Flexible cavity MXene film for SERS (Surface Enhanced Raman Scattering) substrate as well as preparation method and application of flexible cavity MXene film
By introducing Mie resonance structure into MXene materials, the problems of low sensitivity and easy stacking of MXene materials in the SERS field are solved, and a flexible cavity MXene film SERS substrate with high sensitivity is prepared, achieving efficient detection of nanoscale microplastics.
Patent Information
- Application Number
- CN202411136212.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-12-06
AI Technical Summary
The low sensitivity and easy stacking problems of existing MXene materials in the SERS field have led to insufficient accuracy in the detection of nanoscale microplastics in water and terrestrial environments.
A high-yield oligolayer Ti3C2Tx was prepared by gentle wet chemical etching method, and electrostatically self-assembled with polystyrene microspheres. A flexible cavity MXene film was prepared by vacuum-assisted filtration method, and Mie resonance was introduced to improve the sensitivity of the SERS substrate.
A high sensitivity flexible cavity MXene film SERS substrate has been obtained with strong stability and good repeatability, which can be widely used in flexible wearable sensing, medical and environmental monitoring, and has significantly improved the detection sensitivity and accuracy of nano-scale microplastics. sex.
Smart Images

Figure CN119079997A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of SERS substrate materials, and in particular to a flexible cavity MXene film for a SERS substrate, and a preparation method and application thereof. Background Art
[0002] Surface enhanced Raman scattering (SERS) is a molecular spectroscopy technology that can achieve fast and non-destructive detection. It not only inherits the advantages of traditional Raman spectroscopy, but also has higher sensitivity and specificity. It can accurately detect analytes at extremely low concentrations. Therefore, it has become one of the important technologies for measuring analysis. In 1974, Fleischmann et al. accidentally discovered the phenomenon of Raman enhancement on the surface of a rough silver electrode. Subsequently, the research and application of SERS technology rose rapidly and was widely used in environmental medical monitoring, single molecule detection, and sensor imaging. In just a few decades since the discovery of SERS, high-performance SERS substrate designs have emerged, including precious metal nanostructures, composite nanostructures, core-shell nanostructures, metal oxides, single-element semiconductors, organic matter, transition metal sulfides, and some nano-metal-based mixed substrate materials. Currently commercialized precious metal substrates mainly rely on evenly distributed "hot spots" to enhance the Raman signals of the molecules to be tested. However, nanoscale microplastics (MPs), which are usually >20nm, are difficult to approach these hot spots. In addition, the surface end groups of precious metals are limited, resulting in insufficient affinity with molecules on the MPs surface. Therefore, detecting MPs at low concentrations is still challenging.
[0003] MXene is a two-dimensional (2D) material composed of transition metal carbon / nitrogen compounds. It has low visible light absorption, high specific surface area, fluorescence quenching and good molecular enrichment, and has been proven to have excellent SERS activity. As a SERS substrate material, MXene can improve biocompatibility, make the analyte easier to be detected by Raman spectroscopy, and can suppress fluorescence interference in resonance spectroscopy measurement by quenching fluorescence, greatly improving the signal-to-noise ratio of detection. Although MXene as a SERS substrate material has shown great application prospects in the SERS field, it is currently mainly used as a substrate in solution or colloidal materials. This substrate is prone to agglomeration, so that the active sites on its surface cannot be fully utilized. At the same time, since the enhancement of MXene to SERS is mainly based on chemical enhancement (CM), the low sensitivity and poor enrichment of the MXene SRES substrate make it impossible to accurately detect MPs in water environments and terrestrial environments. Therefore, the potential of MXene in the SERS field needs to be further developed. Summary of the invention
[0004] In order to explain the deficiencies in the above background technology, the present invention provides a flexible cavity MXene film for SERS substrate and a preparation method and application thereof. The method uses a mixed solution of HCl and lithium salt in a mild wet chemical etching method to etch and prepare a high-yield few-layer Ti3C2T x and combined with polystyrene microspheres (PS) electrostatic self-assembly to prepare Ti3C2T by vacuum-assisted filtration. x @PS flexible MXene film, and chemically etch to remove PS to obtain a highly sensitive flexible cavity MXene film SRES substrate. The present invention solves the problem of low SERS sensitivity caused by heavy stacking of MXene materials and relying solely on chemical enhancement. Under the condition of Mie resonance (i.e. electromagnetic enhancement) introduced by the cavity, the obtained cavity MXene film SERS substrate has strong stability, good repeatability, adjustable structure size, high sensitivity and can be put into practical application. It has broad application prospects in the fields of flexible wearable sensing, medicine and environmental monitoring.
[0005] The first object of the present invention is to provide a method for preparing a flexible cavity MXene film for a SERS substrate, comprising the following steps: Preparation of single-layer Ti3C2T x Colloidal solutions; Towards single-layer Ti3C2T x PS microsphere suspension was added to the colloidal solution and mixed evenly to obtain a MXene@PS mixed solution; The MXene@PS mixed solution was vacuum-assisted filtered through a microporous filter membrane to form a composite film on the microporous filter membrane, and then dried at 27-40°C for 2-8h to obtain a MXene@PS composite flexible film; The MXene@PS composite flexible film was immersed in tetrahydrofuran and placed in a fume hood for 8 to 12 hours to obtain a flexible cavity MXene film for SERS substrate.
