Preparation method of small-particle-size hollow nano silicon dioxide
Through the polymerization reaction of the mixed reaction system of template agent, surfactant, silicon source and catalyst, and pH adjustment and calcination treatment, the problems of inhomogeneity and process complexity in the preparation of hollow nanosilicon dioxide in small particle size are solved. It realizes an efficient and simple preparation method and is suitable for industrial production.
Patent Information
- Application Number
- CN202411223184.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to stabilize the preparation of small-particle hollow nanosilicon dioxide, the products are uneven and easy to aggregate, and the process is complicated by other drying methods, low efficiency, and has not been seen in industrial applications.
By polymerizing the mixed reaction system of template agent, surfactant, silicon source and catalyst, prepolymerization products of core-shell structure are prepared and aged, and the pH value of the reaction system is adjusted to 2 to 6, and then the pH value of the reaction system is carried out Separation and calcination treatment to produce small-particle hollow nanosilicon dioxide.
It realizes efficient acquisition of small-particle hollow nanosilicon dioxide from polymerization products, eliminating the expensive and complex drying process, and providing a simple and efficient preparation method, suitable for industrial production.
Smart Images

Figure CN119080012A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano materials, and in particular relates to a method for preparing small-diameter hollow nano silicon dioxide. Background Art
[0002] Hollow silica particles have properties such as low density, low refractive index, and material loading and coating performance. They are widely used in lightweight materials, thermal insulation materials, low-reduction reflective materials, biological carrier materials, thermal insulation materials and other fields. At present, hollow silica is mostly prepared by template method, and the general particle size is above 100nm. It is rare to stably prepare small-particle hollow silica. Currently, most of the applications are in the range of 200nm to 3μm. It is difficult to prepare below 100nm, and there is no industrialization. At present, small-particle hollow nano-silica has a very strong size effect, the product is uneven and easy to aggregate, and the product is difficult to obtain by centrifugation from the solution system. The process is complicated and inefficient by other drying methods. Therefore, it is urgent to provide a method for preparing small-particle hollow nano-silica. Summary of the invention
[0003] The main purpose of the present invention is to provide a method for preparing small-particle hollow nano-silica to overcome the shortcomings of the prior art.
[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0005] The present invention provides a method for preparing small-particle hollow nano-silica, which comprises:
[0006] A mixed reaction system containing at least a template, a surfactant, a silicon source and a catalyst is polymerized to obtain a prepolymerized product with a core-shell structure;
[0007] Furthermore, the reaction system obtained by the polymerization reaction is subjected to aging treatment, and the pH value of the reaction system is adjusted to 2-6, and then separated and calcined to obtain small-particle hollow nano-silicon dioxide.
[0008] The embodiment of the present invention also provides small-particle hollow nano-silica prepared by the aforementioned preparation method.
[0009] Compared with the prior art, the present invention has the following beneficial effects:
[0010] (1) The present invention can obtain small-particle hollow nano-silica from the polymer product by reverse acidification and centrifugation, eliminating the current expensive and complicated drying process (such as freeze drying and spray drying);
[0011] (2) The preparation method of small-particle hollow nano-silica provided by the present invention has simple process and high efficiency and can be used for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0013] Figure 1-Figure 2 This is a TEM image of the small-particle hollow nano-silica prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0014] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0015] Specifically, as one aspect of the technical solution of the present invention, a method for preparing small-particle hollow nano-silica includes:
[0016] A mixed reaction system containing at least a template, a surfactant, a silicon source and a catalyst is polymerized to obtain a prepolymerized product with a core-shell structure;
[0017] Furthermore, the reaction system obtained by the polymerization reaction is aged, and the pH value of the reaction system is adjusted to 2-6, and then separated and calcined to obtain small-particle hollow nano-silicon dioxide.
[0018] In some preferred embodiments, the preparation method specifically includes: mixing the template, the catalyst and the mixed solvent, then adding the surfactant and the silicon source to form the mixed reaction system, and performing a polymerization reaction at 20 to 60° C. (for example, 40° C.) to obtain a prepolymer product of a core-shell structure.
[0019] Further, the catalyst includes aqueous ammonia, but is not limited thereto.
