Preparation method for synthesizing high-entropy alloy oxide by ion layer epitaxy method

The ion layer epitaxial method uses liquid-air interface templates and surfactants to synthesize high-entropy oxides at low temperatures, solving the problems of complex and high energy consumption of high-entropy alloy material preparation equipment, and achieving low-temperature and efficient synthesis and material structure optimization.

CN119080079APending Publication Date: 2024-12-06NORTHEAST FORESTRY UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411070344.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The preparation of high-entropy alloy materials requires complex equipment and high-temperature reaction conditions, resulting in high energy consumption and low efficiency. The existing hydrothermal methods are also difficult to solve the yield and adjustability problems.

Method used

The ion layer epitaxial method is used to use the insoluble liquid-air interface as a soft template to attract charges with metal ions on the water surface through an anion/cationic surfactant to form high-entropy oxides, and the reaction conditions are controlled to achieve low-temperature synthesis.

Benefits of technology

Efficiently synthesize different types and morphologies of high-entropy oxides under low temperature conditions, reduce energy consumption, simplify equipment requirements, improve synthesis efficiency, and facilitate observation and optimization of material structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080079A_ABST
    Figure CN119080079A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method for synthesizing a high-entropy alloy oxide by an ion layer epitaxy method. The preparation method comprises the following steps: step 1, preparing a surfactant; 2, preparing a metal salt precursor solution; 3, preparing a urea solution; 4, preparing a reaction precursor solution; 5, high-entropy alloy oxide is obtained; and 6, clamping the silicon wafer with the oxide layer by using tweezers, immersing the silicon wafer in the liquid level in a slightly inclined manner, and vertically pulling the silicon wafer backwards to obtain the high-entropy alloy oxide on the silicon wafer. According to the method, the two-dimensional high-entropy oxide can be synthesized under the low-temperature condition, and the conventional ultrahigh temperature of 1200 DEG C or above and rapid cooling treatment are not needed, so that the energy loss required for synthesizing the high-entropy oxide in the past and the danger in the experiment process can be greatly reduced; in the experiment process, common equipment and simplified operation steps are used, a high-temperature reactor, laser, a special cooling device and the like are not needed, and the used observation substrate can be used for multiple times, so that the synthesis process is easier to popularize and apply.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method for synthesizing high entropy alloy oxide by ion layer epitaxy, belonging to the technical field of material processing. Background Art

[0002] Usually, the preparation of high entropy alloys requires specific experimental equipment, and the temperature is often as high as 1200 ° C, which is accompanied by huge energy consumption, and there are also strict requirements for the cooling rate, which is also a limitation for experimental equipment. Although the hydrothermal method can reduce the energy consumption in the preparation process to a certain extent, the yield and subsequent material adjustability are still a challenge for it. In order to solve the above problems, the present invention overcomes the complex equipment requirements for the preparation of high entropy alloy materials, high temperature reaction conditions and the corresponding high energy consumption, long preparation time, low efficiency and other shortcomings, and provides a method for low-temperature synthesis of two-dimensional high entropy oxide materials by self-assembled ion layer epitaxy. The method uses an immiscible liquid-air interface as a soft template, and uses anion / cation surfactants on the water surface to attract metal cations / anions in the solution to form different high entropy oxides. By changing the type of metal precursor solution, the change of the molar amount used, and the selection of different reaction temperatures, reaction times and different surfactants, a wide range of metal elements can be selected and the structure optimized. Using this invention, high entropy oxides of different types and morphologies can be synthesized over a large area at low cost and high efficiency under low temperature conditions. Summary of the invention

[0003] The invention solves the problem of providing a method for preparing a high entropy alloy material with simple equipment requirements, low energy consumption and high efficiency, and further proposes a method for preparing a high entropy alloy oxide by synthesizing it by an ion layer epitaxy method.