[0006] Preferably, the single layer Ti3C2T x The colloidal solution was prepared according to the following steps: Evenly dispersing LiF in a hydrochloric acid solution to obtain a mixed solution of HCl and LiF; The Ti3AlC2MAX precursor powder was added into a mixed solution of HCl and LiF, stirred and etched at 10-50°C for 20-50 h, and then post-treated to obtain a clay-like precipitate. The clay-like precipitate was evenly dispersed in deionized water, treated with ultrasound, and centrifuged to obtain the upper colloidal solution to obtain a single-layer Ti3C2T x Colloidal solution.
[0007] Preferably, the concentration of the hydrochloric acid solution is 3-12 mol / L; the dosage ratio of LiF to the hydrochloric acid solution is 0.5-5 g:10-60 mL; the mass ratio of the Ti3AlC2MAX precursor powder to LiF is 0.5-3:0.5-5; The single-layer Ti3C2T x The concentration of the colloidal solution is 2~10 mg / mL.
[0008] Preferably, the post-treatment is to wash the etched product with a certain amount of 12 M hydrochloric acid at 8000-10000 rpm for 10-20 min, then remove the supernatant, repeat the acid washing three times, and then repeat the centrifugation washing with deionized water for multiple times, each time for 10-15 min, at a speed of 8000-10000 rpm, until the pH value of the supernatant reaches neutral, stop the centrifugation, pour out the supernatant, and collect the swollen clay-like precipitate in the lower layer.
[0009] Preferably, the concentration of the PS microsphere suspension is 20-30 mg / mL; x The mass concentration ratio of the colloidal solution to the PS microsphere suspension is 1-6:1; the particle size of the PS microspheres in the PS microsphere suspension is 50-500 nm.
[0010] Preferably, towards a single layer Ti3C2T x When the PS microsphere suspension is added to the colloidal solution, the adding speed of the PS microsphere suspension is 5s~15s / drop.
[0011] Preferably, the microporous filter membrane is an aqueous mixed cellulose microporous filter membrane with a pore size of 0.22 μm.
[0012] Preferably, when the MXene@PS composite flexible film is immersed in tetrahydrofuran, the process comprises: Place the MXene@PS composite flexible film in a glass culture dish and add a certain amount of tetrahydrofuran until it covers the film by 0.5-1 cm. After placing in a fume hood for 8 to 12 hours, rinse the film with alcohol until the tetrahydrofuran is completely removed. When rinsing with alcohol, first soak it in alcohol for 2 to 5 minutes, then rinse with alcohol 5 to 8 times, and dry it naturally.
[0013] The second object of the present invention is to provide a flexible cavity MXene film for SERS substrate.
[0014] The third object of the present invention is to provide an application of a flexible cavity MXene film in a SERS substrate.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a flexible cavity MXene film for SERS substrate and a preparation method and application thereof. The present invention adopts a mixed solution of HCl and lithium salt in a mild wet chemical etching method to etch and prepare a high-yield few-layer Ti3C2T x and combined with polystyrene microspheres (PS) electrostatic self-assembly to prepare Ti3C2T by vacuum-assisted filtration. x @PS flexible MXene film, and chemically etched to remove PS to obtain a highly sensitive flexible cavity MXene film SRES substrate. The prepared cavity MXene film solves the problem of metal nanoparticle agglomeration in metal nanoparticle sol solution, which leads to uneven hot spot distribution and unstable structure, and is easily oxidized. At the same time, it eliminates the sampling limitation caused by the metal nanoparticle suspension having to be mixed with the analyte.
[0016] Since the present invention adopts MXene as the base material, the biocompatibility is improved, and the fluorescence interference in the resonance spectrum measurement can be suppressed by quenching the fluorescence, thereby greatly improving the signal-to-noise ratio of the detection.
[0017] In the present invention, a soft sacrificial template is introduced to form a three-dimensional structure, which effectively overcomes the stacking overlap problem caused by the van der Waals force and hydrogen bonding between the two-dimensional nanosheets. This is because the three-dimensional assembly expands the interlayer structure and promotes the cross-linking between the MXene nanosheets, thereby forming a three-dimensional penetrating interconnected network. In addition, by forming an optical resonant cavity between the two-dimensional materials, not only is light collection achieved inside the three-dimensional SERS substrate to provide a large focusing tolerance, but the special cavity structure and large specific surface area effectively increase the adsorption of nanoscale MPs.