[0020] Further, the template includes PS and / or modified PS, but is not limited thereto, and the modified PS is obtained by surface-modifying PS using an active agent. The PS can be purchased or prepared by itself.
[0021] Furthermore, the particle size of the PS is 30-50 nm.
[0022] Furthermore, the mixed solvent includes isopropanol, ethanol and water.
[0023] Furthermore, the mixed solvent also includes methanol.
[0024] Furthermore, the volume ratio of isopropanol, ethanol and water in the mixed solvent is 1-15:1:20:1-25, and is particularly preferably 5-15:5-18:10-25, such as 10:12:15.
[0025] Further, the surfactant includes any one or more combinations of cetyltrimethylammonium bromide (CTAB), cetyltrimethylammonium chloride, and ethylenediamine, but is not limited thereto.
[0026] Further, the silicon source includes any one or more combinations of tetramethoxysilane, tetraethoxysilane, a silane coupling agent, and sodium silicate, but is not limited thereto.
[0027] Furthermore, the silicon source is tetraethoxysilane.
[0028] Furthermore, the pH value of the mixed reaction system is 8-9, for example, the pH value is 9.
[0029] Furthermore, the polymerization reaction time is 8 to 12 hours, for example 12 hours.
[0030] Furthermore, the usage ratio of the mixed solvent, catalyst, template, surfactant and silicon source is 20-45 ml: 0.3-2 ml: 0.03-2 g: 0.05-0.5 g: 0.1-4 g, for example 37 mL: 1 mL: 0.075 g: 0.25 g: 0.5 g.
[0031] In some preferred embodiments, the preparation method specifically comprises:
[0032] The reaction system obtained by the polymerization reaction is aged at room temperature (e.g., 25° C.), and the pH value of the reaction system is adjusted to 2 to 6 using an acidic substance, followed by centrifugation, washing, and drying.
[0033] And, the product obtained by the drying treatment is calcined at 350-750° C. (for example, 550° C.) to obtain small-particle hollow nano-silica.
[0034] Furthermore, the acidic substance includes any one or more combinations of hydrochloric acid, acetic acid, and oxalic acid, but is not limited thereto.
[0035] Furthermore, the preparation method specifically includes: washing the wet material obtained by centrifugal treatment with ethanol and water.
[0036] Furthermore, the aging treatment time is 48 to 200 hours, for example 48 hours.
[0037] Furthermore, the calcination treatment time is 2 to 4.5 hours, for example 3 hours.
[0038] The first step of preparing the hollow nano-silica material in the present invention is a synthesis reaction. The silica material is synthesized by a template method. The material reagents used are pure water, anhydrous ethanol, methanol (a small amount of methanol can be used to reduce the polarity of the system), isopropanol, and ammonia. A template agent is introduced, and tetramethoxysilane, tetraethoxysilane, a silane coupling agent, and sodium silicate are used as silicon sources, preferably tetraethoxysilane. A specific formula and process are designed for polymerization; a prepolymer is obtained to generate a prepolymer product with a core-shell structure. The currently obtained system is a transparent to slightly blue or white liquid. It is difficult to obtain a precipitate by centrifugation when the particle size is less than 100nm, which is the main factor that the current small-particle material is difficult to achieve. The present invention adopts a reverse acidification method, that is, the alkaline prepolymer system is acidified, and the pH value is adjusted to between 2 and 6, so that the small particle material in the system is precipitated, so that the target wet material can be obtained by centrifugation, and then a drying and template removal process is performed in a step to obtain a small-particle hollow nano-silica material.
[0039] Another aspect of the embodiments of the present invention further provides small-particle hollow nano-silica prepared by the aforementioned preparation method.
[0040] In some preferred embodiments, the particle size of the small-particle hollow nano-silica is 30 to 100 nm.
[0041] Furthermore, the particle size of the small-particle hollow nano-silica is 40 to 80 nm.
