Method for improving whiteness of sodium sulfate recovered from raffinate wastewater of waste lithium ion battery

By converting aluminum ions into highly activated aluminum hydroxide and using calcium oxide or calcium hydroxide precipitation and activated carbon to deeply remove activated carbon, the problem of insufficient whiteness of sodium sulfate in lithium-ion battery raffinate is solved, and its recycling value is improved. Simplified operation.

CN119080029APending Publication Date: 2024-12-06LONGNAN JINTAIGE COBALT IND CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411199376.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art has insufficient whiteness of sodium sulfate in the recovery of lithium-ion battery raffinate, resulting in low value and troublesome operation of existing removal methods.

Method used

By converting aluminum ions into highly activated aluminum hydroxide, and precipitating some metal ions with calcium oxide or calcium hydroxide, combining activated carbon to deeply remove organic matter, and improving the whiteness of sodium sulfate after MVR evaporation.

Benefits of technology

It effectively improves the whiteness of sodium sulfate in the wastewater of lithium-ion battery raffinate, improves its recycling value, and simplifies the operation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080029A_ABST
    Figure CN119080029A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the whiteness of recovered sodium sulfate in waste lithium ion battery raffinate wastewater, and belongs to the technical field of waste lithium ion battery wastewater recycling. The method comprises the following steps: adding an aluminum salt into waste raffinate of the waste lithium ion battery to obtain a solution containing the aluminum salt; after adjusting the pH value, stirring to obtain a mixed solution; then adding a calcium compound, stirring and filtering to obtain a precipitate I and a filtrate I; adding activated carbon into the filtrate I, stirring and filtering to obtain a precipitate II and filtrate II; evaporating the filtrate II to obtain anhydrous sodium sulfate. According to the method, aluminum ions are converted into high-activity aluminum hydroxide, and organic matters in the raffinate are adsorbed by utilizing the high adsorption performance of the aluminum hydroxide; meanwhile, calcium oxide or calcium hydroxide is added, part of metal ions are precipitated, organic matter in the wastewater is further deeply removed by adding activated carbon, and the whiteness of sodium sulfate obtained after MVR evaporation is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of recycling waste water from waste lithium ion batteries, and in particular to a method for improving the whiteness of sodium sulfate recovered from waste lithium ion battery raffinate waste water. Background Art

[0002] With the rapid development of lithium-ion batteries, lithium-ion batteries have occupied the portable consumer electronics market and are constantly expanding into new energy electric vehicles and other fields. my country has become the world's largest lithium battery producer, consumer and exporter. It is estimated that by 2030, as a large number of automotive power batteries enter the recycling link, China's lithium-ion battery recycling volume will reach 6.028 million tons. In short, power battery recycling is related to safety, pollution, and resource issues, and also affects the sustainable development of new energy vehicles. The development of waste lithium-ion battery resource technology is not only beneficial to environmental protection, but also has great economic benefits.

[0003] Commonly used lithium-ion batteries on the market include lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, nickel-cobalt-manganese ternary and lithium iron phosphate. When recycling and treating waste ternary lithium-ion batteries, sulfuric acid and other acids are generally used to leach valuable metals from electrode materials. The leachate contains metals such as nickel, cobalt, lithium, copper, manganese, aluminum and iron. At present, valuable metals such as nickel, cobalt and manganese are generally recovered from solutions by sodium saponified phosphorus extractants, and the final raffinate contains a large amount of sodium sulfate; these raffinates not only contain a large amount of sodium sulfate, but also contain a large amount of organic extractants, which cannot be discharged directly. MVR is generally used for evaporation. Due to the presence of extractants and other impurity metal ions, the sodium sulfate evaporated and crystallized is not white enough and has a low value.

[0004] The main methods for removing these extractants include static stratification oil separation, air flotation, advanced oxidation, carbon-based material adsorption and resin adsorption, etc. Although they can achieve good results, the operation is cumbersome. Therefore, it is of great significance to develop a low-cost and highly adaptable method for recovering sodium sulfate from waste lithium-ion battery raffinate wastewater to improve the whiteness. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a method for improving the whiteness of sodium sulfate recovered from waste lithium-ion battery raffinate wastewater. The present invention converts aluminum ions into highly active aluminum hydroxide, and uses the high adsorption performance of aluminum hydroxide to adsorb organic matter in the raffinate; at the same time, calcium oxide or calcium hydroxide is added to precipitate part of the metal ions, and then activated carbon is added to further deeply remove organic matter in the wastewater, thereby improving the whiteness of sodium sulfate after MVR evaporation.