[0018] The present invention introduces Mie scattering resonance by regulating the optical resonant cavity. Mie scattering resonance refers to the ability to utilize the optical resonance (also known as Mie scattering resonance) of Whispering Gallery Modes (WGM) in the visible light range to improve the sensitivity of the SERS substrate when the nanomaterial has a narrowly distributed microscopic cavity structure (usually 100-700nm). An optical resonant cavity is constructed in the MXene flexible film, and the signal generated by the Mie resonance scattering generated by it is effectively utilized to enhance and enrich more nanoscale MPs, overcoming the dilemma of low sensitivity and enhancement factor caused by the main reliance on chemical enhancement of MXene materials, so that the invention can be widely used in flexible wearable electronic products and equipment, medicine, and environmental monitoring. As described above, the present invention solves the problems of poor repeatability, low signal-to-noise ratio, easy stacking of MXene, and low sensitivity in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The multilayer Ti3C2T prepared in the present inventionx SEM images of MXene; Figure 2 The single-layer Ti3C2T prepared in the present invention x AFM photos of MXene; Figure 3 This is a SEM photo of the MXene@PS composite flexible film prepared in the present invention; Figure 4 This is a SEM photo of the flexible cavity MXene film prepared in the present invention; Figure 5 The SERS response signal diagram of the highly sensitive flexible cavity MXene film SERS substrate prepared in the present invention detecting different concentrations of Rhodamine 6G (R6G); Figure 6 The high-sensitivity flexible cavity MXene film SERS substrate prepared in the present invention was tested after being placed for different days for 10 -5 M SERS response signal diagram of R6G; Figure 7 The SERS response signal diagram of the highly sensitive flexible cavity MXene film SERS substrate prepared in the present invention detecting PMMA with different concentrations; Figure 8 The SERS response signal diagram of the highly sensitive flexible cavity MXene film SERS substrate prepared in the present invention detecting PVC of different concentrations; Fig. 9 The SERS response signal diagram of the highly sensitive flexible cavity MXene film SERS substrate prepared in the present invention detecting PS of different concentrations; Fig.10 The high-sensitivity flexible cavity MXene film SERS substrate prepared in the present invention and the flexible MXene film SERS substrate are used to detect 10 -7 SERS response signal diagram of R6G. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.
[0021] The main purpose of the present invention is to solve the problems of poor repeatability, low signal-to-noise ratio, easy stacking of MXene and low sensitivity in the prior art. The present invention is based on the fact that MXene, as a material with high electrical conductivity and chemical activity, can be designed into a micro-nanoscale cavity structure. These cavity structures can induce whispering gallery modes (WGMs). By adjusting the geometric parameters of the cavity, the resonant frequency can be further optimized, thereby enhancing the SERS effect. In addition, the design of the cavity structure can increase the curvature in space, effectively increase the effective volume in the space, allow more molecules to enter the high enhancement area, and greatly improve the sensitivity and accuracy of microplastic detection.
[0022] In order to achieve the above object, the present invention provides a method for preparing a flexible cavity MXene film for a SERS substrate in a first aspect, comprising the following steps: Preparation of single-layer Ti3C2T x Colloidal solutions; Towards single-layer Ti3C2T x PS microsphere suspension was added to the colloidal solution and mixed evenly to obtain a MXene@PS mixed solution; The MXene@PS mixed solution was vacuum-assisted filtered through a microporous filter membrane to form a composite film on the microporous filter membrane, and then dried at 27-40°C for 2-8h to obtain a MXene@PS composite flexible film; The MXene@PS composite flexible film was immersed in tetrahydrofuran and placed in a fume hood for 8 to 12 hours to obtain a flexible cavity MXene film for SERS substrate.
[0023] Wherein, the single layer Ti3C2T x The colloidal solution was prepared according to the following steps: Evenly dispersing LiF in a hydrochloric acid solution to obtain a mixed solution of HCl and LiF; The Ti3AlC2MAX precursor powder was added into a mixed solution of HCl and LiF, stirred and etched at 10-50°C for 20-50 h, and then post-treated to obtain a clay-like precipitate. The clay-like precipitate was evenly dispersed in deionized water, treated with ultrasound, and centrifuged to obtain the upper colloidal solution to obtain a single-layer Ti3C2T x Colloidal solution.
[0024] The post-treatment is to wash the etched product with a certain amount of 12 M hydrochloric acid at 8000-10000 rpm for 10-20 minutes, then remove the supernatant, repeat the acid washing three times, and then repeat the centrifugation washing with deionized water for multiple times, each time for 10-15 minutes, at a speed of 8000-10000 rpm, until the pH value of the supernatant reaches neutral, stop the centrifugation, pour out the supernatant, and collect the swollen clay-like precipitate in the lower layer.
[0025] The concentration of the hydrochloric acid solution is 3-12 mol / L; the dosage ratio of LiF to the hydrochloric acid solution is 0.5-5 g:10-60 mL; the mass ratio of the Ti3AlC2MAX precursor powder to LiF is 0.5-3:0.5-5; The single-layer Ti3C2T x The concentration of the colloidal solution is 2~10 mg / mL.
[0026] Single layer Ti3C2T x In the colloidal solution, the lateral size of the single-layer Ti3C2MXene is 1~2μm, the number of layers is 1~3, the yield is 70~90%, and the surface Zeta potential is negative.
[0027] The concentration of the PS microsphere suspension is 20-30 mg / mL; the monolayer Ti3C2T x The mass concentration ratio of the colloidal solution to the PS microsphere suspension is 1-6:1; the particle size of the PS microspheres in the PS microsphere suspension is 50-500 nm.
[0028] Towards single-layer Ti3C2T x When the PS microsphere suspension is added to the colloidal solution, the adding speed of the PS microsphere suspension is 5s~15s / drop.
[0029] The microporous filter membrane is a water-based mixed cellulose microporous filter membrane, and its pore size is 0.22 μm.
[0030] When the MXene@PS composite flexible film is immersed in tetrahydrofuran, it includes: Place the MXene@PS composite flexible film in a glass culture dish and add a certain amount of tetrahydrofuran until it covers the film by 0.5-1 cm. After placing in a fume hood for 8 to 12 hours, rinse the film with alcohol until the tetrahydrofuran is completely removed. When rinsing with alcohol, first soak it in alcohol for 2 to 5 minutes, then rinse with alcohol 5 to 8 times, and dry it naturally.
