Preparation method of metal nanoparticle-loaded composite carbon aerogel photo-thermal evaporator
The loaded metal nanoparticles are prepared by bacterial cellulose and phenolic-based composite carbon aerogel, and the integration of the photothermal layer and the thermal insulation layer is achieved, solving the problems of high energy consumption and brittleness of aerogels in traditional seawater desalination methods. Improves the efficiency of seawater desalination and the photothermal conversion performance.
Patent Information
- Application Number
- CN202411179696.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional seawater desalination methods such as membrane distillation and electroosmosis have problems of high energy consumption and high cost, and a single phenolic carbon aerogel is highly brittle during photothermal evaporation, making it difficult to achieve efficient photothermal conversion and thermal insulation effects. .
Using bacterial cellulose and phenolic group composite three-dimensional carbon aerogel, a composite carbon aerogel loaded with metal nanoparticles is prepared through sol gel, freeze-drying and high-temperature carbonization processes, realizing the integration of the photothermal layer and the thermal insulation layer, and enhancing the Skeleton strength and doped with metal nanoparticles to improve photothermal conversion capability.
The photothermal evaporator with high water evaporation efficiency has good photothermal conversion performance and low thermal conductivity, which solves the problems of brittleness of aerogels in a single phenolic carbon and high energy consumption of traditional seawater desalination methods.
Smart Images

Figure CN119079972A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a preparation method of a bacterial cellulose and phenolic-based composite three-dimensional carbon aerogel photothermal evaporator with high water evaporation efficiency, which can prepare an integral three-dimensional interface water evaporation device with good photothermal conversion performance, and belongs to the field of energy conversion and clean energy. Background Art
[0002] Water is essential for life and health. Although approximately two-thirds of the Earth's surface is covered by water, 97% of it is seawater and cannot be drunk directly. One effective way to address the scarcity of freshwater resources is to desalinate seawater. Traditional desalination methods include membrane distillation and electroosmosis, but these methods suffer from high energy consumption and costs. In recent years, the use of solar thermal evaporators to absorb solar energy and drive the evaporation of seawater to generate freshwater has been proposed.
[0003] Common photothermal evaporators are generally composed of two layers. The upper layer is the photothermal layer, which absorbs sunlight and converts it into heat, requiring high photothermal conversion capacity. The lower layer is the thermal insulation and water transfer layer, which prevents heat loss caused by direct transfer of heat energy to seawater and requires low thermal conductivity and good water transfer capacity. Carbon aerogel can be used as a photothermal evaporator, both as a photothermal layer for photothermal conversion and as an evaporator itself, leveraging its low thermal conductivity.
[0004] Single phenolic carbon aerogel is very brittle and easily breaks during photothermal evaporation. After being compounded with bacterial cellulose, the bacterial cellulose can enhance the skeleton strength of the carbon aerogel. Summary of the Invention
[0005] The purpose of the present invention is to develop a method for preparing composite carbon aerogel loaded with metal nanoparticles for photothermal evaporation.
[0006] The technical solution of the present invention:
[0007] A method for preparing a composite carbon aerogel loaded with metal nanoparticles for photothermal evaporation comprises dissolving bacterial cellulose, resorcinol, formaldehyde and metal acetate in deionized water in a certain proportion and mixing them evenly. The composite carbon aerogel is obtained through sol-gel, freeze-drying and high-temperature carbonization processes and is used for photothermal water evaporation.
[0008] The specific steps are as follows:
[0009] In step (1), bacterial cellulose is oxidized with TEMPO and sodium bromide, and then collected by centrifugal washing and redispersed in deionized water to form a bacterial cellulose dispersion.
[0010] Step (2) Weigh a certain amount of resorcinol and metal acetate, add them to the bacterial cellulose suspension, stir evenly, adjust the pH of the solution, then add an appropriate amount of formaldehyde solution, and stir to obtain a uniform solution.