[0006] The technical solution of the present invention is as follows:

[0007] The first aspect of the present invention protects a method for improving the whiteness of sodium sulfate recovered from waste lithium ion battery raffinate wastewater, the method being as follows:

[0008] S1: adding aluminum salt to waste lithium-ion battery raffinate waste liquid to obtain an aluminum salt-containing solution;

[0009] S2: Adjust the pH value to 5.5-6.5 and stir to obtain a mixed solution;

[0010] S3: adding a calcium compound to the mixed solution of step S2, stirring, filtering, and obtaining a precipitate I and a filtrate I;

[0011] S4: Add activated carbon to the filtrate I, stir, and filter to obtain precipitate II and filtrate II;

[0012] S5: Evaporate the filtrate II to obtain anhydrous sodium sulfate.

[0013] Furthermore, in step S1, the aluminum salt includes at least one of aluminum sulfate and polyaluminum sulfate.

[0014] Furthermore, in step S1, the concentration of aluminum ions in the aluminum salt-containing solution is 0.5 to 3 g / L.

[0015] Furthermore, in step S1, the content of sodium sulfate in the waste lithium-ion battery raffinate waste liquid is 30-200 g / L, and the COD value is 150-1000 mg / L.

[0016] Furthermore, in step S2, the pH is adjusted by a sodium compound.

[0017] Furthermore, the sodium compound includes at least one of sodium hydroxide, sodium carbonate and sodium bicarbonate.

[0018] Furthermore, in step S2, the stirring speed is 50-600 r / min and the time is 1-3 h.

[0019] Furthermore, in step S3, the calcium compound includes at least one of calcium hydroxide and calcium oxide.

[0020] Furthermore, in step S3, the amount of calcium compound added is 1-5 kg ​​of calcium compound per cubic meter of the mixed solution.

[0021] Furthermore, in step S4, the activated carbon is added at a rate of 100 to 500 g per cubic meter of filtrate I; and in step S5, the evaporation is performed by MVR evaporation.

[0022] The beneficial technical effects of the present invention are:

[0023] The present invention converts aluminum ions into highly active aluminum hydroxide by first adding aluminum salt and then adjusting pH with sodium, and then uses the high adsorption performance of aluminum hydroxide to adsorb organic matter in the raffinate. At the same time, in order to improve the filtering performance of aluminum hydroxide, calcium oxide or calcium hydroxide is added to precipitate part of the metal ions, and then activated carbon is added to further deeply remove organic matter in the wastewater, thereby improving the whiteness of sodium sulfate after MVR evaporation. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the method of the present invention. DETAILED DESCRIPTION

[0025] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.

[0026] Wastewater from waste lithium-ion battery raffinate contains a large amount of sodium sulfate, which can be recycled to achieve resource reuse. However, existing methods for recycling sodium sulfate have different problems, such as insufficient whiteness of the recycled sodium sulfate, which reduces its recycling value. Therefore, this invention proposes a method for increasing the whiteness of sodium sulfate to increase its value.

[0027] The method for recovering sodium sulfate from waste lithium ion battery raffinate wastewater to improve whiteness of the waste lithium ion battery according to the present invention comprises the following steps:

[0028] S1: adding aluminum salt to waste lithium-ion battery raffinate waste liquid to obtain an aluminum salt-containing solution;

[0029] S2: Adjust the pH value to 5.5-6.5 and stir to obtain a mixed solution;

[0030] S3: adding a calcium compound to the mixed solution of step S2, stirring, filtering, and obtaining a precipitate I and a filtrate I;

[0031] S4: Add activated carbon to the filtrate I, stir, and filter to obtain precipitate II and filtrate II;

[0032] S5: Evaporate the filtrate II to obtain anhydrous sodium sulfate.

[0033] In some embodiments, in step S1, the aluminum salt includes at least one of aluminum sulfate and polyaluminum sulfate.