[0031] In one embodiment, a method for preparing a flexible cavity MXene film for a SERS substrate specifically comprises the following steps: Step S1: Preparation of single-layer MXene: Ti3C2T was prepared by chemical wet etching x Specifically, 10 to 60 mL of 3 to 12 mol / L hydrochloric acid solution is prepared, and then it is transferred to a polytetrafluoroethylene container, 0.5 to 5 g of lithium fluoride (LiF) is slowly added thereto, and stirred with a water bath magnetic stirrer for 15 to 30 min until it is completely dissolved (the temperature is set at 20 to 50°C and the speed is 350 to 600 rpm), to obtain a mixed solution of HCl and LiF; Weigh 0.5 ~ 3 g Ti3AlC2MAX precursor powder and add it to the mixed solution of HCl and LiF. After stirring and etching at 10 ~ 50 ° C for 20 ~ 50 h, the obtained mixed solution is centrifuged and washed at 8000 rpm for 10 min with a certain amount of 9 ~ 12 M hydrochloric acid, and then the supernatant is removed. Repeat the acid washing three times. Then the obtained precipitate is repeatedly centrifuged and washed with deionized water for 10 min each time at 8000 rpm until the pH of the supernatant reaches neutral, stop centrifugation, pour out the supernatant, collect the swollen clay-like precipitate in the lower layer, disperse it in a certain amount of deionized water, use an ultrasonic cell crusher (60 ~ 300 W) for ice bath ultrasonication for 20 ~ 40 minutes, and then centrifuge the sonicated solution at 3500 ~ 5000 rpm for 10 ~ 30 min, and take the upper dark green colloidal solution, which is the single layer Ti3C2T x MXene colloidal solution, Ti3C2T x The appropriate concentration of the colloidal solution is 2 to 10 mg / ml; Among them, single-layer Ti3C2T x Determination of MXene colloidal solution concentration: Take a certain volume of the single-layer Ti3C2T x The MXene colloidal solution was vacuum-assisted filtered using an aqueous mixed cellulose microporous filter membrane with a pore size of 0.22 μm. The MXene film obtained after filtration was vacuum dried at 40 °C for 4 h, and finally the dry MXene film was peeled off from the microporous filter membrane. The weight of the dried MXene film was measured to determine the concentration of the MXene solution.
[0032] In step S1, by chemical wet etching, a single-layer MXene is prepared with a lateral size of 1 to 2 μm, a layer number of 1 to 3 layers, a yield of 70% to 90%, a negative surface Zeta potential, and a positive edge potential.
[0033] Step S2: Preparation of MXene@PS mixed solution: Single-layer Ti3C2T xand PS nanospheres. The specific steps are to take a certain amount of the single-layer Ti3C2T x The MXene colloidal solution was placed in a sample bottle and stirred at 1000-1500 rpm for 20-30 min at room temperature. A certain amount of PS microsphere suspension was slowly dripped into the sample bottle while stirring. The mixture was then ultrasonically mixed for 10-20 min and finally stirred at 800 rpm for 8-12 h at room temperature to obtain a MXene@PS mixed solution. The dripping speed of the PS microsphere suspension was 5s-15s / drop, and the particle size of the PS microspheres was in the range of 50-500 nm.
[0034] Step S3: Preparation of MXene@PS composite flexible film: The solution described in step S2 is vacuum-assisted filtered through a water-based mixed cellulose microporous filter membrane with a pore size of 0.22 μm, and the composite film obtained after filtration is dried in a vacuum oven at 27~40 ℃ for 2~8 hours, and finally peeled off from the microporous filter membrane to obtain a dry MXene@PS composite flexible film.
[0035] Step S4: Preparation of highly sensitive flexible cavity MXene film SERS substrate: Place the MXene@PS composite flexible film obtained in step S3 in a glass culture dish, add a certain amount of tetrahydrofuran to a height of 0.5 to 1 cm above the film, place it in a fume hood for 8 to 12 h, rinse the film with alcohol to completely remove the tetrahydrofuran, and obtain a highly sensitive flexible cavity MXene film SERS substrate after drying.
[0036] When rinsing with alcohol, first soak it in alcohol for 2 to 5 minutes, then rinse with alcohol 5 to 8 times, and dry it naturally.
[0037] A second aspect of the present invention provides a flexible cavity MXene film for a SERS substrate.
[0038] A third aspect of the present invention provides an application of a flexible cavity MXene film in a SERS substrate.
[0039] In one embodiment, it is used for a high-sensitivity flexible cavity MXene thin film SERS substrate, characterized in that it is assembled into a three-dimensional high-sensitivity MXene aerogel flexible film SERS substrate for detecting low-concentration, nanoscale microplastic waste.
[0040] During use, for the detection of low-concentration nanoscale microplastics (MPs): prepare several sample bottles, dilute the 25 mg / ml MPs suspension into 0.001 mg / ml ~ 1 mg / ml MPs suspension with a scale of 50 nm. Cut the flexible cavity MXene film prepared in step S4 above into 0.5 cm × 0.5 cm slices, adhere them to the glass substrate with double-sided tape, take out 10 ~ 100 μl of the test liquid droplets on the flexible cavity MXene film with a pipette, dry them naturally or in a 40 ° C oven, and then perform Raman spectroscopy analysis.