[0011] Step (3) placing the mixed solution obtained in step (2) in a sealed container, and performing gelation and aging treatment in a blast oven to obtain a composite hydrogel.
[0012] Step (4) placing the composite hydrogel obtained in step (3) into a vacuum freeze dryer and freeze-drying for 48 hours to obtain a composite aerogel.
[0013] Step (5) The composite aerogel obtained in step (4) is subjected to high-temperature carbonization treatment under nitrogen atmosphere protection to obtain bacterial cellulose / phenolic composite carbon aerogel loaded with metal nanoparticles.
[0014] Preferably, in step (1), the mass ratio of TEMPO: sodium bromide: bacterial cellulose is 0.0016:0.1:1; and the concentration of the bacterial cellulose suspension is 0.2-0.8 mg / mL.
[0015] Preferably, the precursor concentration (resorcinol + formaldehyde) in step (2) is generally selected to be 8-12%; the molar ratio of resorcinol to formaldehyde is fixed at 1:2; the metal salt is generally selected from nickel acetate, zinc acetate, cobalt acetate, etc.; the molar ratio of metal salt to resorcinol is generally 1:50-1:20; and the pH of the precursor solution is selected to be in the range of 6.4-6.7.
[0016] Preferably, in step (3), the oven temperature is 40-80° C., the gel time is 1-4 hours, and the aging time is 3-5 days.
[0017] Preferably, in step (5), the carbonization temperature is selected between 600-900°C, and the holding time is 2h.
[0018] The present invention has the following advantages:
[0019] (1) The composite carbon aerogel evaporator prepared by the present invention realizes the integration of the photothermal layer and the thermal insulation layer, and has both good photothermal conversion capability and low thermal conductivity.
[0020] (2) The present invention uses bacterial cellulose as a reinforcing skeleton to prepare bacterial cellulose / phenolic carbon composite aerogel to solve the problem of high brittleness of single phenolic carbon aerogel.
[0021] (3) The present invention uses a “one-step in-situ composite method” to achieve both the composite of bacterial cellulose and phenolic formaldehyde and the doping of metal nanoparticles, further improving the photothermal conversion capability of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the SEM image of Example 4 of the present invention.
[0023] Figure 2 4 and 5 are water evaporation rate curves of various embodiments.
[0024] Figure 3 The following are curves showing the surface temperature variation with time under water evaporation in each embodiment. DETAILED DESCRIPTION
[0025] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these cases.
[0026] Example 1:
[0027] 0.8g of resorcinol and 60mg of nickel acetate tetrahydrate were weighed and added to 10mL of deionized water. The pH was adjusted to 6.6, and 1.1mL of formaldehyde solution was added. After mixing thoroughly, the mixture was transferred to a sealed container and placed in a 60°C oven for gelation and aging for 3 days. The prepared composite hydrogel was then freeze-dried for 48 hours to obtain a composite aerogel. The composite aerogel was then carbonized in a tubular furnace under a nitrogen atmosphere at 800°C for 2 hours to obtain a bacterial cellulose / phenolic carbon aerogel loaded with nickel metal nanoparticles.
[0028] Example 2:
[0029] 1 mmol of TEMPO and 1 mmol of sodium bromide were weighed to oxidize 1 g of bacterial cellulose, then washed by centrifugation and redispersed to form a 0.2 mg / mL bacterial cellulose dispersion. 0.8 g of resorcinol and 60 mg of nickel acetate tetrahydrate were added to 10 mL of the bacterial dispersion. The pH was adjusted to 6.6, and 1.1 mL of formaldehyde solution was added. After mixing thoroughly, the mixture was transferred to a sealed container and placed in a 60°C oven for gelation and aging for 3 days. The resulting composite hydrogel was then freeze-dried for 48 hours to obtain a composite aerogel. The composite aerogel was then carbonized in a tube furnace under a nitrogen atmosphere at 800°C for 2 hours to obtain a bacterial cellulose / phenolic carbon aerogel loaded with nickel metal nanoparticles.