[0004] The technical solution adopted by the present invention to solve the above problems is: the present invention proposes a preparation method of high entropy alloy oxide synthesized by ion layer epitaxy, comprising:

[0005] Step 1: prepare surfactant;

[0006] Step 2: preparing a metal salt precursor solution;

[0007] Step 3: prepare urea solution;

[0008] Step 4: According to the type of surfactant, selectively use a pipette to suck the prepared metal salt precursor solution and the prepared urea solution in turn, put them into a 15mL glass bottle, and add 5mL of deionized water to the glass bottle; according to the type of solution in the glass bottle, use a pipette to suck the corresponding surfactant, drop it on the surface of the solution in the glass bottle, open the bottle mouth and let it stand for 10 minutes, wait for the surfactant solvent to evaporate, and then tighten the bottle cap to obtain a reaction precursor solution;

[0009] Step 5: If an anionic surfactant is added dropwise on the surface of the solution in the glass bottle, the glass bottle is placed in a forced air drying oven at 80°C, and the high entropy alloy oxide is obtained at the water-air two-phase interface after being kept warm for 100min-2.5h; if a cationic surfactant is added dropwise on the surface of the solution in the glass bottle, the reaction is carried out in a cool room temperature environment for 6-7.5h to obtain a high entropy alloy oxide at the water-air two-phase interface;

[0010] Step 6: Use tweezers to pick up the silicon wafer with an oxide layer, immerse it in the liquid at a slight angle, and then pull it back vertically to obtain a high entropy alloy oxide on the silicon wafer.

[0011] In step 6, the silicon wafer must be tilted at a certain angle and subsequently lifted and pulled to avoid failure of stacking and retrieval of the two-dimensional material, which would make subsequent morphology observation difficult.

[0012] Optionally, in step 1, the surfactant is prepared by a surfactant solution and a solvent, and the surfactant includes a cationic surfactant and an anionic surfactant;

[0013] Surfactant solutions include, but are not limited to, stearic acid, oleylamine, sodium lauryl sulfate, sodium oleyl sulfate, and sodium dodecylbenzene sulfonate;

[0014] Solvents include, but are not limited to, dichloromethane and chloroform.

[0015] Optionally, the steps of preparing the anionic surfactant include:

[0016] 2.56 g of stearic acid and 10 mL of dichloromethane were mixed into a 0.9 M solution, and the mixture was fully mixed to form a clear and transparent solution. The anionic surfactant was obtained after standing for 24 hours.

[0017] Optionally, the steps of preparing the cationic surfactant include:

[0018] Oleylamine and dichloromethane in a volume ratio of 1:500 were prepared into a solution with a volume of 10 mL, and the solution was fully mixed to form a clear and transparent solution. The solution was allowed to stand for 24 hours to obtain a cationic surfactant.

[0019] Since the configured anionic surfactants and cationic surfactants are both volatile, they should be stored in a cool, dark place, and the glass bottles storing the surfactant solutions should be covered with headspace caps to prevent toxic gas pollution caused by the volatilization of the solvent in the surfactant and deviation in the concentration of the surfactant solution.

[0020] Optionally, the step of preparing the metal precursor solution in step 2 includes:

[0021] Use an electronic balance to weigh Pt salt, Ni salt, Fe salt, Co salt, Zn salt, Cu salt, Al salt and Mo salt in a mass ratio of 0.002g:0.0435g:0.019g:0.0436g:0.0271g:0.024g:0.037g:0.135g, put the weighed Pt salt, Ni salt, Fe salt, Co salt, Zn salt, Cu salt, Al salt and Mo salt into a glass bottle, use a pipette to transfer 34μL of Mn salt solution dropwise into the glass bottle, add 5mL of deionized water to the glass bottle, fully dissolve and mix, and then stir magnetically for 10min to obtain a metal salt precursor solution with a total volume of 5mL;

[0022] The metal salt solution includes, but is not limited to, solutions of chloroplatinic acid hexahydrate, nickel nitrate hexahydrate, ferrous chloride, cobalt nitrate hexahydrate, zinc nitrate hexahydrate, manganese nitrate solution, aluminum nitrate nonahydrate, copper nitrate hexahydrate, and ammonium molybdate.

[0023] Among them, ferrous chloride solution is easily oxidized and needs to be reconfigured each time it is used to ensure the repeatability and success rate of the experiment.

[0024] Optionally, the step of preparing the urea solution in step 3 includes:

[0025] Weigh 0.018 g of urea with an electronic balance, put it into a 15 mL glass bottle, add 10 mL of deionized water to the glass bottle to dissolve it, and mix it thoroughly to obtain a urea solution;

[0026] The urea solution is used to adjust the alkaline environment of the solution and can be replaced by one of hexamethylenetetramine and sodium hydroxide.