[0041] It should be noted that the experimental methods used in the present invention are all conventional methods unless otherwise specified; the reagents and materials used are all commercially available unless otherwise specified.
[0042] Example 1 Preparation of Highly Sensitive Flexible Cavity MXene Film SERS Substrate Step 1: Multilayer Ti3C2T x Preparation of MXene mixed solution: HF is generated in situ by mixing HCl and LiF, and the Al atomic layer in the MAX ceramic phase (Ti3AlC2) is selectively etched to prepare a Ti3AlC2MXene dispersion. Specifically: First, prepare 20 mL of 9 mol / L hydrochloric acid solution, then transfer it to a polytetrafluoroethylene container, slowly add 1.6 g of lithium fluoride (LiF), and stir it with a water bath magnetic stirrer for 30 min until it is completely dissolved. Set the temperature to 35 °C and the speed to 400 rpm to obtain a mixed solution of HCl and LiF. Weigh 1 g of Ti3AlC2MAX precursor powder into the above-mentioned mixed solution of HCl and LiF. Be careful to add it slowly to avoid overheating. After stirring and etching at 35 °C for 24 h, collect the product to finally obtain a multilayer Ti3C2MXene dispersion. The prepared multilayer Ti3C2T x The SEM images are as follows Figure 1 shown.
[0043] Step 2: Single-layer Ti3C2T xPreparation of MXene colloidal solution: The multilayer Ti3C2MXene dispersion after etching in step 1 was centrifuged and washed at 8000 rpm for 10 min with a certain amount of 12 M hydrochloric acid, and then the supernatant was removed and the acid washing was repeated three times. The obtained precipitate was then repeatedly centrifuged and washed with deionized water for 10 min each time at 8000 rpm until the pH value of the supernatant reached neutral, the centrifugation was stopped, the supernatant was poured out, and the swollen clay-like precipitate in the lower layer was collected and dispersed in a certain amount of deionized water. The ultrasonic cell crusher (300 W) was used for ice bath ultrasonication for 30 min, and then the ultrasonicated solution was centrifuged at 3500 rpm for 15 min, and the upper dark green colloidal solution was taken and stored in a dark environment of 4 ~ 8 °C. The obtained single-layer Ti3C2T x AFM images of colloidal solutions are shown in Figure 2. Figure 2 shown.
[0044] Step 3: Single layer Ti3C2T x Determination of the concentration of MXene colloidal solution: Take a certain volume of the colloidal solution obtained in step 2, and use a water-based mixed cellulose microporous filter membrane with a pore size of 0.22 μm for vacuum filtration. The MXene film obtained after filtration is vacuum dried at 40 °C for 4 h, and finally the dry MXene film is peeled off from the microporous filter membrane, and the weight of the dried MXene film is measured to determine the concentration of the MXene solution.
[0045] Step 4, electrostatic self-assembly: To prepare a highly sensitive flexible cavity MXene film SERS substrate, a 25 mg / ml monodisperse PS microsphere suspension was mixed with a single layer of Ti3C2T4 obtained in step 2 at a known concentration by stirring and ultrasonic treatment. x The MXene colloidal solution is electrostatically self-assembled into a uniform mixed solution, specifically, a certain amount of the single-layer Ti3C2T x The MXene colloidal solution was placed in a sample bottle and stirred at 1200 rpm for 30 min at room temperature. A certain amount of PS microsphere suspension was added very slowly (1 drop / 10 s) while stirring, followed by ultrasonic mixing for 15 min. Finally, it was stirred at 800 rpm for 8 h at room temperature. The mixture was vacuum-assisted filtered through a water-based mixed cellulose microporous filter membrane with a pore size of 0.22 μm. The composite film obtained after filtration was dried in a vacuum oven at 40 °C for 4 h, and finally peeled off from the microporous filter membrane to obtain a dry MXene@PS composite flexible film. The cross-sectional SEM of the obtained MXene@PS composite flexible film is shown in Figure 2. Figure 3 shown.
[0046] Step 5, preparation of highly sensitive flexible cavity MXene film SERS substrate: Place the composite film obtained in step 4 in a glass culture dish, add a certain amount of tetrahydrofuran to cover the film by about 0.5 to 1 cm, place it in a fume hood overnight, rinse the film with alcohol to completely remove the tetrahydrofuran, and dry it to obtain a highly sensitive flexible cavity MXene film SERS substrate. The cross-sectional SEM of the prepared highly sensitive flexible cavity MXene film SERS substrate is as follows Figure 4 shown.
[0047] Example 2 Preparation of Highly Sensitive Flexible Cavity MXene Film SERS Substrates with Different Cavity Scales Step 1: Multilayer Ti3C2T x Preparation of MXene mixed solution: HF is generated in situ by mixing HCl and LiF, and the Al atomic layer in the MAX ceramic phase (Ti3AlC2) is selectively etched to prepare Ti3AlC2MXene dispersion. Specifically: First, prepare 20 mL of 9 mol / L hydrochloric acid solution, then transfer it to a polytetrafluoroethylene container, slowly add 1.6 g of lithium fluoride (LiF), and stir it with a water bath magnetic stirrer for 30 min until it is completely dissolved (set the temperature to 35°C and the speed to 400 rpm). Weigh 1 g of Ti3AlC2MAX precursor powder into the above-mentioned HCl and LiF mixed solution, and be careful to add it slowly to avoid overheating. After stirring and etching at 35°C for 24 h, collect the product and finally obtain a multilayer Ti3C2MXene dispersion.
