, and is applied to self-powered electrochemical sensing to detect heavy metal ions Pb in water. 2+ , with the characteristics of low detection limit and high electrochemical performance response.

[0026] The present invention also provides a self-powered photoelectrochemical sensor, comprising a photoanode, a cathode and an electrolyte, wherein the electrode material on the photoanode is the porous carbon nitride described in the above technical solution. The self-powered photoelectrochemical sensor provided by the present invention can detect Pb in water. 2+ , and the detection limit is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A schematic diagram of the structure of the porous carbon nitride obtained by the present invention;

[0028] Figure 2 The SEM images of the carbon nitride materials of Example 1 and Comparative Examples 1 to 3;

[0029] Figure 3 The XRD patterns of the carbon nitride materials of Example 1 and Comparative Examples 1 to 3;

[0030] Figure 4 The BET diagrams of the carbon nitride materials of Example 1 and Comparative Examples 1 to 3;

[0031] Figure 5 The self-powered electrochemical sensor Pb obtained in Comparative Example 1 2+ Detection performance;

[0032] Figure 6 The self-powered electrochemical sensor Pb obtained in Example 1 2+ Detection performance;

[0033] Figure 7 Schematic diagram of the process of preparing porous carbon nitride in Example 1 and Comparative Examples 1-3. DETAILED DESCRIPTION

[0034] The present invention provides a method for preparing porous carbon nitride, comprising the following steps:

[0035] Mixing melamine, an acidic reagent, ethylene glycol and water to obtain a pretreatment precursor;

[0036] The pretreated precursor is subjected to gradient calcination to obtain the porous carbon nitride.

[0037] The present invention mixes melamine, an acidic reagent, ethylene glycol and water to obtain a pretreatment precursor.

[0038] In the present invention, the water is preferably distilled water. In the present invention, the mass ratio of melamine to water is preferably 3:10-15. In the present invention, the acidic reagent preferably includes hydrochloric acid or acetic acid; the concentration of the acidic reagent is preferably 8-12 mol·L -1 The volume ratio of the acidic reagent to ethylene glycol is preferably 0.5-1:1-1.5, and more preferably 1:1; the volume ratio of the acidic reagent to water is preferably 1:2-5.

[0039] In the present invention, the mixing preferably comprises: ultrasonically dispersing melamine in water to obtain a mixed solution, and then adding an acidic reagent and ethylene glycol to the mixed solution for stirring. In the present invention, the ultrasonic dispersion time is preferably 0.5 to 1 hour, the temperature is preferably room temperature; the stirring time is preferably 1 to 3 hours.

[0040] After the mixing, the present invention also preferably includes centrifuging, washing and drying the obtained mixed system. The centrifugation, washing and drying processes of the present invention are not particularly limited and can be performed by methods well known to those skilled in the art.

[0041] After obtaining the pretreated precursor, the present invention performs gradient calcination on the pretreated precursor to obtain the porous carbon nitride.

[0042] In the present invention, the procedure of the gradient roasting is preferably:

[0043] Performing a first heating from room temperature to a first temperature at a first heating rate;

[0044] The second temperature is raised from the first temperature to the second temperature at a second temperature rising rate, and the temperature is kept constant.

[0045] In the present invention, the first heating rate is preferably 5°C / min, the first temperature is preferably 250-300°C, and the first heating time is preferably 45-55min; the second heating rate is preferably 10°C / min, the second temperature is preferably 550-600°C, the second heating time is preferably 30-35min, and the insulation time is preferably 2-4h.

[0046] After the gradient calcination, the present invention also preferably includes naturally cooling the obtained material to room temperature.

[0047] The present invention also provides porous carbon nitride prepared by the preparation method described in the above technical solution, wherein the specific surface area of ​​the porous carbon nitride is 10 to 46 m 2 / g.

[0048] The present invention also provides the use of the porous carbon nitride described in the above technical solution as an electrode material in self-powered photoelectrochemical sensing. The porous carbon nitride obtained by the present invention detects heavy metal ions Pb 2+ When the surface area is large, the amount of adsorbed heavy metal ions is greatly increased, making the valence band of the porous carbon nitride more positive during the experiment, making the oxidation ability of the holes stronger, the electrochemical performance response higher, and the detection limit lower.

[0049] The present invention also provides a self-powered photoelectrochemical sensor, comprising a photoanode, a cathode and an electrolyte, wherein the electrode material on the photoanode is the porous carbon nitride described in the above technical solution.