[0027] Optionally, during the preparation of the reaction precursor solution in step 4, if the type of surfactant added is a positive surfactant, 5 μL of the prepared metal salt precursor solution including ammonium molybdate is taken with a pipette and placed in a 15 mL glass bottle, 5 mL of deionized water is added to the glass bottle, and after standing for 30 minutes, 6-10 μL of cationic surfactant is taken with a pipette and dropped on the surface of the solution in the bottle, the bottle mouth is opened and stood for 10 minutes, and after the surfactant solvent is evaporated, the bottle cap is tightened;

[0028] If the added surfactant type is anionic surfactant, use a pipette to successively pipette 5 μL of the prepared metal salt precursor solution and 10 μL of urea solution, add 5 mL of deionized water to the glass bottle, let the metal salt precursor solution and urea solution stand in the glass bottle for 30 minutes, then use a pipette to pipette 6-10 μL of anionic surfactant and drop it on the surface of the solution in the bottle, open the bottle mouth and let it stand for 10 minutes, wait for the surfactant solvent to evaporate, and then tighten the bottle cap.

[0029] In step 4, the deionized water must be added smoothly without splashing onto the wall of the glass bottle, so that the subsequent addition of surfactant will not contaminate the bottle wall and fail to add the correct amount of surfactant onto the solution surface.

[0030] The purpose of standing for 30 minutes is to allow the metal salt solution to be fully mixed and evenly mixed. Do not use a magnetic stirring device to avoid solution contamination and solution wall adhesion, which may cause experimental errors or experimental failure.

[0031] There are two methods for adding surfactants. One is to add it slowly along a small section of the bottle wall close to the liquid surface to cover the surface. The other is to add it slowly along the vertical bottle wall on one side of the liquid surface.

[0032] Optionally, a substrate is used for real-time observation during the reaction process of steps 4-6, and the substrate includes but is not limited to silicon wafer, FTO glass and ITO glass.

[0033] The beneficial effects of the present invention are:

[0034] 1. The present invention can synthesize two-dimensional high-entropy oxides under low temperature conditions, without the need for conventional ultra-high temperatures of 1200°C or above and subsequent rapid cooling treatments, which can greatly reduce the energy loss required for the previous synthesis of high-entropy oxides and the dangers in the experimental process.

[0035] 2. Due to the flexibility of the experimental process, the present invention makes it easier to observe the morphology, structure and growth trend of high entropy oxides, and can be used to study whether the selected metal analogy has a synthesis trend. If there is no obvious synthesis trend, it can avoid unnecessary waste of resources and save time costs.

[0036] 3. The present invention can explore the synthesis of different high entropy oxides by changing or replacing different metal salt precursors, changing the reaction temperature, reaction time, surfactant type, surfactant dosage, etc., and has unique advantages in adjusting the microstructure of high entropy oxides and optimizing their uses.

[0037] 4. Although a small amount of precious metals was used in this experiment, due to its extremely small amount and the extremely limited amount of metal salts used overall, the utilization rate of these materials is very high. A small amount of metal salts can be used for a large number of synthesis reactions. Therefore, many parallel experiments can be carried out without considering issues such as reagent waste, which can enable more efficient and convenient large-scale synthesis of high-entropy oxides.

[0038] 5. In the experimental process of the present invention, common equipment and simplified operation steps are used, and no high-temperature reactor, laser, special cooling device, etc. are required. The observation substrate used can be used multiple times, making the synthesis process easier to promote and apply. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A flow chart of a method for preparing high entropy alloy oxide by ion layer epitaxy provided by the present invention;

[0040] Figure 2 This is a scanning electron microscope image of the prepared (FeNiZnMo)O provided by the present invention;

[0041] Figure 3 This is a scanning electron microscope image of the prepared (FeNiCuMo)O provided by the present invention;

[0042] Figure 4 This is a scanning electron microscope image of the prepared (FeNiCoCuMo)O provided by the present invention. Example

[0043] Example 1

[0044] like Figure 1 As shown, the steps of the method for preparing high entropy alloy oxide by ion layer epitaxy described in this embodiment include:

[0045] S1: Preparation of precursor solution: Take 0.0435g nickel nitrate hexahydrate, 0.019g ferrous chloride, 0.0436g cobalt nitrate hexahydrate, 34μL manganese nitrate solution and 0.018g urea, prepare 10mM nickel nitrate, ferrous chloride, cobalt nitrate, manganese nitrate and 20mM urea solutions in 15mL glass bottles respectively, and shake well to dissolve.