[0048] Step 2: Single-layer Ti3C2T x Preparation of MXene colloidal solution: The black turbidity after etching in step 1 was washed by centrifugation at 8000 rpm for 10 min with a certain amount of 12 M hydrochloric acid, and then the supernatant was removed. This step was repeated three times. The obtained precipitate was washed repeatedly by centrifugation with deionized water, each time for 10 min, at a speed of 8000 rpm, until the pH value of the supernatant reached neutral, the centrifugation was stopped, the supernatant was poured out, and the swollen clay-like precipitate in the lower layer was collected and dispersed in a certain amount of deionized water. Ultrasonic cell crusher (300 W) was used for ice bath ultrasonication for 30 min, and then the ultrasonic solution was centrifuged at 3500 rpm for 15 min, and the upper dark green colloidal solution was taken and stored in a dark environment of 4 ~ 8 °C.
[0049] Step 3: Single layer Ti3C2T x Determination of MXene colloidal solution concentration: Take a certain volume of the single-layer Ti3C2T xThe MXene colloidal solution was vacuum-assisted filtered using an aqueous mixed cellulose microporous filter membrane with a pore size of 0.22 μm. The MXene film obtained after filtration was vacuum dried at 40 °C for 4 h, and finally the dry MXene film was peeled off from the microporous filter membrane. The weight of the dried MXene film was measured to determine the concentration of the MXene solution.
[0050] Step 4, electrostatic self-assembly: To prepare a scale-adjustable, highly sensitive, flexible cavity MXene film SERS substrate, a 25 mg / ml monodisperse PS microsphere suspension was mixed with a single layer of Ti3C2T4 obtained in step 2 at a known concentration by stirring and ultrasonic treatment. x The MXene colloidal solution is electrostatically self-assembled into a uniform mixed solution, specifically, a certain amount of the single-layer Ti3C2T x The MXene colloidal solution was placed in a sample bottle and stirred at 1200 rpm for 30 min at room temperature. A certain amount of PS microsphere (50 nm, 150 nm, 240 nm, 350 nm, 500 nm) suspension was added very slowly (1 drop / 10 s) while stirring, followed by ultrasonic mixing for 15 min. Finally, the solution was stirred at 800 rpm for 8 h at room temperature. The mixture was vacuum-assisted filtered through a water-based mixed cellulose microporous filter membrane with a pore size of 0.22 μm. The composite film obtained after filtration was dried in a vacuum oven at 40 °C for 4 h, and finally peeled off from the microporous filter membrane to obtain a dry MXene@PS composite flexible film.
[0051] Step 5, preparation of multi-scale high-sensitivity flexible cavity MXene film SERS substrate: place the composite film obtained in step 4 in a glass culture dish, add a certain amount of tetrahydrofuran to cover the film by about 0.5 to 1 cm, place it in a fume hood overnight, rinse the film with alcohol to completely remove the tetrahydrofuran, and obtain a multi-scale high-sensitivity flexible cavity MXene film SERS substrate after drying.
[0052] Example 3 Highly sensitive flexible cavity MXene film SERS substrate and SERS performance test Step 1: Preparation of a highly sensitive flexible cavity MXene thin film SERS substrate: Referring to the operation in Example 1, a highly sensitive flexible cavity MXene thin film SERS substrate is prepared.
[0053] Step 2: Sample preparation: Prepare a 10 -15 ~ 10 -3 M of organic pollutant molecules in ethanol (Rhodamine 6G).
[0054] Step 3: Cut the highly sensitive flexible cavity MXene film SERS substrate prepared in step 1 into 0.5 cm × 0.5 cm thin sheets, stick them on the glass substrate with double-sided tape, take out 20 μl of analysis sample with a pipette and drop it on the highly sensitive flexible cavity MXene film SERS substrate, dry it naturally or in a 40 °C oven for further Raman spectroscopy analysis.
[0055] Step 4: Test the sensitivity and stability of SERS on the highly sensitive flexible cavity MXene film SERS substrate obtained in step 3. Figure 5 The SERS response signal diagram of the high-sensitivity flexible cavity MXene film SERS substrate detecting different concentrations of rhodamine 6G shows that the detection limit of rhodamine 6G by the high-sensitivity flexible cavity MXene film SERS substrate prepared by the present invention can be as low as 10 -15 M.
[0056] Figure 6 The high-sensitivity flexible cavity MXene film SERS substrate was tested after being placed for different days. -5 M SERS response signal diagram of Rhodamine 6G, which shows that the high-sensitivity flexible cavity MXene film SERS substrate prepared by the present invention can still maintain good SERS performance after 60 days.
[0057] Step 5: Reuse of substrate: Rinse the high-sensitivity flexible cavity MXene film SERS substrate after spectral detection in step 3 with ethanol for 5 times. After rinsing the analysis sample, dry it naturally and reuse it as a high-sensitivity flexible cavity MXene film SERS substrate.