[0050] In the present invention, the photoanode preferably includes a catalyst support and an electrode material located on the surface of the catalyst support; the catalyst support is preferably a nickel mesh; the electrode material is the porous carbon nitride described in the above technical solution; the content of the electrode material on the photoanode is preferably 10 to 15 mg / cm 2 ; The size of the photoanode is preferably 1cm*1cm~2cm*2cm.

[0051] In the present invention, the method for preparing the photoanode preferably comprises:

[0052] The electrode material, anhydrous ethanol and Nafion D520 solution are ultrasonically mixed to obtain a slurry;

[0053] The slurry is coated on a catalyst support and dried to obtain the photoanode.

[0054] In the present invention, the mass concentration of the Nafion D520 solution is preferably 5%. In the present invention, the amount ratio of the electrode material, anhydrous ethanol and Nafion D520 solution is preferably 10-15 mg: 260-300 μL: 40-50 μL. In the present invention, the ultrasonic mixing time is preferably 30-60 min. The present invention has no special limitation on the coating process, and the process known to those skilled in the art can be adopted. In the present invention, the drying time is preferably 6-12 h.

[0055] In the present invention, the cathode preferably comprises carbon paper and a cathode material supported on the carbon paper, and the cathode material preferably comprises iron phthalocyanine. In the present invention, the content of the cathode material on the cathode is preferably 6 to 10 mg / cm 2 In the present invention, the size of the cathode is preferably 1 cm*1 cm to 2 cm*2 cm.

[0056] In the present invention, the method for preparing the cathode preferably comprises:

[0057] The cathode material, anhydrous ethanol and Nafion D520 solution are ultrasonically mixed to obtain a slurry;

[0058] The slurry is coated on carbon paper and dried to obtain the cathode.

[0059] In the present invention, the mass concentration of the Nafion D520 solution is preferably 5%. In the present invention, the dosage ratio of the cathode material, anhydrous ethanol and Nafion D520 solution is preferably 6-10 mg: 260-300 μL: 40-50 μL. In the present invention, the ultrasonic mixing time is preferably 30-60 min. The present invention has no special limitation on the coating process, and the process known to those skilled in the art can be adopted. In the present invention, the drying time is preferably 6-12 h.

[0060] In the present invention, the electrolyte is preferably a nitric acid solution. In the present invention, the concentration of the electrolyte is preferably 0.05 to 0.2 mol / L.

[0061] The present invention has no special limitation on the construction method of the self-powered electrochemical sensor, and any method known to those skilled in the art may be adopted.

[0062] The present invention also provides the self-powered photoelectrochemical sensor described in the above technical solution for detecting Pb 2+ Application in.

[0063] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.

[0064] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0065] Example 1

[0066] Melamine was dissolved in distilled water at room temperature and ultrasonicated for 0.5 h, wherein the mass ratio of melamine to distilled water was 3:10; then hydrochloric acid (concentration of 12 mol·L) was added in a volume ratio of 1:1. -1 ) and ethylene glycol solution, wherein the volume ratio of hydrochloric acid to distilled water is 1:2, and the mixture is stirred for 2 hours; the stirred mixture is centrifuged, washed and dried to obtain a white powder, which is a pretreatment precursor;

[0067] The white powder was subjected to gradient calcination, and the gradient calcination procedure was as follows: the temperature was increased from 25°C to 250°C at a heating rate of 5°C / min for 45 min; then the temperature was increased from 250°C to 550°C at a heating rate of 10°C / min for 30 min, and then the temperature was kept at 550°C for 2 h, and naturally cooled to room temperature to obtain the porous carbon nitride (schematic diagram of the structure is shown in FIG. Figure 1 shown);

[0068] The nickel mesh was cut into a size of 1cm*1cm, 10mg of the porous carbon nitride obtained above was weighed and placed in a vial, 260μL of anhydrous ethanol and 40μL of a 5% mass concentration of Nafion D520 solution were added, and ultrasonication was performed for 30min until it was completely dispersed to obtain a slurry. The slurry was coated on the nickel mesh and placed in a vacuum drying oven for 12h to obtain a photoanode (wherein the content of the electrode material on the photoanode was 10mg / cm 2 ).

[0069] Preparation of cathode: Cut carbon paper into 1cm*1cm size, weigh 7mg of iron phthalocyanine (Fe II Pc) was placed in a vial, 260 μL of anhydrous ethanol and 40 μL of a 5% Nafion D520 solution were added, and ultrasonic treatment was performed for 30 min. After the dispersion was complete, the mixture was evenly coated on carbon paper, and then placed in a vacuum drying oven for 12 h to obtain a cathode (wherein the content of the electrode material on the cathode was 7 mg / cm 2 ).