[0046] S2: Preparation of anionic surfactant: 2.56 g of stearic acid was dissolved in 10 mL of dichloromethane, and after fully dissolved, it was allowed to stand at room temperature for 24 h.

[0047] S3: Use a pipette to transfer 5 μL of ferrous chloride solution, 5 μL of nickel nitrate solution, 5 μL of cobalt nitrate solution, and 5 μL of manganese nitrate solution from the various metal salt solutions prepared in step 1 into a 15 mL glass bottle. Use a pipette to transfer 10 μL of urea solution, add 5 mL of deionized water to the bottle, and let it stand for 30 minutes.

[0048] S4: Take 8 μL of the anionic surfactant prepared in S2, drop it on the surface of the reaction precursor solution, and leave it in a cool and ventilated place for 10 minutes to allow the dichloromethane to evaporate completely.

[0049] S5: Growth of (FeNiCoMn)O: Tighten the bottle cap, put the prepared reaction precursor solution into a forced air drying oven, and keep it at 80°C for 2h to complete the growth of (FeNiCoMn)O.

[0050] S6: Transfer of (FeNiCoMn)O: Use a silicon wafer with an oxide layer, immerse it slightly at an angle in the liquid, and then pull it back vertically to complete the transfer of (FeNiCoMn)O, and dry it naturally in air for several hours.

[0051] Example 2

[0052] like Figure 1 As shown, the steps of the method for preparing high entropy alloy oxide by ion layer epitaxy described in this embodiment include:

[0053] S1: Preparation of precursor solution: Take 0.0435g nickel nitrate hexahydrate, 0.019g ferrous chloride, 0.0436g cobalt nitrate hexahydrate, 0.0271g zinc nitrate hexahydrate and 0.018g urea, prepare 10mM nickel nitrate, ferrous chloride, cobalt nitrate, zinc nitrate and 20mM urea solutions in 15mL glass bottles respectively, and shake well to dissolve.

[0054] S2: Preparation of anionic surfactant: 2.56 g of stearic acid was dissolved in 10 mL of dichloromethane, and after fully dissolved, it was allowed to stand at room temperature for 24 h.

[0055] S3: Use a pipette to transfer 8 μL of ferrous chloride solution, 6 μL of nickel nitrate solution, 6 μL of cobalt nitrate solution, and 5 μL of zinc nitrate solution from the various metal salt solutions prepared in step 1 into a 15 mL glass bottle. Use a pipette to transfer 15 μL of urea solution, add 5 mL of deionized water to the bottle, and let it stand for 30 minutes.

[0056] S4: Take 6 μL of the anionic surfactant prepared in S2, drop it on the surface of the reaction precursor solution, and leave it in a cool and ventilated place for 10 minutes to allow the dichloromethane to evaporate completely.

[0057] S5: Growth of (FeNiCoZn)O: Tighten the bottle cap, place the prepared reaction precursor solution into a forced air drying oven, and keep it at 80°C for 2.5h to complete the growth of (FeNiCoZn)O.

[0058] S6: Transfer of (FeNiCoZn)O: Use a silicon wafer with an oxide layer, immerse it slightly at an angle in the liquid, then pull it back vertically to complete the transfer of (FeNiCoZn)O, and dry it naturally in air for several hours.

[0059] Example 3

[0060] like Figure 1 As shown, the steps of the method for preparing high entropy alloy oxide by ion layer epitaxy described in this embodiment include:

[0061] S1: Preparation of precursor solution: Take 0.0435g nickel nitrate hexahydrate, 0.019g ferrous chloride, 0.0436g cobalt nitrate hexahydrate, and 0.185g ammonium molybdate, and prepare 10mM nickel nitrate, ferrous chloride, cobalt nitrate, and ammonium molybdate solutions in 15mL glass bottles, respectively, and shake well to dissolve.