[0058] Example 4 Preparation of substrate for detecting low concentration nanoscale MPs and detection of nanoscale MPs Step 1: Preparation of a highly sensitive flexible cavity MXene thin film SERS substrate: Referring to the operation in Example 1, a highly sensitive flexible cavity MXene thin film SERS substrate is prepared.
[0059] Step 2: MPs analysis sample preparation: prepare several sample bottles, dilute the suspensions with a size of 50 nm and a concentration of 25 mg / ml to concentrations of 0.001 mg / ml ~ 1 mg / ml.
[0060] Step three, cut the high-sensitivity flexible cavity MXene film SERS substrate prepared in step one into 0.5 cm × 0.5 cm thin sheets, stick them on the glass substrate with double-sided tape, use a pipette to take out 20 μl of PMMA microspheres, PVC microspheres and PS microspheres to be tested droplets respectively on the labeled high-sensitivity flexible cavity MXene film SERS substrate, dry them naturally or in a 40 °C oven for further Raman spectroscopy analysis.
[0061] Step 4: Test the sensitivity and stability of SERS on the highly sensitive flexible cavity MXene film SERS substrate obtained in step 3. Figure 7 The SERS response signal diagram of the high-sensitivity flexible cavity MXene film SERS substrate detecting PMMA microspheres of different concentrations shows that the detection limit of the PMMA microspheres by the high-sensitivity flexible cavity MXene film SERS substrate prepared by the present invention can be as low as 0.001 mg / ml; Figure 8 The SERS response signal diagram of the high-sensitivity flexible cavity MXene film SERS substrate detecting PVC microspheres of different concentrations shows that the detection limit of the high-sensitivity flexible cavity MXene film SERS substrate prepared by the present invention for PVC microspheres can be as low as 0.01 mg / ml; Fig. 9 This is a SERS response signal diagram of the high-sensitivity flexible cavity MXene film SERS substrate detecting PS microspheres of different concentrations. The figure shows that the detection limit of the high-sensitivity flexible cavity MXene film SERS substrate prepared by the present invention for PS microspheres can be as low as 0.05 mg / ml.
[0062] Step 5: Reuse of substrate: Rinse the high-sensitivity flexible cavity MXene film SERS substrate after spectral detection in step 3 with ethanol for 5 times. After rinsing the analysis sample, dry it naturally and reuse it as a high-sensitivity flexible cavity MXene film SERS substrate.
[0063] Example 5 Same as Example 1, except that Prepare 20 mL of 3 mol / L hydrochloric acid solution; Weigh 0.5 g of lithium fluoride; Weigh 0.5g of Ti3AlC2MAX precursor powder.
[0064] Single layer Ti3C2T x The mass concentration ratio of the colloidal solution to the PS microsphere suspension is 2:1 Example 6 Same as Example 1, except that Prepare 20 mL of 12 mol / L hydrochloric acid solution; Weigh 5 g of lithium fluoride; Weigh 3 g of Ti3AlC2MAX precursor powder; Single layer Ti3C2T x The mass concentration ratio of the colloidal solution to the PS microsphere suspension was 6:1. Comparative Example 1 Preparation of flexible MXene film SERS substrate Step 1: Multilayer Ti3C2T x Preparation of MXene mixed solution: HF is generated in situ by mixing HCl and LiF, and the Al atomic layer in the MAX ceramic phase (Ti3AlC2) is selectively etched to prepare Ti3AlC2MXene dispersion. Specifically: First, prepare 20 mL of 9 mol / L hydrochloric acid solution, then transfer it to a polytetrafluoroethylene container, slowly add 1.6 g of lithium fluoride (LiF), stir it with a water bath magnetic stirrer for 30 min until it is completely dissolved, set the temperature to 35 °C and the speed to 400 rpm. Weigh 1 g of Ti3AlC2MAX precursor powder into the above-mentioned HCl and LiF mixed solution, pay attention to add it slowly to avoid overheating, stir and etch at 35 °C for 24 h, and collect the product to finally obtain a multilayer Ti3C2MXene dispersion.
[0065] Step 2: Single-layer Ti3C2T x Preparation of MXene solution: The black turbidity after etching in step 1 was washed by centrifugation at 8000 rpm for 10 min with a certain amount of 12 M hydrochloric acid, and then the supernatant was removed. Repeat the acid washing three times. Then the obtained precipitate was washed repeatedly by centrifugation with deionized water, each time for 10 min, at a speed of 8000 rpm, until the pH value of the supernatant reached neutral, the centrifugation was stopped, the supernatant was poured out, and the swollen clay-like precipitate in the lower layer was collected and dispersed in a certain amount of deionized water. Ultrasonic cell crusher (300 W) was used for ice bath ultrasonication for 30 min, and then the ultrasonic solution was centrifuged at 3500 rpm for 15 min, and the upper dark green colloidal solution was taken and stored in a dark environment of 4 ~ 8 °C.
[0066] Step 3, determination of MXene solution concentration: take a certain volume of the colloidal solution obtained in step 2, use a water-based mixed cellulose microporous filter membrane with a pore size of 0.22 μm for vacuum filtration, and vacuum dry the MXene film obtained after filtration at 40°C for 4 h. Finally, peel off the dry MXene film from the microporous filter membrane, and measure the weight of the dried MXene film to determine the concentration of the MXene solution.