[0070] Step 4: Using HNO3 (0.1M) as the electrolyte, the photoanode and cathode obtained above were constructed into a self-powered electrochemical sensor.

[0071] Comparative Example 1

[0072] The original bulk carbon nitride calcined with melamine as raw material was used as a blank control to construct a self-powered electrochemical sensor.

[0073] Comparative Example 2

[0074] The porous carbon nitride prepared in the manner of Example 1 is different in that the volume ratio of 1:1 hydrochloric acid (concentration of 12 mol·L -1) and ethylene glycol solution, replace them with 2 times of hydrochloric acid, that is, the volume ratio of hydrochloric acid to water is 1:1, and the stirring mixing time is 2h.

[0075] The porous carbon nitride obtained above was constructed into a self-powered electrochemical sensor in the manner of Example 1.

[0076] Comparative Example 3

[0077] The porous carbon nitride prepared in the manner of Example 1 is different in that the volume ratio of 1:1 hydrochloric acid (concentration of 12 mol·L -1 ) and ethylene glycol solution, replace them with 2 times the ethylene glycol, that is, the volume ratio of ethylene glycol to water is 1:1, and the stirring mixing time is 2h.

[0078] The porous carbon nitride obtained above was constructed into a self-powered electrochemical sensor in the manner of Example 1.

[0079] The schematic diagram of the process of preparing porous carbon nitride in Example 1 and Comparative Examples 1 to 3 is as follows Figure 7 shown.

[0080] Performance Testing

[0081] Test Example 1

[0082] The carbon nitride materials of Example 1 and Comparative Examples 1 to 3 were examined by scanning electron microscopy, and the obtained SEM images are as follows: Figure 2 As shown, Figure 2 (a) is CN (original bulk carbon nitride, i.e., Comparative Example 1), (b) is E-CN (EG-g-C3N4, i.e., Comparative Example 3), (c) is H-CN (HCl-g-C3N4, i.e., Comparative Example 2), and (d) is HE-CN (EG+HCl-g-C3N4, i.e., Example 1); Figure 2 As can be seen from (a), CN is a bulk phase structure. Figure 2 (b) and Figure 2 (c) are samples obtained by treating melamine with ethylene glycol and hydrochloric acid and then calcining. The figure clearly shows the successful construction of the pore structure. The pore structures of different geometric sizes indicate that the pore-forming mechanisms of the two are different. The present invention modifies melamine with hydrochloric acid and ethylene glycol at the same time, wherein hydrogen bonds are formed between EG and melamine molecules, hindering the thermal polymerization of some amino groups with other amino groups, thereby forming a pore structure. HCl reacts with melamine, and part of the melamine is converted into cyanuric acid. At high calcination temperatures, cyanuric acid cannot polymerize with melamine, forming a pore structure. Compared with E-CN and H-CN materials, HE-CN materials have more abundant pores, which may be due to the simultaneous existence of the two pore-forming mechanisms, such as Figure 2 as shown in (d).

[0083] Figure 3 The XRD patterns of the carbon nitride materials of Example 1 and Comparative Examples 1 to 3 are shown in FIG. 1 , wherein HE-CN is Example 1, H-CN is Comparative Example 2, E-CN is Comparative Example 3, and CN is Comparative Example 1. Figure 3 It can be seen that CN shows a typical (002) interlayer stacking peak at 27.5° and a (100) peak at 12.9°. Compared with bulk CN, E-CN and H-CN have a weaker (002) peak diffraction intensity due to the reduced content of lamellar morphology in the porous microstructure. HE-CN has a weaker (002) peak diffraction intensity than E-CN and H-CN because it has more abundant micropores.

[0084] Figure 4 The BET diagrams of the carbon nitride materials of Example 1 and Comparative Examples 1 to 3, wherein the left diagram is the BJH pore size distribution curve and the right diagram is the adsorption isotherm; Figure 4 It can be seen that CN, E-CN, H-CN and HE-CN all have type IV isotherms with H3-type hysteresis loops, and the specific surface areas in the figure can prove that they all have porous microstructures. The BJH pore size distribution curve shows that the strong and broad pore size distribution peaks of CN, E-CN, H-CN and HE-CN in the range of 20 to 100 nm originate from the formation of porous microstructures. The surface areas of E-CN, H-CN and HE-CN are larger than those of bulk CN. Because their porous microstructures lead to more exposed geometric surfaces compared to the latter's bulk bulk structure, the BET surface area of ​​HE-CN is larger than that of the other three samples due to its richer porous microstructure.