[0062] S2: Preparation of cationic surfactant: Dissolve 20 μL of oleylamine in 10 mL of chloroform, and let stand at room temperature for 24 h after it is fully dissolved.

[0063] S3: Use a pipette to transfer 10 μL of ferrous chloride solution, 10 μL of nickel nitrate solution, 10 μL of cobalt nitrate solution and 10 μL of ammonium molybdate solution prepared in step 1 into a 15 mL glass bottle. Add 5 mL of deionized water to the bottle, stir the precursor solution with a low-intensity magnetic stirrer to mix it thoroughly, and then let it stand for 10 minutes.

[0064] S4: Take 6 μL of the cationic surfactant prepared in S2, drop it on the surface of the reaction precursor solution, and leave it in a cool and ventilated place for 10 minutes to allow the chloroform to evaporate completely.

[0065] S5: Growth of (FeNiZnMo)O: Tighten the bottle cap and place the prepared reaction precursor solution in a cool, dark cabinet. React at room temperature for 7 hours to complete the growth of (FeNiZnMo)O.

[0066] S6: Transfer of (FeNiZnMo)O: Use a silicon wafer with an oxide layer, immerse it slightly at an angle in the liquid, and then pull it back vertically to complete the transfer of (FeNiZnMo)O, and dry it naturally in air for several hours.

[0067] The (FeNiZnMo)O transferred in this example was observed using a scanning electron microscope. Figure 2 As shown, the formed high entropy oxide (FeNiZnMo)O film is dense and uniform, showing a good synthesis trend, which reflects the advantages of ion layer epitaxy in preparing high entropy alloy oxides.

[0068] Example 4

[0069] like Figure 1 As shown, the steps of the method for preparing high entropy alloy oxide by ion layer epitaxy described in this embodiment include:

[0070] S1: Preparation of precursor solution: Take 0.0435g nickel nitrate hexahydrate, 0.019g ferrous chloride, 0.024g copper nitrate hexahydrate, and 0.185g ammonium molybdate, and prepare 10mM nickel nitrate, ferrous chloride, copper nitrate, and ammonium molybdate solutions in 15mL glass bottles, respectively, and shake well to dissolve.

[0071] S2: Preparation of cationic surfactant: Dissolve 20 μL of oleylamine in 10 mL of chloroform, and let stand at room temperature for 24 h after it is fully dissolved.

[0072] S3: Use a pipette to transfer 7 μL of ferrous chloride solution, 5 μL of nickel nitrate solution, 6 μL of copper nitrate solution, and 8 μL of ammonium molybdate solution prepared in step 1 into a 15 mL glass bottle. Add 5 mL of deionized water to the bottle and let it stand for 20 minutes.

[0073] S4: Take 8 μL of the cationic surfactant prepared in S2, drop it on the surface of the reaction precursor solution, and leave it in a cool and ventilated place for 10 minutes to allow the chloroform to evaporate completely.

[0074] S5: Growth of (FeNiCuMo)O: Tighten the bottle cap and place the prepared reaction precursor solution in a cool and dark place. React at room temperature for 6 hours to complete the growth of (FeNiCuMo)O.

[0075] S6: Transfer of (FeNiCuMo)O: Use a silicon wafer with an oxide layer, immerse it slightly at an angle in the liquid, and then pull it back vertically to complete the transfer of (FeNiCuMo)O, and dry it naturally in air for several hours.

[0076] The (FeNiCuMo)O transferred in this example was observed using a scanning electron microscope. Figure 3 As shown, the prepared high entropy oxide (FeNiCuMo)O presents an extremely small nanosheet form and has an ultra-thin morphology, which reflects the advantage of ion layer epitaxy using the water-air interface as a template to synthesize high entropy alloy oxides, and it is simple and efficient to obtain small-sized, ultra-thin high entropy oxides.