[0034] In some embodiments, in step S1, the concentration of aluminum ions in the solution containing aluminum salt is 0.5 to 3 g / L.

[0035] In some embodiments, in step S1, the content of sodium sulfate in the waste lithium-ion battery raffinate waste liquid is 30-200 g / L, including but not limited to 30 g / L, 50 g / L, 100 g / L, 150 g / L, 200 g / L, and the COD value is 150-1000 mg / L.

[0036] It can be understood that the present invention converts aluminum ions into highly active aluminum hydroxide by first adding aluminum salt and then adjusting the pH with sodium salt, and then utilizes the high adsorption of aluminum hydroxide to not only remove the sodium-saponified phosphorus extractant, but also remove other organic matter in the extract at the same time. The present invention utilizes the high adsorption of aluminum hydroxide to not only remove the sodium-saponified phosphorus extractant, but also remove other organic matter in the extract at the same time.

[0037] In some embodiments, in step S2, the pH is adjusted by a sodium compound.

[0038] In some embodiments, the sodium compound includes at least one of sodium hydroxide, sodium carbonate, and sodium bicarbonate.

[0039] In some embodiments, in step S2, the stirring speed is 50-600 r / min, and the time is 1-3 h. The stirring speed includes but is not limited to 50 r / min, 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min; the time includes but is not limited to 1 h, 2 h, 3 h.

[0040] In some embodiments, in step S3, the calcium compound includes at least one of calcium hydroxide and calcium oxide.

[0041] In some embodiments, in step S3, the amount of calcium compound added is 1-5 kg ​​of calcium compound per cubic meter of mixed solution, including but not limited to 1 kg, 2 kg, 3 kg, 4 kg, and 5 kg.

[0042] It is understandable that the addition of calcium oxide or calcium hydroxide can precipitate some metal ions, such as nickel, cobalt, manganese, etc., and improve the filtration performance of aluminum hydroxide, thereby achieving the precipitation and removal of other metal ions.

[0043] In some embodiments, in step S4, the activated carbon is added at a rate of 100-500 g per cubic meter of filtrate I, including but not limited to 100 g, 200 g, 300 g, 400 g, and 500 g; in step S5, the evaporation is performed by MVR evaporation.

[0044] The present invention will be further described below by way of examples.

[0045] Example 1

[0046] A method for recovering sodium sulfate from waste lithium-ion battery raffinate wastewater to improve whiteness comprises the following steps:

[0047] Prepare raffinate wastewater: Take the raffinate wastewater of a waste lithium-ion battery containing 150g / L of sodium sulfate and 361mg / L of COD as the experimental wastewater.

[0048] Based on the aluminum ion concentration of 1g / L in the solution, aluminum sulfate was weighed and added to the waste lithium-ion battery raffinate wastewater; sodium hydroxide was then added to adjust the pH value of the raffinate to 6.0, and stirred for 3 hours; then 1kg of calcium oxide was added per cubic meter of solution, and the calcium oxide was added to the above solution and stirred for 1 hour. The filtration was very rapid, and a precipitate and filtrate 1 were obtained by filtration, and the COD of filtrate 1 was 50mg / L.

[0049] Activated carbon was added to filtrate 1 at a rate of 200 g / m3, and the mixture was stirred for 2 hours and then filtered. The COD of filtrate 2 was 17 mg / L. The MVR of the filtrate was evaporated to 20% of the volume to obtain sodium sulfate, and the whiteness of the sodium sulfate was 91%.

[0050] Example 2

[0051] A method for recovering sodium sulfate from waste lithium-ion battery raffinate wastewater to improve whiteness comprises the following steps:

[0052] Prepare raffinate wastewater: Take the raffinate wastewater of a waste lithium-ion battery containing 150g / L of sodium sulfate and 361mg / L of COD as the experimental wastewater.

[0053] Based on the aluminum ion concentration of 3 g / L in the solution, aluminum sulfate was weighed and added to the waste lithium-ion battery raffinate wastewater; sodium carbonate was added to adjust the pH value of the raffinate to 5.8, and stirred for 1 hour; 5 kg of calcium hydroxide was added per cubic meter of solution, and stirred for 3 hours. The filtration was very rapid, and a precipitate and filtrate 1 were obtained by filtration. The COD of filtrate 1 was 47 mg / L.