[0042] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0043] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0044] Example 1
[0045] Use 10ml isopropanol, 12ml ethanol and 15ml ultrapure water as a mixed solvent, use modified PS as a template, add 1ml ammonia water, mix thoroughly for fifteen minutes, add 0.025g CTAB and stir to dissolve, slowly drop 0.5g TEOS, continue to react to obtain a prepolymer, age for 48 hours, then drop hydrochloric acid to adjust the pH value to 3, obtain a white flocculent precipitate, use a high-speed centrifuge to centrifuge to obtain a wet material, wash it three times with ethanol and pure water respectively, put it in an oven to dry, move it into a crucible, and calcine it at 550℃ in a muffle furnace for 3h to obtain a white powder. Scanning by TEM electron microscope Figure 1-Figure 2 As shown, the product is hollow nano-silica with a size between 40 and 60 nm.
[0046] Example 2
[0047] 15ml isopropanol, 10ml ethanol and 10ml ultrapure water were used as mixed solvents, modified PS was used as template, 1ml ammonia water was added, and the mixture was fully mixed for 15 minutes. 0.04g CTAB was added and fully stirred to dissolve. 0.5g tetraethoxysilane was slowly added, and the reaction was continued to obtain a prepolymer, which was aged for 48 hours. Then hydrochloric acid was added to adjust the pH value to 3 to obtain a white flocculent precipitate. The wet material was centrifuged using a high-speed centrifuge, and washed three times with ethanol and pure water respectively, placed in an oven to dry, moved into a crucible, and calcined at 550℃ in a muffle furnace for 3h to obtain a white powder. TEM scanning showed that the product was hollow nano-silica with different shell thicknesses and a wide particle size distribution.
[0048] Example 3
[0049] 10ml isopropanol, 12ml ethanol and 15ml ultrapure water were used as mixed solvents, modified PS was used as template, 0.5ml ammonia water was added, and the mixture was fully mixed for 15 minutes. 0.05g CTAB was added and fully stirred to dissolve. 1.2g sodium silicate was slowly added, and the reaction was continued to obtain a prepolymer, which was aged for 48 hours. Then hydrochloric acid was added to adjust the pH value to 3 to obtain a white flocculent precipitate. The wet material was centrifuged using a high-speed centrifuge, and washed three times with ethanol and pure water respectively, placed in an oven to dry, moved into a crucible, and calcined at 750℃ in a muffle furnace for 2h to obtain a white powder. Through TEM electron microscope scanning, it can be seen that the product is hollow nano-silica, the shell layer is significantly thickened, and the size is between 30 and 100nm.
[0050] Example 4
[0051] 15ml isopropanol, 10ml ethanol and 10ml ultrapure water were used as mixed solvents, modified PS was used as template, 0.5ml ammonia water was added, and the mixture was fully mixed for 15 minutes. 0.1g hexadecyl ammonium bromide was added and stirred to dissolve. 1.2g TEOS was slowly added and continued to react to obtain a prepolymer, which was aged for 48 hours. Then hydrochloric acid was added to adjust the pH value to 3 to obtain a white flocculent precipitate. The wet material was centrifuged using a high-speed centrifuge, and washed three times with ethanol and pure water respectively. It was placed in an oven to dry and moved into a crucible. The product was calcined at 550℃ in a muffle furnace for 3h to obtain a white powder. Through TEM scanning, it can be seen that the product is hollow nano-silica, the shell layer is significantly thickened, the aggregation is obviously broken, and the size is between 30 and 100nm.
[0052] Comparative Example 1
[0053] The method is the same as Example 1, except that the pH value is not adjusted after aging, and no product can be obtained by subsequent centrifugation.
[0054] 10 ml of isopropanol, 12 ml of ethanol and 15 ml of ultrapure water were used as a mixed solvent, modified PS was used as a template, 1 ml of ammonia water was added, and the mixture was fully mixed for fifteen minutes. 0.025 g of CTAB was added and fully stirred to dissolve. 0.5 g of TEOS was slowly added dropwise, and the reaction was continued to obtain a prepolymer. The prepolymer was aged for 48 hours. No precipitate could be obtained by centrifugation in a high-speed centrifuge, and the target product was not obtained.