[0077] Example 5

[0078] like Figure 1 As shown, the steps of the method for preparing high entropy alloy oxide by ion layer epitaxy described in this embodiment include:

[0079] S1: Preparation of precursor solution: 0.0435 g nickel nitrate hexahydrate, 0.019 g ferrous chloride, 0.0436 g cobalt nitrate hexahydrate, 0.024 g copper nitrate hexahydrate and 0.185 g ammonium molybdate were prepared into 10 mM mixed solutions in 15 mL glass bottles and shaken thoroughly to dissolve.

[0080] S2: Preparation of cationic surfactant: Dissolve 20 μL of oleylamine in 10 mL of chloroform, and let stand at room temperature for 24 h after it is fully dissolved.

[0081] S3: Use a pipette to transfer 7 μL of ferrous chloride solution, 7 μL of nickel nitrate solution, 9 μL of cobalt nitrate solution, 8 μL of copper nitrate solution and 5 μL of ammonium molybdate solution prepared in step 1 into a 15 mL glass bottle. Add 5 mL of deionized water to the bottle and let it stand for 10 minutes.

[0082] S4: Take 10 μL of the cationic surfactant prepared in S2, drop it on the surface of the reaction precursor solution, and leave it in a cool and ventilated place for 10 minutes to allow the chloroform to evaporate completely.

[0083] S5: Growth of (FeNiCoCuMo)O: Tighten the bottle cap and place the prepared reaction precursor solution in a cool, dark place. React at room temperature for 7.5 h to complete the growth of (FeNiCoCuMo)O.

[0084] S6: Transfer of (FeNiCoCuMo)O: Use a silicon wafer with an oxide layer, immerse it slightly at an angle in the liquid, and then pull it back vertically to complete the transfer of (FeNiCoCuMo)O, and then dry it in air at room temperature for 24 hours.

[0085] The (FeNiCoCuMo)O transferred in this example was observed using a scanning electron microscope. Figure 4 As shown, the high entropy oxide (FeNiCoCuMo)O presents a thin film form with extremely small size and thickness and uniform morphology.

[0086] Example 6

[0087] like Figure 1 As shown, the steps of the method for preparing high entropy alloy oxide by ion layer epitaxy described in this embodiment include:

[0088] S1: Preparation of precursor solution: Take 0.002g of chloroplatinic acid hexahydrate, 0.0435g of nickel nitrate hexahydrate, 0.019g of ferrous chloride, 0.0436g of cobalt nitrate hexahydrate, 34μL of manganese nitrate solution and 0.018g of urea, prepare 10mM nickel nitrate, ferrous chloride, cobalt nitrate, manganese nitrate and 20mM urea solutions in 15mL glass bottles respectively, and shake well to dissolve.

[0089] S2: Preparation of anionic surfactant: 2.56 g of stearic acid was dissolved in 10 mL of dichloromethane, and after fully dissolved, it was allowed to stand at room temperature for 24 h.

[0090] S3: Use a pipette to transfer 25 μL of chloroplatinic acid solution, 7 μL of ferrous chloride solution, 8 μL of nickel nitrate solution, 5 μL of cobalt nitrate solution, and 7 μL of manganese nitrate solution prepared in step 1 into a 15 mL glass bottle. Use a pipette to transfer 20 μL of urea solution, add 5 mL of deionized water to the bottle, and let it stand for 30 minutes.

[0091] S4: Take 10 μL of the anionic surfactant prepared in S2, drop it on the surface of the reaction precursor solution, and leave it in a cool and ventilated place for 10 minutes to allow the dichloromethane to evaporate completely.

[0092] S5: Growth of (PtFeNiCoMn)O: Tighten the bottle cap, put the prepared reaction precursor solution into a forced air drying oven, and keep it at 80°C for 100 minutes to complete the growth of (PtFeNiCoMn)O.

[0093] S6: Transfer of (PtFeNiCoMn)O: Avoid partially solidified surfactant on the liquid surface, quickly immerse the silicon wafer with an oxide layer slightly tilted at the liquid surface, then pull it back vertically to complete the transfer of (PtFeNiCoMn)O, and dry it naturally in air for several hours.