[0067] Step 4, preparation of flexible MXene film: Take a certain amount of the single-layer Ti3C2 colloidal solution obtained in step 2, and perform vacuum-assisted filtration through a water-based mixed cellulose microporous filter membrane with a pore size of 0.22 μm. The film obtained after filtration is dried in a vacuum oven at 40 °C for 4 h, and finally peeled off from the microporous filter membrane to obtain a dry flexible MXene film.
[0068] Step 5: Perform SERS test on the flexible MXene film obtained in step 4. Fig.10 Flexible MXene film and high sensitivity flexible cavity MXene film SERS substrate detection 10 -7 The SERS response signal diagram of Rhodamine 6G shows that the enhancement effect of the high-sensitivity flexible cavity MXene film SERS substrate prepared by the present invention is much higher than that of the flexible MXene film.
Claims
1. A method for preparing a flexible cavity MXene film for a SERS substrate, characterized in that: The following steps are involved: Preparation of single-layer Ti3C2T x Colloidal solutions; Towards monolayer Ti3C2T x PS microsphere suspension was added to the colloidal solution and mixed evenly to obtain a MXene@PS mixed solution; The MXene@PS mixed solution was vacuum-assisted filtered through a microporous filter membrane to form a composite film on the microporous filter membrane, and then dried at 27-40°C for 2-8h to obtain a MXene@PS composite flexible film; The MXene@PS composite flexible film was immersed in tetrahydrofuran and placed in a fume hood for 8 to 12 hours to obtain a flexible cavity MXene film for SERS substrate.
2. The method for preparing a flexible cavity MXene film for a SERS substrate according to claim 1, characterized in that: The single-layer Ti3C2T x The colloidal solution was prepared according to the following steps: Evenly dispersing LiF in a hydrochloric acid solution to obtain a mixed solution of HCl and LiF; The Ti3AlC2 MAX precursor powder was added into a mixed solution of HCl and LiF, stirred and etched at 10-50°C for 20-50 h, and then post-treated to obtain a clay-like precipitate. The clay-like precipitate was evenly dispersed in deionized water, subjected to ultrasound and centrifugation, and the upper colloidal solution was taken to obtain a single-layer Ti3C2T x Colloidal solution.
3. The method for preparing a flexible cavity MXene film for a SERS substrate according to claim 2, characterized in that: The concentration of the hydrochloric acid solution is 3-12 mol / L; the dosage ratio of LiF to the hydrochloric acid solution is 0.5-5 g:10-60 mL; the mass ratio of the Ti3AlC2 MAX precursor powder to LiF is 0.5-3:0.5-5; The single-layer Ti3C2T x The concentration of the colloidal solution is 2~10 mg / mL.
4. The method for preparing a flexible cavity MXene film for a SERS substrate according to claim 2, characterized in that: The post-treatment is to wash the etched product with a certain amount of 12 M hydrochloric acid at 8000-10000 rpm for 10-20 minutes, then remove the supernatant, repeat the acid washing three times, and then repeat the centrifugation washing with deionized water for multiple times, each time for 10-15 minutes, at a speed of 8000-10000 rpm, until the pH value of the supernatant reaches neutral, stop the centrifugation, pour out the supernatant, and collect the swollen clay-like precipitate in the lower layer.
5. The method for preparing a flexible cavity MXene film for a SERS substrate according to claim 1, characterized in that: The concentration of the PS microsphere suspension is 20-30 mg / mL; The single-layer Ti3C2T x The mass concentration ratio of the colloidal solution to the PS microsphere suspension was 1 to 6:1; The particle size of the PS microspheres in the PS microsphere suspension is 50 to 500 nm.
6. The method for preparing a flexible cavity MXene film for a SERS substrate according to claim 1, characterized in that: Towards monolayer Ti3C2T x When the PS microsphere suspension is added to the colloidal solution, the adding speed of the PS microsphere suspension is 5s~15s / drop.
7. The method for preparing a flexible cavity MXene film for a SERS substrate according to claim 1, characterized in that: The microporous filter membrane is a water-based mixed cellulose microporous filter membrane, and its pore size is 0.22 μm.
8. The method for preparing a flexible cavity MXene film for a SERS substrate according to claim 1, characterized in that: When the MXene@PS composite flexible film is immersed in tetrahydrofuran, it includes: Place the MXene@PS composite flexible film in a glass culture dish and add a certain amount of tetrahydrofuran until it covers the film by 0.5-1 cm. After placing in a fume hood for 8 to 12 hours, rinse the film with alcohol until the tetrahydrofuran is completely removed. When rinsing with alcohol, first soak it in alcohol for 2 to 5 minutes, then rinse with alcohol 5 to 8 times, and dry it naturally.
9. A flexible cavity MXene film for SERS substrate prepared by the method according to any one of claims 1 to 8.
10. Use of the flexible cavity MXene film according to claim 9 in a SERS substrate.
Citation Information
Patent Citations
MXene-based three-dimensional porous flexible self-supporting membrane, preparation method thereof and application of membrane in electrochemical adsorption of dyes
CN112452299A
Ti3C2Tx-MXene flexible self-supporting film and preparation method thereof
CN113493207A
Mxene / metal composite aerogel, preparation method therefor and use thereof, and thermal interface material containing same
WO2021056851A1