[0030] Example 3:
[0031] The oxidized bacterial cellulose was redispersed in deionized water to form a 0.5 mg / mL bacterial cellulose dispersion. Subsequently, the precursor solution was prepared in 10 mL of the bacterial cellulose dispersion. Other conditions were the same as those in Example 2.
[0032] Example 4:
[0033] The oxidized bacterial cellulose was redispersed in deionized water to form a 0.8 mg / mL bacterial cellulose dispersion. Subsequently, the precursor solution was prepared in 10 mL of the bacterial cellulose dispersion. Other conditions were the same as in Example 2.
[0034] Some embodiments of the present invention have been described in detail above, but the present invention is not limited to the described embodiments. Those skilled in the art may make equivalent modifications or substitutions without departing from the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. The present invention provides a method for preparing bacterial cellulose / phenolic carbon aerogel loaded with metal nanoparticles for photothermal evaporation. The problem of large brittleness of single phenolic carbon aerogel is overcome to a certain extent by compounding with bacterial cellulose. The main preparation steps are as follows: Step (1) oxidizes bacterial cellulose with TEMPO and sodium bromide, collects the cellulose through centrifugation, washes it, and then redisperses it in deionized water to form a bacterial cellulose dispersion. Step (2) Weigh a certain amount of resorcinol and metal acetate, add them to the bacterial cellulose suspension, stir evenly, adjust the pH of the solution, then add an appropriate amount of formaldehyde solution, and stir to obtain a uniform solution. Step (3) placing the mixed solution obtained in step (2) in a sealed container, and performing gelation and aging treatment in a forced air oven to obtain a composite hydrogel. Step (4) placing the composite hydrogel obtained in step (3) into a vacuum freeze dryer and freeze-drying for 48 hours to obtain a composite aerogel. Step (5) The composite aerogel obtained in step (4) is subjected to high-temperature carbonization treatment under the protection of a nitrogen atmosphere to obtain a bacterial cellulose / phenolic composite carbon aerogel loaded with metal nanoparticles.
2. The method according to claim 1, characterized in that In step (1), the mass ratio of TEMPO: sodium bromide: bacterial cellulose is 0.0016:0.1:1; and the concentration of the bacterial cellulose suspension is 0.2-0.8 mg / mL.
3. The method according to claim 1, characterized in that In step (2), the concentration of the precursor (resorcinol + formaldehyde) is generally selected to be 8-12%; the molar ratio of resorcinol to formaldehyde is fixed at 1:2; the metal salt is generally selected from nickel acetate, zinc acetate, cobalt acetate, etc.; the molar ratio of the metal salt to resorcinol is generally 1:50-1:20; and the pH of the precursor solution is selected to be in the range of 6.4-6.
7.
4. The method according to claim 1, characterized in that In step (3), the oven temperature is 40-80° C., the gel time is 1-4 hours, and the aging time is 3-5 days.
5. The method according to claim 1, characterized in that: In step (5), the carbonization temperature is selected between 600-900° C. and the insulation time is 2 h.
6. A composite carbon aerogel material prepared by the method according to any one of claims 1 to 5, characterized in that: The prepared material has good photothermal conversion performance and low thermal conductivity. Under the irradiation of one sun, a precision electronic analytical balance was used to record the change in water mass of the composite carbon aerogel during evaporation in real time, and an infrared camera was used to record the change in surface temperature of the composite carbon aerogel. The water evaporation rate can reach 1.77-2.17 kg m -2 h -1 .
Citation Information
Patent Citations
Lignin / bacterial cellulose composite flexible carbon aerogel and preparation method and application thereof
CN106698389A
Preparation method of modified phenolic resin cellulose composite membrane and application thereof
CN109021297A
Preparation method of lithium metal negative electrode based on lithium-philic three-dimensional carbon-based current collector
CN112750987A
Preparation method of carbon aerogel capable of loading metal and having high photothermal conversion efficiency
CN117069090A
Production of monodisperse aerogel particles
DE102021100898A1