[0094] Example 7

[0095] like Figure 1 As shown, the steps of the method for preparing high entropy alloy oxide by ion layer epitaxy described in this embodiment include:

[0096] S1: Preparation of precursor solution: Take 0.002g of chloroplatinic acid hexahydrate, 0.0435g of nickel nitrate hexahydrate, 0.019g of ferrous chloride, 0.0436g of cobalt nitrate hexahydrate, 0.0271g of zinc nitrate hexahydrate and 0.018g of urea, prepare 10mM nickel nitrate, ferrous chloride, cobalt nitrate, zinc nitrate and 20mM urea solutions in 15mL glass bottles respectively, and shake well to dissolve.

[0097] S2: Preparation of anionic surfactant: 2.56 g of stearic acid was dissolved in 10 mL of dichloromethane, and after fully dissolved, it was allowed to stand at room temperature for 24 h.

[0098] S3: Use a pipette to transfer 25 μL of chloroplatinic acid solution, 7 μL of ferrous chloride solution, 8 μL of nickel nitrate solution, 5 μL of cobalt nitrate solution, and 5 μL of zinc nitrate solution prepared in step 1 into a 15 mL glass bottle. Use a pipette to transfer 20 μL of urea solution, add 5 mL of deionized water to the bottle, and let it stand for 30 minutes.

[0099] S4: Take 8 μL of the anionic surfactant prepared in S2, drop it on the surface of the reaction precursor solution, and leave it in a cool and ventilated place for 10 minutes to allow the dichloromethane to evaporate completely.

[0100] S5: Growth of (PtFeNiCoZn)O: Tighten the bottle cap, place the prepared reaction precursor solution into a forced air drying oven, and keep it at 80°C for 2h to complete the growth of (PtFeNiCoZn)O.

[0101] S6: Transfer of (PtFeNiCoZn)O: Avoid partially solidified surfactant on the liquid surface, quickly immerse the silicon wafer with an oxide layer at a slight angle on the liquid surface, then pull it back vertically to complete the transfer of (PtFeNiCoZn)O, and dry it naturally in air for several hours.

[0102] In summary, the experimental equipment used in Examples 1-7 is relatively common, and the amount of precious metals used in the preparation process is extremely small, and the material utilization rate is high. During the reaction process, silicon wafers or the like are used as substrates for observation to observe the morphology, structure and growth trend of high entropy oxides, so as to study whether the selected metal analogy has a synthesis trend. If there is no obvious synthesis trend, unnecessary subsequent waste of resources can be avoided, time costs can be saved, and high entropy oxides can be efficiently and conveniently synthesized on a large scale.

[0103] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent replacement and improvement made to the above embodiments without departing from the content of the technical solution of the present invention, based on the technical essence of the present invention, within the spirit and principles of the present invention, still fall within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing high entropy alloy oxide by ion layer epitaxy, characterized in that: The steps of the preparation method of synthesizing high entropy alloy oxide by ion layer epitaxy include: Step 1: prepare surfactant; Step 2: preparing a metal salt precursor solution; Step 3: prepare urea solution; Step 4: According to the type of surfactant, selectively use a pipette to suck the prepared metal salt precursor solution and the prepared urea solution in turn, put them into a 15mL glass bottle, and add 5mL of deionized water to the glass bottle; according to the type of solution in the glass bottle, use a pipette to suck the corresponding surfactant, drop it on the surface of the solution in the glass bottle, open the bottle mouth and let it stand for 10 minutes, wait for the surfactant solvent to evaporate, and then tighten the bottle cap to obtain a reaction precursor solution; Step 5: If an anionic surfactant is added dropwise on the surface of the solution in the glass bottle, the glass bottle is placed in a forced air drying oven at 80°C, and the high entropy alloy oxide is obtained at the water-air two-phase interface after being kept warm for 100min-2.5h; if a cationic surfactant is added dropwise on the surface of the solution in the glass bottle, the reaction is carried out in a cool room temperature environment for 6-7.5h to obtain a high entropy alloy oxide at the water-air two-phase interface; Step 6: Use tweezers to pick up the silicon wafer with an oxide layer, immerse it in the liquid at a slight angle, and then pull it back vertically to obtain a high entropy alloy oxide on the silicon wafer.