[0055] Comparative Example 2
[0056] The method is the same as in Example 1, except that: after aging, hydrochloric acid is used to adjust the pH value to 1;
[0057] Use 10ml isopropanol, 12ml ethanol and 15ml ultrapure water as a mixed solvent, use modified PS as a template, add 1ml ammonia water, mix thoroughly for fifteen minutes, add 0.025g CTAB and stir to dissolve, slowly add 0.5g TEOS, continue to react to obtain a prepolymer, age for 48 hours, then add hydrochloric acid to adjust the pH value to 1, and obtain a white flocculent precipitate. Use a high-speed centrifuge to centrifuge to obtain a wet material, wash it three times with ethanol and pure water respectively, put it into an oven to dry, move it into a crucible, and calcine it in a muffle furnace at 550°C for 3h to obtain a white powder. The product is aggregated silica with an amorphous structure.
[0058] Comparative Example 3
[0059] The method is the same as in Example 1, except that: after aging, hydrochloric acid is used to adjust the pH value to 7;
[0060] 10 ml of isopropanol, 12 ml of ethanol and 15 ml of ultrapure water were used as a mixed solvent, modified PS was used as a template, 1 ml of ammonia water was added, and the mixture was fully mixed for fifteen minutes. 0.025 g of CTAB was added and fully stirred to dissolve. 0.5 g of TEOS was slowly added dropwise, and the reaction was continued to obtain a prepolymer. The prepolymer was aged for 48 hours, and then hydrochloric acid was added dropwise to adjust the pH value to 7. No precipitate was obtained, and no product was obtained by centrifugation using a high-speed centrifuge.
[0061] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0062] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing small-particle hollow nano-silica, characterized in that: include: A mixed reaction system containing at least a template, a surfactant, a silicon source and a catalyst is polymerized to obtain a prepolymerized product with a core-shell structure; Furthermore, the reaction system obtained by the polymerization reaction is subjected to aging treatment, and the pH value of the reaction system is adjusted to 2-6, and then separated and calcined to obtain small-particle hollow nano-silicon dioxide.
2. The preparation method according to claim 1, characterized in that: Specifically include: The template, the catalyst and the mixed solvent are mixed, and then a surfactant and a silicon source are added to form the mixed reaction system, and a polymerization reaction is carried out at 20 to 60° C. to obtain a prepolymer product with a core-shell structure.
3. The preparation method according to claim 2, characterized in that: The catalyst includes aqueous ammonia; And / or, the template comprises PS and / or modified PS; preferably, the particle size of the PS is 30 to 50 nm; And / or, the mixed solvent includes isopropanol, ethanol and water; preferably, the mixed solvent also includes methanol; preferably, the volume ratio of isopropanol, ethanol and water in the mixed solvent is 1-15:1:20:1-25, particularly preferably 5-15:5-18:10-25; And / or, the surfactant includes any one or more combinations of cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, and ethylenediamine; And / or, the silicon source includes any one or more combinations of tetramethoxysilane, tetraethoxysilane, a silane coupling agent, and sodium silicate, preferably tetraethoxysilane.
4. The preparation method according to claim 2, characterized in that: The pH value of the mixed reaction system is 8 to 9; And / or, the polymerization reaction time is 8 to 12 hours; And / or, the usage ratio of the mixed solvent, catalyst, template, surfactant and silicon source is 20-45 ml: 0.3-2 ml: 0.03-2 g: 0.05-0.5 g: 0.1-4 g.
5. The preparation method according to claim 1, characterized in that: Specifically include: The reaction system obtained by the polymerization reaction is aged at room temperature, and the pH value of the reaction system is adjusted to 2-6 by using an acidic substance, and then centrifuged, washed, and dried; And, the product obtained by the drying treatment is calcined at 350-750° C. to obtain small-particle hollow nano-silica.
6. The preparation method according to claim 5, characterized in that: The acidic substance includes any one or more combinations of hydrochloric acid, acetic acid and oxalic acid.
7. The preparation method according to claim 5, characterized in that: Specifically include: The wet material obtained by centrifugal treatment is washed with ethanol and water.
8. The preparation method according to claim 5, characterized in that: The aging treatment time is 48 to 200 hours; and / or the calcination treatment time is 2 to 4.5 hours.
9. The small-particle hollow nano-silica prepared by the preparation method described in any one of claims 1-8.
10. The small-particle hollow nano-silica according to claim 9, characterized in that: The particle size of the small-particle hollow nano-silica is 30 to 100 nm, preferably 40 to 80 nm.
Citation Information
Patent Citations
Silica support material, its application in a polyalkene catalyst, and its preparation process