[0054] Activated carbon was added to filtrate 1 at a rate of 500 g / m3, and the mixture was stirred for 2 hours and then filtered. The COD of filtrate 2 was 15 mg / L. The MVR of the filtrate was evaporated to 20% of the volume to obtain sodium sulfate, and the whiteness of the sodium sulfate was 92%.

[0055] Example 3

[0056] A method for recovering sodium sulfate from waste lithium-ion battery raffinate wastewater to improve whiteness comprises the following steps:

[0057] Prepare raffinate wastewater: The raffinate wastewater from a waste lithium-ion battery contains 30g / L of sodium sulfate and 210mg / L of COD, which is used for experimental wastewater.

[0058] Based on the aluminum ion concentration of 0.5 g / L in the solution, weigh polyaluminum sulfate and add it to the waste water of the raffinate of used lithium-ion batteries; add sodium bicarbonate to adjust the pH value of the raffinate to 5.6, and stir for 3 hours; add 2 kg of calcium oxide per cubic meter of solution, stir for 2 hours, and filter very quickly to obtain a precipitate and filtrate 1, and the COD of filtrate 1 is 71 mg / L.

[0059] Activated carbon was added to filtrate 1 at 100 g / m3, and the mixture was stirred for 1 hour and then filtered. The COD of filtrate 2 was 55 mg / L. The MVR of the filtrate was evaporated to 10% of the volume to obtain sodium sulfate, and the whiteness of the sodium sulfate was 85%.

[0060] Example 4

[0061] A method for recovering sodium sulfate from waste lithium-ion battery raffinate wastewater to improve whiteness comprises the following steps:

[0062] Prepare raffinate wastewater: The raffinate wastewater from a waste lithium-ion battery contains 190g / L of sodium sulfate and 470mg / L of COD, which is used for experimental wastewater.

[0063] According to the aluminum ion concentration of 1.5g / L in the solution, a mixture of polyaluminum sulfate and aluminum sulfate (the mass ratio of polyaluminum sulfate to aluminum sulfate is 2:1) is weighed and added into the waste water of the raffinate of the waste lithium-ion battery; a mixture of sodium hydroxide and sodium carbonate (the mass ratio of sodium hydroxide to sodium carbonate is 1:1) is added to adjust the pH value of the raffinate to 6.5, and the mixture is stirred for 2 hours; 1Kg of calcium hydroxide is added to the above solution per cubic meter of solution, and the mixture is stirred for 3 hours. The filtration is very rapid, and a precipitate and a filtrate 1 are obtained by filtration, and the COD of the filtrate 1 is 52mg / L.

[0064] Activated carbon was added to filtrate 1 at a rate of 400 g / m3, and the mixture was stirred for 3 hours and then filtered. The COD of filtrate 2 was 19 mg / L. The MVR of the filtrate was evaporated to 30% of the volume to obtain sodium sulfate, and the whiteness of the sodium sulfate was 90%.

[0065] Comparative Example 1

[0066] A method for recovering sodium sulfate from waste lithium-ion battery raffinate wastewater to improve whiteness comprises the following steps:

[0067] Prepare raffinate wastewater: The raffinate wastewater of a waste lithium-ion battery contains 150g / L of sodium sulfate and 361mg / L of COD, and the wastewater for the experiment is obtained.

[0068] Activated carbon was added at 200 g / m3, and the mixture was stirred for 2 hours and then filtered. The COD of the filtrate was 282 mg / L. The MVR of the filtrate was evaporated to 20% of the total volume to obtain sodium sulfate. The whiteness of the sodium sulfate was 65%.

[0069] Comparative Example 2

[0070] A method for recovering sodium sulfate from waste lithium-ion battery raffinate wastewater to improve whiteness comprises the following steps:

[0071] Prepare raffinate wastewater: The raffinate wastewater of a waste lithium-ion battery contains 150g / L of sodium sulfate and 361mg / L of COD, and the wastewater for the experiment is obtained.