2. The method for preparing high entropy alloy oxide by ion layer epitaxy according to claim 1, characterized in that: The surfactant in step 1 is prepared from a surfactant solution and a solvent, and the surfactant includes a cationic surfactant and an anionic surfactant; The surfactant solution includes but is not limited to stearic acid, oleylamine, sodium lauryl sulfate, sodium oleyl sulfate and sodium dodecylbenzene sulfonate; Such solutions include, but are not limited to, dichloromethane and chloroform.

3. The method for preparing high entropy alloy oxide by ion layer epitaxy according to claim 2, characterized in that: The steps of configuring the anionic surfactant include: 2.56 g of stearic acid and 10 mL of dichloromethane were mixed into a 0.9 M solution, and the mixture was fully mixed to form a clear and transparent solution. The anionic surfactant was obtained after standing for 24 hours.

4. The method for preparing high entropy alloy oxide by ion layer epitaxy according to claim 2, characterized in that: The steps of configuring the cationic surfactant include: Oleylamine and dichloromethane in a volume ratio of 1:500 were prepared into a solution with a volume of 10 mL, and the solution was fully mixed to form a clear and transparent solution. The solution was allowed to stand for 24 hours to obtain a cationic surfactant.

5. The method for preparing high entropy alloy oxide by ion layer epitaxy according to claim 1, characterized in that: The steps of preparing the metal precursor solution in step 2 include: Use an electronic balance to weigh Pt salt, Ni salt, Fe salt, Co salt, Zn salt, Cu salt, Al salt and Mo salt in a mass ratio of 0.002g:0.0435g:0.019g:0.0436g:0.0271g:0.024g:0.037g:0.135g, put the weighed Pt salt, Ni salt, Fe salt, Co salt, Zn salt, Cu salt, Al salt and Mo salt into a glass bottle, use a pipette to transfer 34μL of Mn salt solution dropwise into the glass bottle, add 5mL of deionized water to the glass bottle, fully dissolve and mix, and then stir magnetically for 10min to obtain a metal salt precursor solution with a total volume of 5mL; The metal salt precursor solution includes, but is not limited to, solutions of chloroplatinic acid hexahydrate, nickel nitrate hexahydrate, ferrous chloride, cobalt nitrate hexahydrate, zinc nitrate hexahydrate, manganese nitrate solution, aluminum nitrate nonahydrate, copper nitrate hexahydrate and ammonium molybdate.

6. The method for preparing high entropy alloy oxide by ion layer epitaxy according to claim 1, characterized in that: The steps of preparing the urea solution in step 3 include: Weigh 0.018 g of urea with an electronic balance, put it into a 15 mL glass bottle, add 10 mL of deionized water to the glass bottle to dissolve it, and mix it thoroughly to obtain a urea solution; The urea solution is used to adjust the alkaline environment of the solution and can be replaced by one of hexamethylenetetramine and sodium hydroxide. The urea solution is prepared from a mixture of one or more of urea, hexamethylenetetramine and sodium hydroxide.

7. The method for preparing high entropy alloy oxide by ion layer epitaxy according to claim 1, characterized in that: In the process of preparing the reaction precursor solution in step 4, if the type of surfactant added is a positive surfactant, use a pipette to draw 5 μL of the prepared metal salt precursor solution including ammonium molybdate, put it into a 15 mL glass bottle, add 5 mL of deionized water to the glass bottle, let it stand for 30 minutes, then use a pipette to draw 6-10 μL of cationic surfactant and drop it on the surface of the solution in the bottle, open the bottle mouth and let it stand for 10 minutes, wait for the surfactant solvent to evaporate, and then tighten the bottle cap; If the added surfactant type is anionic surfactant, use a pipette to successively pipette 5 μL of the prepared metal salt precursor solution and 10 μL of urea solution, add 5 mL of deionized water to the glass bottle, let the metal salt precursor solution and urea solution stand in the glass bottle for 30 minutes, then use a pipette to pipette 6-10 μL of anionic surfactant and drop it on the surface of the solution in the bottle, open the bottle mouth and let it stand for 10 minutes, wait for the surfactant solvent to evaporate, and then tighten the bottle cap.

8. The method for preparing high entropy alloy oxide by ion layer epitaxy according to claim 1, characterized in that: During the reaction process of steps 4-6, a substrate is used for real-time observation, and the substrate includes but is not limited to silicon wafer, FTO glass and ITO glass.