[0085] Test Example 2

[0086] The self-powered electrochemical sensors obtained in Example 1 and Comparative Example 1 were added with different concentrations of Pb 2+ , study the detection performance of heavy metal ions;

[0087] in Figure 5 The self-powered electrochemical sensor Pb obtained in Comparative Example 1 2+ The detection performance, Figure 6 The self-powered electrochemical sensor Pb obtained in Example 1 2+ detection performance.

[0088] according to Figure 5 and Figure 6 It can be seen that when the same concentration of Pb is added 2+ When the electrochemical response of the self-powered sensor improved in the present application is higher than that of CN (i.e., comparative example 1), it is proved that the sensor of the present application has a higher output potential Eocpt and better detection performance.

[0089] In heavy metal detection, it involves drawing a standard curve, where R 2 It is an important statistical indicator used to evaluate the fit of experimental data. 2 The value indicates a high correlation between the experimental data and the fitting curve, which increases the reliability and accuracy of the measurement results. 2 The closer the value is to 1, the higher the fitting degree between the experimental data and the standard curve is, and the better the detection performance is, thus ensuring the reliability and accuracy of the measurement results. Figure 5 and Figure 6 It can be seen that the self-powered electrochemical sensor of the present application has a higher R 2 , Pb 2+ The detection performance is better.

[0090] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing porous carbon nitride, characterized in that: The following steps are involved: Mixing melamine, an acidic reagent, ethylene glycol and water to obtain a pretreatment precursor; The pretreated precursor is subjected to gradient calcination to obtain the porous carbon nitride.

2. The preparation method according to claim 1, characterized in that: The mass ratio of melamine to water is 3:10-15; The acidic reagent includes hydrochloric acid or acetic acid, and the concentration of the acidic reagent is 8 to 12 mol·L -1 , the volume ratio of the acidic reagent to ethylene glycol is 0.5-1:1-1.5; The volume ratio of the acidic reagent to water is 1:2-5.

3. The preparation method according to claim 1, characterized in that: The mixing includes: Ultrasonic dispersion of melamine in water to obtain a mixed solution, and then adding an acidic reagent and ethylene glycol to the mixed solution for stirring; The ultrasonic dispersion time is 0.5 to 1 hour, and the temperature is room temperature; the stirring time is 1 to 3 hours.

4. The preparation method according to claim 1, characterized in that: The procedure of the gradient roasting is: Performing a first heating from room temperature to a first temperature at a first heating rate; The second temperature is raised from the first temperature to the second temperature at a second temperature rising rate, and the temperature is kept constant.

5. The preparation method according to claim 4, characterized in that: The first heating rate is 5°C / min, the first temperature is 250-300°C, and the first heating time is 45-55min; The second heating rate is 10° C. / min, the second temperature is 550-600° C., the second heating time is 30-35 min, and the insulation time is 2-4 h.

6. The porous carbon nitride prepared by the preparation method according to any one of claims 1 to 5, characterized in that: The specific surface area of ​​the porous carbon nitride is 10 to 46 m 2 / g.

7. Use of the porous carbon nitride according to claim 6 as an electrode material in self-powered photoelectrochemical sensing.

8. A self-powered photoelectrochemical sensor comprising a photoanode, a cathode and an electrolyte, characterized in that: The electrode material on the photoanode is the porous carbon nitride as claimed in claim 6.

9. The self-powered photoelectrochemical sensor according to claim 8, characterized in that: The cathode comprises carbon paper and a cathode material loaded on the carbon paper; the cathode material comprises iron phthalocyanine; The electrolyte is a nitric acid solution.

10. The self-powered photoelectrochemical sensor according to claim 8 or 9 is used to detect Pb 2+ Application in.

Citation Information

Patent Citations

  • Preparation method of multi-stage structure melamine with high specific surface area

    CN109608410A

  • Preparation method and application of super-long hollow chain spherical carbon nitride photocatalytic material

    CN110813375A

  • Synthesis and application of alkaline earth metal coordination modified bubbling porous g-C3N4 nanosheet photocatalyst

    CN115155634A

  • Mesoporous carbon nitride used as lithium ion battery negative electrode material and preparation method thereof

    CN115626611A

  • Preparation of nitrogen rich three dimensional mesoporous carbon nitride and its sensing and photocatalytic properties

    WO2018033829A1