[0072] Based on the aluminum ion concentration of 1 g / L in the solution, aluminum sulfate was weighed and added to the waste lithium-ion battery raffinate wastewater; sodium hydroxide was added to adjust the pH value of the raffinate to 5.0, and the mixture was stirred for 3 hours. If filtering was difficult, a precipitate and filtrate 1 were obtained by filtration, and the COD of filtrate 1 was 180 mg / L.

[0073] Activated carbon was added to filtrate 1 at a rate of 200 g / m3, and the mixture was stirred for 2 hours and then filtered. The COD of filtrate 2 was 130 mg / L. The MVR of the filtrate was evaporated to 20% of the volume to obtain sodium sulfate, and the whiteness of the sodium sulfate was 71%.

[0074] Comparative Example 3

[0075] A method for recovering sodium sulfate from waste lithium-ion battery raffinate wastewater to improve whiteness comprises the following steps:

[0076] Prepare raffinate wastewater: The raffinate wastewater of a waste lithium-ion battery contains 150g / L of sodium sulfate and 361mg / L of COD, and the wastewater for the experiment is obtained.

[0077] Based on the aluminum ion concentration of 1 g / L in the solution, aluminum sulfate was weighed and added to the waste water of the raffinate of the used lithium-ion battery; sodium hydroxide was added to adjust the pH value of the raffinate to 7.0, and the solution was stirred for 3 hours; 2 kg of calcium oxide was added per cubic meter of solution, and the solution was stirred for 2 hours, and the solution was filtered very quickly to obtain a precipitate and a filtrate 1; the precipitate and the filtrate 1 were obtained by filtration, and the COD of the filtrate 1 was 170 mg / L.

[0078] Activated carbon was added to filtrate 1 at a rate of 200 g / m3, and the mixture was stirred for 2 hours and then filtered. The COD of filtrate 2 was 125 mg / L. The MVR of the filtrate was evaporated to 20% of the volume to obtain sodium sulfate, and the whiteness of the sodium sulfate was 73%.

[0079] The above is only a preferred embodiment of the present invention, and the present invention is not limited to the above embodiments. It is understood that other improvements and changes directly derived or associated by those skilled in the art without departing from the spirit and concept of the present invention should be considered to be included in the protection scope of the present invention.

Claims

1. A method for improving the whiteness of sodium sulfate recovered from waste lithium-ion battery raffinate wastewater, characterized in that: The method is as follows: S1: adding aluminum salt to waste lithium-ion battery raffinate waste liquid to obtain an aluminum salt-containing solution; S2: Adjust the pH value to 5.5-6.5 and stir to obtain a mixed solution; S3: adding a calcium compound to the mixed solution of step S2, stirring, filtering, and obtaining a precipitate I and a filtrate I; S4: Add activated carbon to the filtrate I, stir, and filter to obtain precipitate II and filtrate II; S5: Evaporate the filtrate II to obtain anhydrous sodium sulfate.

2. The method according to claim 1, characterized in that: In step S1, the aluminum salt includes at least one of aluminum sulfate and polyaluminum sulfate.

3. The method according to claim 1, characterized in that In step S1, the concentration of aluminum ions in the aluminum salt-containing solution is 0.5 to 3 g / L.

4. The method according to claim 1, characterized in that In step S1, the content of sodium sulfate in the waste lithium-ion battery raffinate waste liquid is 30-200 g / L, and the COD value is 150-1000 mg / L.

5. The method according to claim 1, characterized in that: In step S2, the pH is adjusted by a sodium compound.

6. The method according to claim 5, characterized in that The sodium compound includes at least one of sodium hydroxide, sodium carbonate and sodium bicarbonate.

7. The method according to claim 1, characterized in that In step S2, the stirring speed is 50-600 r / min and the time is 1-3 h.

8. The method according to claim 1, characterized in that In step S3, the calcium compound includes at least one of calcium hydroxide and calcium oxide.

9. The method according to claim 1, characterized in that: In step S3, the calcium compound is added in an amount of 1-5 kg ​​per cubic meter of the mixed solution.

10. The method according to claim 1, characterized in that In step S4, the activated carbon is added at a rate of 100 to 500 g per cubic meter of filtrate I; and in step S5, the evaporation is performed by MVR evaporation.

Citation Information

Cited By

  • Deep purification method of industrial solid waste sodium sulfate

    CN122646875A